A kind of durable green coating and preparation method thereof

By using a mixture of hydroxyl acrylic resin and fluorocarbon resin and the compound technology of chromium trioxide, strontium oxide and yttrium trioxide, the shortcomings of existing green paints in durability and cooling and insulation effects are solved, and durable The development of environmentally friendly green coatings is suitable for applications in a variety of situations.

CN116751486BActive Publication Date: 2024-10-11SHIJIAZHUANG PAINT FACTORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310925776.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-26
Publication Date
2024-10-11
Estimated Expiration
2043-07-26

AI Technical Summary

Technical Problem

Existing green coatings have deficiencies in cooling and insulation effects and durability. They cannot have excellent insulation, cooling and durability at the same time, and their color effects are poor, making it difficult to meet the needs of different occasions.

Method used

A mixture of hydroxyl acrylic resin and fluorocarbon resin is used as the resin matrix, combined with compound reflective pigments of chromium trioxide, strontium oxide and yttrium trioxide. By adjusting the optical properties and ingredient ratio, the loss rate and powdering degree are reduced. , improve adhesion and corrosion resistance, and optimize the reflective properties of coatings.

Benefits of technology

The prepared durable green paint is not easy to fade, has excellent durability and heat insulation and cooling effect, is suitable for industrial production, and adapts to the color requirements of different occasions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of coating technology, and in particular to a durable green coating and a preparation method thereof. The durable green coating provided by the present invention comprises the following components by mass: 30 parts to 50 parts of a resin matrix, 20 parts to 30 parts of a reflective pigment, 5 parts to 15 parts of a toning pigment, 5 parts to 15 parts of a filler, 2 parts to 6 parts of an auxiliary agent, 1 part to 3 parts of an infrared absorber, and 10 parts to 15 parts of an organic solvent. By selecting a specific resin matrix and components such as a reflective pigment and a toning filler, through a reasonable component ratio, the light loss rate and powdering degree of the coating are reduced, the adhesion is improved, the corrosion resistance is improved, and the durability of the coating is improved. The optical properties of the coating can also be optimized to improve the reflective performance of the coating to green light, and the prepared coating is not easy to fade; the components of the present invention work synergistically, so that the prepared coating has both excellent durability and heat insulation and cooling effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a durable green coating and a preparation method thereof. Background Art

[0002] The sun is an indispensable part of human production and life. The effective use of solar energy has brought good news to the technological revolution of human new energy, but strong solar radiation will also bring many adverse effects to industrial production and life. For example, after a long period of exposure to the sun, the surface energy of equipment and facilities will accumulate and the temperature will soar. The sunlight will quickly conduct to the inside of the object through the metal material, resulting in a reduction in the service life of equipment and facilities. In addition, the high temperature environment inside the equipment or facilities is not conducive to human production or life. Therefore, it is urgent to reduce the temperature of equipment and facilities in hot summer and increase the service life of equipment and facilities.

[0003] There are many cooling measures for equipment and facilities, and coating is one of the most economical, convenient, fast, positive and effective ways. At present, the most common reflective heat insulation and cooling paint on the market is white. White reflective cooling paint is widely used because of its good reflective effect, but white heat insulation reflective paint is not suitable for all occasions. It should be combined with the actual situation to meet the different needs of different occasions for color. Therefore, it is very necessary to develop a colored cooling and heat insulation paint. Among the colored reflective heat insulation and cooling paints, green cooling and heat insulation paints can reflect sunlight and dissipate heat, effectively reduce the temperature of the surface of equipment or facilities, reduce the frequency of use and energy consumption of indoor air conditioners, slow down material aging, and extend the service life of buildings. However, most of the existing green paints use low-brightness organic pigments or increase the amount of pigments to reduce the resin content to reduce the brightness, but the coating of the green paint prepared by this preparation method either has a large difference in near-infrared reflectivity from green plants and poor heat insulation and cooling effect, or the prepared coating has poor mechanical properties and is not practical, and cannot have both cooling and heat insulation and durability. Therefore, it is of great significance to provide a green paint with both durability and cooling and heat insulation. Summary of the invention

