A kind of real stone paint emulsion and its preparation method and application
By using the core-shell polymerization process to coat nano-ultraviolet barrier agents and functional monomers in the real stone paint emulsion, the problem of poor weather resistance of the real stone paint emulsion under ultraviolet light is solved, and the water resistance and adhesion of the paint film is improved, so as to achieve Cost reduction and performance improvement.
Patent Information
- Application Number
- CN202310709445.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-15
AI Technical Summary
The existing real stone paint emulsion has poor weather resistance under ultraviolet light, resulting in yellowing of the paint film, and the cost of styrene acrylic emulsion is high and the market acceptance is low.
The core-shell polymerization process is adopted to coat the outer layer of the latex particles of the real stone paint emulsion to form a shell layer, which improves the water resistance, yellowing resistance and adhesion of the paint film.
It effectively improves the weather resistance and adhesion of real stone paint emulsion, enhances the UV resistance of the paint film, stabilizes the paint matching performance, and reduces costs.
Smart Images

Figure BDA0004287100070000041 
Figure BDA0004287100070000131 
Figure BDA0004287100070000142
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of real stone paint emulsion preparation, in particular to a real stone paint emulsion and a preparation method and application thereof, and particularly to a real stone paint emulsion with a core-shell structure and a preparation method and application thereof. Background Art
[0002] In recent years, stone paint has become popular due to its low cost, simple construction, and elegance and solemnity similar to marble and granite. However, with the continuous expansion of the market, competitiveness is becoming increasingly serious. The first problem facing manufacturers is the cost issue. At present, the main raw material that determines the cost is the adhesive water-based emulsion in the stone paint. There are currently two types of emulsions, one is styrene-acrylate copolymer, and the other is all-acrylate copolymer. The two emulsions have their own characteristics.
[0003] Due to the presence of benzene rings in styrene-acrylate copolymers, when exposed to ultraviolet light in the atmosphere, the benzene rings open, the paint film surface turns yellow, the weather resistance of the polymer deteriorates, and some defects of the paint film occur, resulting in secondary rework. The main characteristics of styrene acrylic emulsion are low cost and high cost.
[0004] The emulsion used in existing real stone paint usually optimizes the yellowing performance by reducing the styrene content, which cannot balance the performance well, and the cost of the monomer to replace styrene is high. There are currently two types of emulsions, one is styrene-acrylate copolymer, and the other is all-acrylate copolymer. The two emulsions have their own characteristics. Due to the presence of benzene rings in styrene-acrylate copolymers, they are exposed to ultraviolet light in the atmosphere, causing the benzene rings to open, the paint film surface to turn yellow, the weather resistance of the polymer to deteriorate, and some defects in the paint film are formed, resulting in secondary rework. The main feature of styrene-acrylate emulsions is that they are cheap, so in order to use styrene-acrylate emulsions well in real stone paint, the problem of styrene-acrylate emulsion weather resistance must be solved. All-acrylate copolymers have excellent weather resistance, but the biggest problem is that the cost is too high and the market acceptance is too poor.
[0005] CN102977257A discloses a water-whitening resistant core-shell structure real stone paint emulsion and a preparation method thereof. The real stone paint emulsion uses styrene, alkyl methacrylate, alkyl acrylate, and alkenyl carboxylic acid as monomers, introduces room temperature self-crosslinking monomers and silane coupling agents into the reaction system, and uses a composite emulsifier mainly composed of a reactive emulsifier; the preparation method adopts a semi-continuous seed emulsion polymerization process to obtain a water-whitening resistant real stone paint emulsion. The hard shell of the real stone paint emulsion of the invention can only ensure good anti-fouling performance, but does not have an anti-ultraviolet effect.
[0006] CN112940170A discloses a real stone paint emulsion and its preparation method. The core-shell polymerization process is adopted, the core part is mainly composed of tough monomers such as isooctyl acrylate, butyl acrylate, and long-chain acrylate, which give the polymer molecule sufficient flexible segments; the shell part is mainly composed of hard monomers such as styrene and methyl methacrylate, and is grafted with silicon functional monomer segments, which promotes the outer layer of the polymer molecule to form a rigid protective layer, but it does not have an anti-ultraviolet effect.
[0007] CN111393078A discloses a UV-resistant, weather-resistant, anti-fouling and heat-insulating real stone paint specially designed for plateau climates, which includes water, cellulose, UV absorbers, silicone-acrylic emulsions, glass beads, polystyrene particles, perlite particles, additives and aggregates; the UV absorber is an organic / inorganic core-shell composite UV absorber with TiO2 as the core and modified graphene as the shell, and the anti-UV effect is achieved by adding a UV absorber with a core-shell structure.
[0008] The emulsion used in existing stone paint usually optimizes the yellowing performance by reducing the styrene content, which cannot balance the performance well, and the cost of the monomer to replace styrene is high. Therefore, in order to use styrene acrylic emulsion well in stone paint, the problem of styrene acrylic emulsion weather resistance must be solved. All-acrylate copolymers have excellent weather resistance, but the biggest problem is that the cost is too high and the market acceptance is too poor.
[0009] In view of this, the present invention is proposed. Summary of the invention
[0010] One of the purposes of the present invention is to provide a real stone paint emulsion. The present invention effectively improves the yellowing resistance and weather resistance of the styrene acrylic emulsion in the real stone paint through the core-shell polymerization process, and also effectively improves the stain resistance and adhesion of the paint film.
[0011] The second purpose of the present invention is to provide a method for preparing a real stone paint emulsion. Through a two-step polymerization process design, the first step is to prepare a nano-UV slurry of the shell layer, and the second step is to prepare the real stone paint emulsion through a core-shell polymerization process. The use of core-shell technology effectively reduces the yellowing and poor weather resistance of the paint film due to ultraviolet radiation.
[0012] The third object of the present invention is to use the above-mentioned real stone paint emulsion in preparing a paint film with hydrophobic and UV-blocking functions.
[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0014] In a first aspect, the present invention provides a real stone paint emulsion, which has a core-shell structure; the shell layer of the core-shell structure includes an ultraviolet blocker and a functional monomer; the functional monomer includes a functional monomer with a hydrophobic group and a functional monomer with a hydrophilic group.
[0015] In the present invention, the shell layer of the core-shell structure includes an ultraviolet blocker and a functional monomer through a core-shell polymerization process, and the outer layer is formed with the functions of being hydrophobic and blocking ultraviolet rays, which effectively reduces the yellowing and poor weather resistance of the paint film due to ultraviolet radiation. The prepared coating has the characteristics of good adhesion, water resistance, yellowing resistance, good weather resistance, stable paint matching performance, etc.
[0016] Preferably, the UV blocking agent comprises nano-sized titanium dioxide.
[0017] Preferably, the particle size of the nano-scale titanium dioxide is 10-100 nm, for example, it can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc., preferably 15-50 nm.
[0018] Preferably, the nano-scale titanium dioxide includes rutile nano-titanium dioxide and / or anatase nano-titanium dioxide.
[0019] Nano titanium dioxide is a white loose powder with strong UV shielding effect, good dispersibility and weather resistance. Nano titanium dioxide has two main crystal forms: anatase and rutile. Rutile titanium dioxide is more stable and dense than anatase titanium dioxide, with higher hardness, density, dielectric constant and refractive index, and higher hiding power and tinting power. The reflectivity of anatase titanium dioxide in the short-wave part of visible light is higher than that of rutile titanium dioxide, with a blue hue, and its absorption capacity for ultraviolet rays is lower than that of rutile, and its photocatalytic activity is higher than that of rutile.
[0020] Preferably, the functional monomer having a hydrophilic group includes any one of acrylic acid, acrylamide or glyceryl methacrylate, or a combination of at least two thereof.
[0021] Preferably, the functional monomer having a hydrophobic group includes an organic silicon monomer; preferably a silane coupling agent, and more preferably triethyltrimethoxysilane and / or γ-(methacryloyloxy)propyltrimethoxysilane.
[0022] Preferably, the raw materials for preparing the real stone paint emulsion include the following components by mass:
[0023]
[0024] In the raw materials for preparing the real stone paint emulsion, the content of the slurry containing the ultraviolet blocking agent is 1-10 parts, for example, it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0025] In the raw materials for preparing the real stone paint emulsion, the content of the functional monomer is 1-10 parts, for example, it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0026] In the raw materials for preparing the real stone paint emulsion, the content of the hard monomer is 15-25 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.
[0027] In the raw materials for preparing the real stone paint emulsion, the content of the soft monomer is 15-25 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.
[0028] In the raw materials for preparing the real stone paint emulsion, the content of the emulsifier is 0.5-5 parts, for example, it can be 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.
[0029] In the raw materials for preparing the real stone paint emulsion, the content of the initiator is 0.05-1 part, for example, it can be 0.05 part, 0.08 part, 0.1 part, 0.12 part, 0.15 part, 0.2 part, 0.4 part, 0.6 part, 0.8 part, 1 part, etc.