[0004] In view of this, the present application provides a durable green coating and a preparation method thereof. By selecting a specific resin matrix and various components such as reflective pigments and color-adjusting fillers, and through a reasonable component ratio, the gloss loss rate and powdering degree of the coating are reduced, the adhesion is improved, the corrosion resistance is increased, and thus the durability of the coating is improved. The optical properties of the coating can also be optimized to improve the coating's reflective performance for green light, and the prepared coating is not easy to fade. The various components of the present invention act synergistically, so that the prepared coating has both excellent durability and heat insulation and cooling effects.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0006] The first aspect of the present invention provides a durable green coating, comprising the following components in parts by weight: 30-50 parts of a resin matrix, 20-30 parts of a reflective pigment, 5-15 parts of a toning pigment, 5-15 parts of a filler, 2-6 parts of an additive, 1-3 parts of an infrared absorber, and 10-15 parts of an organic solvent;

[0007] Wherein, the resin matrix is ​​a mixture of hydroxy acrylic resin and fluorocarbon resin;

[0008] The reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide.

[0009] When used as a film-forming substance, hydroxy acrylic resin is prone to problems such as coating cracking, fading and loss of gloss, thereby reducing the service life of the coating.

[0010] Compared with the prior art, the durable green coating provided by the present invention selects a composite of hydroxy acrylic resin and fluorocarbon resin as a resin matrix, and by introducing the synergistic effect of fluorocarbon resin and hydroxy acrylic resin, the problems of cracking, fading and gloss loss of the coating caused by the hydroxy acrylic resin can be significantly improved, and the stability of the coating in the outdoor environment can be improved, so that the prepared coating has excellent durability; the cobalt ion in cobalt trioxide has a strong ability to emit blue light, and it is difficult to reflect green light when used alone. The present invention further selects chromium trioxide and cobalt trioxide for composite use, and combines chromium trioxide that absorbs yellow-green light with cobalt trioxide that absorbs red light. The absorption characteristics and reflection characteristics of chromium trioxide and cobalt trioxide are superimposed on each other, and blue light and green light can be reflected, thereby The pigment achieves a dark green effect; further, the present invention accidentally discovered that by using strontium oxide and yttrium trioxide as auxiliary additive pigments, doping them into chromium trioxide and cobalt trioxide, and adjusting the absorption and reflection characteristics of the pigment to light by changing the lattice structure, the pigment finally obtained achieves a reflection channel similar to that of green plants, greatly improving the near-infrared reflectance and hemispherical emissivity of the pigment obtained by compounding chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide, so that the prepared coating achieves the effect of heat insulation and cooling; the specific resin matrix of the present invention can also improve the dispersibility of the reflective pigment in the coating, and the compounding of the two can not only improve the near-infrared reflectance and hemispherical emissivity of the coating, achieving the effect of heat insulation and cooling, but also greatly improve the durability of the coating.

[0011] The durable green coating provided by the present invention selects specific resin matrix and reflective pigments, color-adjusting fillers and other components, and reduces the gloss loss rate and powdering degree of the coating, improves adhesion, improves corrosion resistance and thus improves the durability of the coating through a reasonable component ratio. It can also optimize the optical properties of the coating to improve the reflective performance of the coating to green light, and the prepared coating is not easy to fade; the components of the present invention act synergistically, so that the prepared coating has both excellent durability and heat insulation and cooling effects.

[0012] Preferably, the resin matrix is ​​a mixture of hydroxy acrylic resin and fluorocarbon resin in a mass ratio of 1:(1-2).

[0013] The preferred resin matrix can further improve the durability and heat insulation and cooling effect of the coating.

[0014] Preferably, the reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide in a mass ratio of (25-35):(28-32):(2-4):(7-11).

[0015] The preferred reflective pigment and resin matrix play a synergistic role, greatly improving the heat insulation and cooling effect and durability of the coating.

[0016] Preferably, the method for preparing the reflective pigment comprises the following steps:

[0017] Step 1, grinding chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide to a particle size of 40 μm-50 μm, and drying to obtain a first treated product;

[0018] Step 2: Grind the first treated product to a particle size of 20 μm-30 μm, calcine at 1100° C.-1500° C., sieve, and retain the undersize to obtain the reflective pigment.

[0019] The preferred preparation method can further improve the near-infrared reflectance and hemispherical emissivity of the reflective pigment.