[0030] In the raw materials for preparing the real stone paint emulsion, the content of water is 40-55 parts, for example, it can be 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 55 parts, etc.
[0031] In the present invention, by using the components in the raw materials for preparing the real stone paint emulsion in the above-mentioned specific ratio, the cross-linking density between molecules in the reaction process is improved, so that the polymer molecules form a compact network structure, and more cross-linking points are stably introduced into the system, thereby maximizing the cross-linking density between latex particles, effectively improving the water resistance and hardness of the paint film, and then also improving the adhesion of the paint film to the substrate.
[0032] Preferably, the hard monomer includes any one of styrene, methyl acrylate or methyl methacrylate or a combination of at least two thereof, preferably styrene.
[0033] Preferably, the soft monomer includes any one of butyl acrylate, isooctyl acrylate or ethyl acrylate, or a combination of at least two thereof, preferably butyl acrylate.
[0034] Preferably, the mass ratio of the functional monomer having a hydrophobic group to the functional monomer having a hydrophilic group in the functional monomer is (3-5):1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, etc.
[0035] Preferably, the emulsifier is a composite emulsifier.
[0036] Preferably, the composite emulsifier includes any one of anionic emulsifier, nonionic emulsifier or anionic and nonionic emulsifier, or a combination of at least two thereof.
[0037] Preferably, the anionic emulsifier includes any one of sodium fatty alcohol polyoxyethylene ether sulfate, sodium modified alkyl alcohol sulfonate, sodium dodecylbenzene sulfonate or sodium dodecyl sulfate, or a combination of at least two thereof.
[0038] Preferably, the nonionic emulsifier includes any one of polyoxyethylene ether, propylene oxide block copolymer or polyol fatty acid ester, or a combination of at least two thereof.
[0039] Preferably, the anionic nonionic emulsifier includes any one of polyoxyethylene nonylphenol succinate disodium, ethoxylated alcohol sulfosuccinate disodium or polyoxyethylene nonylphenol ether, or a combination of at least two thereof.
[0040] Preferably, the initiator includes any one of sodium persulfate, ammonium persulfate or potassium persulfate, or a combination of at least two thereof.
[0041] Preferably, the raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts (for example, 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, etc.) of a defoaming agent.
[0042] Preferably, the defoamer includes any one of an organosilicon defoamer, a mineral oil defoamer or a polyether modified defoamer, or a combination of at least two of them.
[0043] Preferably, the organosilicon defoaming agent includes any one of trimethyl silicone oil, dimethyl polysiloxane, silicone paste or polysiloxane, or a combination of at least two thereof.
[0044] Preferably, the mineral oil defoamer includes any one of white oil, liquid wax or naphthenic oil, or a combination of at least two of them.
[0045] Preferably, the polyether-modified defoamer comprises polyether-modified polysiloxane.
[0046] Preferably, the raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts (for example, 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, etc.) of preservatives.
[0047] Preferably, the preservative comprises Kathon and / or BIT.
[0048] Preferably, the BIT includes BIT10 and / or BIT20.
[0049] Preferably, the raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts (for example, 0.05 parts, 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, etc.) of a pH regulator.
[0050] Preferably, the pH regulator is an alkaline pH regulator, preferably any one of ammonia, AMP-95 or triethanolamine, or a combination of at least two thereof.
[0051] Preferably, the water is deionized water, and the conductivity of the deionized water is less than 10 μS / cm, for example, it may be 9.9 μS / cm, 9.8 μS / cm, 9.5 μS / cm, 9.2 μS / cm, etc.
[0052] Preferably, the raw materials for preparing the slurry containing the ultraviolet blocking agent include the following components by weight:
[0053] 40-70 parts of UV blocker
[0054] Dispersing wetting agent 0.05-1 part
[0055] 30-60 parts of water.
[0056] In the raw materials for preparing the slurry containing the ultraviolet blocking agent, the content of the ultraviolet blocking agent is 40-70 parts, for example, it can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, etc.
[0057] In the raw materials for preparing the slurry containing the ultraviolet blocking agent, the content of the dispersing wetting agent is 0.05-1 part, for example, it can be 0.05 part, 0.08 part, 0.1 part, 0.12 part, 0.15 part, 0.2 part, 0.4 part, 0.6 part, 0.8 part, 1 part, etc.
[0058] In the raw materials for preparing the slurry containing the ultraviolet blocking agent, the water content is 30-60 parts, for example, it can be 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, etc.
[0059] Preferably, the dispersing wetting agent is selected from any one of sulfate wetting agents, polycarboxylate wetting agents or sulfonate wetting agents, or a combination of at least two thereof, preferably a sulfonate wetting agent.
[0060] Preferably, the sulfate ester wetting agent is selected from any one of sodium lauryl sulfate, sodium polyoxyethylene fatty alcohol ether sulfate or sodium polyoxyethylene fatty amine sulfate, or a combination of at least two thereof.
[0061] Preferably, the polycarboxylate wetting agent is selected from any one of sodium polyacrylate, sodium polymethacrylate or sodium maleic acid-acrylate, or a combination of at least two thereof.
[0062] Preferably, the sulfonate wetting agent is selected from any one of sodium dodecylbenzenesulfonate, sodium butylnaphthalenesulfonate or sodium aminobenzenesulfonate, or a combination of at least two thereof.
[0063] Preferably, the water is deionized water, and the conductivity of the deionized water is less than 10 μS / cm, for example, it may be 9.9 μS / cm, 9.8 μS / cm, 9.5 μS / cm, 9.2 μS / cm, etc.
[0064] Preferably, the raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.1-0.2 parts (for example, 0.1 parts, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, 0.2 parts, etc.) of a defoaming agent;
[0065] Preferably, the defoamer includes any one of an organosilicon defoamer, a mineral oil defoamer or a polyether modified defoamer, or a combination of at least two of them.
[0066] Preferably, the organosilicon defoaming agent includes any one of trimethyl silicone oil, dimethyl polysiloxane, silicone paste or polysiloxane, or a combination of at least two thereof.
[0067] Preferably, the mineral oil defoamer includes any one of white oil, liquid wax or naphthenic oil, or a combination of at least two of them.
[0068] Preferably, the polyether-modified defoamer comprises polyether-modified polysiloxane.
[0069] Preferably, the raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.05-0.1 parts (for example, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 0.1 parts, etc.) of preservatives.
[0070] Preferably, the preservative comprises Kathon and / or BIT.
[0071] Preferably, the BIT includes BIT10 and / or BIT20.
[0072] Preferably, the raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.1-0.2 parts (for example, 0.1 parts, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, 0.2 parts, etc.) of a pH regulator.
[0073] Preferably, the pH regulator is an alkaline pH regulator, preferably any one of ammonia, AMP-95 or triethanolamine, or a combination of at least two thereof.
[0074] In the second aspect, the present invention provides a method for preparing the real stone paint emulsion as described in the first aspect, wherein the preparation method is: preparing by a core-shell polymerization process, coating the ultraviolet blocker and the functional monomer on the outer layer of the latex particles of the real stone paint emulsion to form a shell layer, and obtaining a real stone paint emulsion with a core-shell structure.
[0075] In the present invention, the nano-anti-ultraviolet interlayer agent is wrapped on the surface of the latex particles through the core-shell polymerization process design, which then plays a role in shielding ultraviolet rays, thereby effectively improving the weather resistance of the styrene acrylic real stone paint emulsion. At the same time, the shell layer introduces functional monomers, which effectively improves the water resistance and hardness of the paint film, and then also improves the adhesion of the paint film to the substrate. The prepared real stone paint emulsion has the characteristics of excellent paint stability and the like.
[0076] Preferably, the preparation method comprises the following steps:
[0077] Preparation of slurry containing ultraviolet blocking agent: mixing various components in the raw materials for preparing the slurry containing ultraviolet blocking agent to obtain the slurry containing ultraviolet blocking agent;
[0078] Preparation of mixed monomer solution: Mix the emulsifier, hard monomer, soft elastomer, functional monomer and part of water in the raw materials for preparing the real stone paint emulsion to obtain a pre-emulsified solution containing monomers;
[0079] Preparation of initiator solution: Mix the initiator and part of water in the raw materials for preparing the real stone paint emulsion to obtain an initiator solution;
[0080] Preparation of real stone paint emulsion: first, part of the mixed monomer solution and the initiator solution are mixed and reacted to form the latex particle core of the real stone paint emulsion, and then mixed with a slurry containing a UV blocker and reacted to coat the UV blocker and the functional monomer on the outer layer of the latex particles of the real stone paint emulsion to form a shell layer, thereby obtaining a real stone paint emulsion with a core-shell structure.
[0081] Preferably, the slurry containing the UV blocking agent is prepared by the following steps:
[0082] (1) stirring and mixing water and a dispersing and wetting agent to obtain a dispersion;
[0083] (2) The ultraviolet shielding agent and the above dispersion are stirred and mixed to obtain a material containing the ultraviolet shielding agent.