[0020] Preferably, in step 2, the calcination time is 3h-4h.

[0021] Preferably, the particle size of the reflective pigment is ≤30 μm.

[0022] Preferably, the hydroxyl acrylic resin has a hydroxyl value of 120 mgKOH / g-140 mgKOH / g, a solid content of 60%-75%, and a glass transition temperature of 55°C-90°C.

[0023] Further preferably, the model of the hydroxy acrylic resin is at least one of Allnex SETALUX 1907BA-75, Tongde ACR6736A or Deqian FS-4365.

[0024] Preferably, the fluorine content of the fluorocarbon resin is ≥25%.

[0025] The present invention further defines the hydroxyl value content, solid content and glass transition temperature of the hydroxy acrylic resin and the fluorine content of the fluorocarbon resin. The selection of specific hydroxy acrylic resin and fluorocarbon resin can further improve the durability of the coating. The specific hydroxy acrylic resin and fluorocarbon resin also cooperate with specific reflective resin to improve the heat insulation and cooling effect of the coating.

[0026] Further preferably, the fluorocarbon resin is at least one of Daikin GK570, Wanbo WF-Q212, and Dongfu JF-2X.

[0027] Preferably, the coloring pigment is at least one of copper oxide, ferric oxide, nickel oxide or lanthanum oxide.

[0028] Preferably, the filler is at least one of barium sulfate, talc, lime powder, silicon powder, calcium carbonate or silicon dioxide.

[0029] Preferably, the infrared absorber is at least one of HSYP-01 infrared absorber, cesium tungsten infrared absorber or GTO-P100 infrared absorber.

[0030] Preferably, the organic solvent is at least one of cyclohexanone, butyl acetate, ethyl acetate, butanol, phosphomolybdic acid or ethylene glycol diacetate.

[0031] Preferably, the auxiliary agent includes a dispersant, a defoamer, an anti-settling agent, a leveling agent, an adhesion promoter and a UV absorber.

[0032] Preferably, the mass ratio of the dispersant, defoamer, anti-settling agent, leveling agent, adhesion promoter and ultraviolet absorber in the auxiliary agent is (0.4-0.6):(0.2-0.4):(0.5-0.7):(0.25-0.4):1:(0.5-0.7).

[0033] Preferably, the dispersant is at least one of a polyurethane dispersant, a polyacrylate dispersant or a cationic surfactant.

[0034] Preferably, the defoamer is a mineral oil defoamer, a silicone defoamer or a silicone-free polymer defoamer.

[0035] Preferably, the anti-settling agent is at least one of fumed silica, polyamide wax or bentonite.

[0036] Preferably, the leveling agent is at least one of polyacrylate, polydimethylsiloxane or cellulose acetate butyrate.

[0037] Preferably, the adhesion promoter is at least one of an acrylic adhesion promoter, a sulfide adhesion promoter or a silane adhesion promoter.

[0038] Preferably, the ultraviolet absorber is at least one of a salicylate ultraviolet absorber, a triazine ultraviolet absorber or a benzophenone ultraviolet absorber.

[0039] The second aspect of the present invention provides a method for preparing the above-mentioned durable green coating, comprising the following preparation steps:

[0040] Weigh each component according to the mass ratio, evenly disperse the weighed resin matrix, reflective pigment, toning pigment, filler, additive, infrared absorber and 4wt%-6wt% organic solvent, grind to a fineness of ≤25μm, add the remaining organic solvent, and obtain the durable green coating.

[0041] The preparation method of the durable green coating provided by the invention is simple to operate, has no complicated process, does not require special equipment, has low cost, is suitable for industrial large-scale production, and has broad market prospects. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0043] Example 1

[0044] This embodiment provides a durable green coating, comprising the following components in parts by weight: 30 parts of a resin matrix, 30 parts of a reflective pigment, 5 parts of ferric oxide, 15 parts of barium sulfate, 2 parts of an additive, 3 parts of an HSYP-01 infrared absorber, and 10 parts of cyclohexanone;

[0045] The resin matrix is ​​a mixture of hydroxyl acrylic resin Deqian FS-4365 and fluorocarbon resin Dongfu JF-2X in a mass ratio of 1:1;

[0046] The reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide in a mass ratio of 35:28:4:11;

[0047] The preparation method of the reflective pigment comprises the following steps:

[0048] Step 1, weighing each component according to the mass ratio, grinding the weighed chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide to a particle size of 40 μm-50 μm, and drying to obtain a first treated product;

[0049] Step 2, grinding the first treated product to a particle size of 20 μm-30 μm, calcining at 1500° C. for 3 h, sieving, retaining the undersize, and obtaining a reflective pigment with a particle size of ≤30 μm;

[0050] The auxiliary agents are a polyurethane dispersant, a silicone defoamer, a fumed silica, a polyacrylate, an acrylic adhesion promoter and a salicylate UV absorber in a mass ratio of 0.4:0.4:0.5:0.4:1:0.7.

[0051] The method for preparing the above-mentioned durable green coating comprises the following preparation steps:

[0052] Weigh each component according to the mass ratio, disperse the weighed resin matrix, reflective pigment, ferric oxide, barium sulfate, additives, HSYP-01 infrared absorber and 4wt% of cyclohexanone evenly, grind to a fineness of ≤25μm, add the remaining cyclohexanone, and obtain the durable green coating.

[0053] Example 2

[0054] This embodiment provides a durable green coating, comprising the following components in parts by weight: 50 parts of a resin matrix, 20 parts of a reflective pigment, 15 parts of nickel oxide, 5 parts of talcum powder, 6 parts of an additive, 1 part of a GTO-P100 infrared absorber, and 15 parts of butyl acetate;

[0055] The resin matrix is ​​a mixture of hydroxyl acrylic resin Allsin SETALUX 1907BA-75 and fluorocarbon resin Daikin GK570 in a mass ratio of 1:2;

[0056] The reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide in a mass ratio of 25:32:2:7;

[0057] The preparation method of the reflective pigment comprises the following steps:

[0058] Step 1, weighing each component according to the mass ratio, grinding the weighed chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide to a particle size of 40 μm-50 μm, and drying to obtain a first treated product;

[0059] Step 2, grinding the first treated product to a particle size of 20 μm-30 μm, calcining at 1100° C. for 4 hours, sieving, retaining the undersize, and obtaining a reflective pigment with a particle size of ≤30 μm;

[0060] The additives are polyacrylate dispersant, mineral oil defoamer, polyamide wax, polydimethylsiloxane, sulfide adhesion promoter and triazine ultraviolet absorber in a mass ratio of 0.6:0.2:0.7:0.25:1:0.5.

[0061] The method for preparing the above-mentioned durable green coating comprises the following preparation steps:

[0062] Weigh each component according to the mass ratio, disperse the weighed resin matrix, reflective pigment, nickel oxide, talcum powder, additives, GTO-P100 infrared absorber and 6wt% butyl acetate evenly, grind to a fineness of ≤25μm, add the remaining butyl acetate, and obtain the durable green coating.

[0063] Example 3

[0064] This embodiment provides a durable green coating, comprising the following components in parts by weight: 40 parts of a resin matrix, 25 parts of a reflective pigment, 10 parts of lanthanum oxide, 10 parts of silicon powder, 4 parts of an additive, 2 parts of a cesium tungsten infrared absorber, and 12 parts of butanol;

[0065] The resin matrix is ​​a mixture of hydroxyl acrylic resin Tongde ACR6736A and fluorocarbon resin Wanbo WF-Q212 in a mass ratio of 1:1.5;

[0066] The reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide in a mass ratio of 30:30:3:10;

[0067] The preparation method of the reflective pigment comprises the following steps:

[0068] Step 1, weighing each component according to the mass ratio, grinding the weighed chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide to a particle size of 40 μm-50 μm, and drying to obtain a first treated product;

[0069] Step 2, grinding the first treated product to a particle size of 20 μm-30 μm, calcining at 1200° C. for 3.5 hours, sieving, retaining the undersize, and obtaining a reflective pigment with a particle size of ≤30 μm;

[0070] The additives are a polyacrylate dispersant, a silicone-free polymer defoamer, bentonite, cellulose acetate butyrate, a silane adhesion promoter and a benzophenone ultraviolet absorber in a mass ratio of 0.5:0.3:0.6:0.35:1:0.6.

[0071] The method for preparing the above-mentioned durable green coating comprises the following preparation steps:

[0072] Weigh each component according to the mass ratio, disperse the weighed resin matrix, reflective pigment, lanthanum oxide, silicon powder, additives, cesium tungsten infrared absorber and 5wt% of butyl acetate evenly, grind to a fineness of ≤25μm, add the remaining butanol, and obtain the durable green coating.

[0073] Comparative Example 1

[0074] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that chromium trioxide is replaced by an equal amount of iron oxide green, and the other components and steps are the same as those in Example 1.

[0075] Comparative Example 2

[0076] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that strontium oxide is replaced by an equal amount of titanium oxide, and the other components and steps are the same as those in Example 1.

[0077] Comparative Example 3

[0078] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that the hydroxylated acrylic resin Deqian FS-4365 is replaced by an equal amount of SETATHANE D1150, and the other components and steps are the same as those in Example 1.

[0079] Comparative Example 4

[0080] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that the number of parts of the resin matrix is ​​increased to 60 parts, and the other components and steps are the same as those in Example 1.

[0081] Comparative Example 5

[0082] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that the number of parts of the resin matrix is ​​reduced to 20 parts, and the other components and steps are the same as those in Example 1.

[0083] Comparative Example 6

[0084] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that the number of reflective pigments is increased to 40 parts, and the other components and steps are the same as those in Example 1.

[0085] Comparative Example 7

[0086] This comparative example provides a method for preparing a coating. Compared with Example 1, the difference is that the number of reflective pigments is reduced to 15 parts, and the other components and steps are the same as those in Example 1.

[0087] Application Examples

[0088] The coatings provided in Examples 1-3 and Comparative Examples 1-7 of the present invention were tested for performance, and the specific test standards are as follows:

[0089] According to the requirements and test methods for cyclic aging resistance in GB / T31415-2015 standard, a cyclic aging resistance experiment was conducted; the composite coating was coated on a 150mm×75mm×3mm steel plate for testing, the primer: epoxy zinc phosphate primer, the film thickness is 80μm-100μm, the top coating: the coating of Examples 1-3 and Comparative Examples 1-7, the film thickness is between 80μm-100μm;

[0090] According to the plate making requirements and test methods of near infrared reflectance and hemispherical emissivity in HG / T4341-2012 standard, the near infrared reflectance and hemispherical emissivity were tested; the composite coating was coated on a 150mm×70mm×1mm aluminum alloy plate for testing, the primer: epoxy zinc phosphate primer, the film thickness is 80μm-100μm, the top coating: the coating of Examples 1-3 and Comparative Examples 1-7, the film thickness is between 80μm-100μm;

[0091] According to the board making requirements and test methods in Appendix A of HG / T4341-2012 standard, the thermal insulation temperature difference test was carried out; the composite coating was applied on a 200mm×300mm×2mm steel plate for testing, primer: epoxy zinc phosphate primer, film thickness is 80μm-100μm, top coating: coatings of Examples 1-3 and Comparative Examples 1-7, film thickness is between 160μm-180μm.

[0092] After the new coating is naturally cured in a constant temperature room for 168 hours, the cyclic aging resistance, near infrared reflectance, hemispherical emissivity, and thermal insulation temperature difference tests are carried out;

[0093] After the near-infrared reflectance, hemispherical emissivity, and thermal insulation temperature difference tests, the near-infrared reflectance sample (without markings), hemispherical emissivity sample (without markings), thermal insulation temperature difference sample (without markings) and the sample that needs to be subjected to the cyclic aging test (with markings) are simultaneously subjected to the cyclic aging test;

[0094] After the cyclic aging test: rinse the near-infrared reflectance sample, hemispherical emissivity sample, and thermal insulation temperature difference sample with clean water, wipe them clean, place them in a constant temperature chamber for 24 hours, and then test the near-infrared reflectance, hemispherical emissivity, and thermal insulation temperature difference again.

[0095] The specific test results are as follows:

[0096] Table 1 Cyclic aging resistance test

[0097]

[0098]

[0099] Table 2 Cyclic aging resistance test

[0100]

[0101]

[0102]

[0103]

[0104] The cyclic aging resistance test uses an exposure cycle lasting one full week (168h), including:

[0105] a: Exposure to ultraviolet light and condensation for 72 hours, using a UVA-340 ultraviolet lamp, alternating between 4 hours of ultraviolet radiation at (60±3)℃ and 4 hours of condensation exposure at (50±3)℃, starting with ultraviolet radiation and ending with condensation exposure;

[0106] b: Expose to salt spray environment for 72 hours; the test panels can be rinsed with deionized water, but do not need to be dried;

[0107] c: Expose to low temperature at (-20±2)℃ for 24h. Rinse with deionized water before the experiment without drying. The test plate should reach the temperature of (-20±2)℃ within 30min.

[0108] Table 3 New coating tested after 168h of curing

[0109]

[0110] Table 4 Test results after cyclic aging

[0111]

[0112]

[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A durable green coating, characterized in that: The invention is composed of the following components in parts by weight: 30-50 parts of a resin matrix, 20-30 parts of a reflective pigment, 5-15 parts of a toning pigment, 5-15 parts of a filler, 2-6 parts of an auxiliary agent, 1-3 parts of an infrared absorber and 10-15 parts of an organic solvent; The resin matrix is ​​a mixture of hydroxy acrylic resin and fluorocarbon resin in a mass ratio of 1: (1-2); the hydroxy value of the hydroxy acrylic resin is 120 mgKOH / g-140 mgKOH / g, the solid content is 60%-70%, and the glass transition temperature is 55°C-90°C; the fluorine content of the fluorocarbon resin is ≥25%; The reflective pigment is a mixture of chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide in a mass ratio of (25-35): (28-32): (2-4): (7-11); the coloring pigment is at least one of copper oxide, iron trioxide, nickel oxide or lanthanum oxide; the filler is at least one of barium sulfate, talc, lime powder, silica powder, calcium carbonate or silicon dioxide; the infrared absorber is at least one of HSYP-01 infrared absorber or GTO-P100 infrared absorber; The preparation method of the reflective pigment comprises the following steps: Step 1, grinding chromium trioxide, cobalt trioxide, strontium oxide and yttrium trioxide to a particle size of 40 μm-50 μm, and drying to obtain a first treated product; Step 2: Grind the first treated product to a particle size of 20 μm-30 μm, calcine at 1100° C.-1500° C., sieve, and retain the undersize to obtain the reflective pigment.

2. The durable green coating according to claim 1, characterized in that: In step 2, the calcination time is 3h-4h; and / or The particle size of the reflective pigment is ≤30 μm.

3. The durable green coating according to claim 1, characterized in that: The organic solvent is at least one of cyclohexanone, butyl acetate, ethyl acetate, butanol or ethylene glycol diacetate; and / or The auxiliary agents include dispersants, defoamers, anti-settling agents, leveling agents, adhesion promoters and ultraviolet absorbers.

4. The durable green coating according to claim 3, characterized in that: The mass ratio of the dispersant, defoamer, anti-settling agent, leveling agent, adhesion promoter and ultraviolet absorber in the auxiliary agent is (0.4-0.6): (0.2-0.4): (0.5-0.7): (0.25-0.4): 1: (0.5-0.7).

5. The durable green coating according to claim 3, characterized in that: The dispersant is at least one of a polyurethane dispersant, a polyacrylate dispersant or a cationic surfactant; and / or The defoamer is a mineral oil defoamer, a silicone defoamer or a silicone-free polymer defoamer; and / or The anti-settling agent is at least one of fumed silica, polyamide wax or bentonite.

6. The durable green coating according to claim 3, characterized in that: The leveling agent is at least one of polyacrylate, polydimethylsiloxane or cellulose acetate butyrate; and / or The adhesion promoter is at least one of an acrylic adhesion promoter, a sulfide adhesion promoter or a silane adhesion promoter; and / or The ultraviolet absorber is at least one of a salicylate ultraviolet absorber, a triazine ultraviolet absorber or a benzophenone ultraviolet absorber.

7. A method for preparing the durable green coating according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: Weigh each component according to the mass ratio, evenly disperse the weighed resin matrix, reflective pigment, toning pigment, filler, additive, infrared absorber and 4wt%-6wt% of organic solvent, grind to a fineness of ≤25μm, add the remaining organic solvent, and obtain the durable green coating.