[0084] Preferably, in step (1), any one or a combination of at least two of a defoaming agent, a preservative or a pH adjuster is also added.
[0085] Preferably, in step (1), the stirring and mixing speed is 200-300 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, etc., and the stirring and mixing time is 4-6 min, for example, it can be 4 min, 4.5 min, 5 min, 5.5 min, 6 min, etc.
[0086] Preferably, in step (2), the stirring and mixing speed is 800-1000rpm, for example, it can be 800rpm, 850rpm, 900rpm, 950rpm, 1000rpm, etc., and the stirring and mixing time is 40-60min, for example, it can be 40min, 45min, 50min, 55min, 60min, etc.
[0087] Preferably, the monomer-containing pre-emulsion is prepared by the following steps:
[0088] (a) stirring and mixing an emulsifier and water to obtain a pre-emulsion; stirring and mixing a hard monomer, a soft elastomer, and a functional monomer to obtain a mixed monomer;
[0089] (b) The pre-emulsion and the mixed monomer are stirred and mixed to obtain a pre-emulsion containing the monomer.
[0090] Preferably, in step (a), the water accounts for 40-50% of the total mass of water in the raw materials for preparing the real stone paint emulsion, for example, it can be 40%, 42%, 44%, 46%, 48%, 50%, etc.
[0091] Preferably, in step (a), the stirring and mixing rotation speed is independently 100-200 rpm, for example, it can be 100 rpm, 120 rpm, 140 rpm, 160 rpm, 180 rpm, 200 rpm, etc., and the stirring and mixing time is independently 5-15 min, for example, it can be 5 min, 8 min, 10 min, 12 min, 15 min, etc.
[0092] Preferably, in step (b), the stirring and mixing speed is 500-600 rpm, for example, it can be 500 rpm, 520 rpm, 540 rpm, 560 rpm, 580 rpm, 600 rpm, etc., and the stirring and mixing time is 20-40 min, for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min, etc.
[0093] Preferably, the initiator solution is prepared by the following steps:
[0094] Mix 4-6% (eg 4%, 4.5%, 5%, 5.5%, 6%, etc.) of water accounting for the total mass of water in the raw materials for preparing the real stone paint emulsion with the initiator, stir and dissolve evenly with a glass rod, and set aside to obtain the initiator solution.
[0095] Preferably, the real stone paint emulsion is prepared by the following steps:
[0096] (A) heating water, and then mixing it with 0.5-3% (for example, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 2%, 3%, etc.) of the pre-emulsion containing monomers and 15-25% (for example, 15%, 16%, 18%, 20%, 22%, 25%, etc.) of the initiator solution to react and obtain an initial reaction solution;
[0097] (B) mixing the above-mentioned initial reaction liquid, 0.5-3% (for example, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 2%, 3%, etc.) of the total mass of the pre-emulsion containing monomers, and 5-15% (for example, 5%, 6%, 8%, 10%, 12%, 15%, etc.) of the initiator solution of the total mass of the initiator solution, reacting, and keeping warm to form the latex particle core of the real stone paint emulsion, and obtaining a polymerization reaction liquid;
[0098] (C) After mixing the slurry containing the ultraviolet blocking agent with the remaining pre-emulsion containing the monomer, the slurry is mixed with the above-mentioned polymerization reaction liquid, reacted, and aged to form a shell layer, thereby obtaining the real stone paint emulsion with a core-shell structure.
[0099] Preferably, in step (A), the heating temperature is 84-86°C, for example, it can be 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.
[0100] Preferably, in step (A), the reaction temperature is 84-86°C, for example, 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc., and the reaction time is 10-20min, for example, 10min, 12min, 14min, 16min, 18min, 20min, etc.
[0101] Preferably, in step (B), after the temperature of the initial reaction liquid is stabilized at 84-86°C (for example, 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.), the pre-emulsion containing monomers and the initiator solution are added dropwise to the initial reaction liquid.
[0102] Preferably, in step (B), the reaction temperature is 84-86°C (for example, 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.), and the reaction time is 2-3h (for example, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, etc.).
[0103] Preferably, in step (B), the insulation temperature is 84-86°C (for example, it can be 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.), and the insulation time is 20-40min (for example, it can be 20min, 25min, 30min, 35min, 40min, etc.).
[0104] Preferably, in step (C), the slurry containing the UV blocker is added to the remaining pre-emulsion containing the monomer and stirred for 15-25 min (15 min, 16 min, 18 min, 20 min, 22 min, 25 min, etc.), and then continued to be added dropwise to the above-mentioned polymerization reaction solution.
[0105] Preferably, in step (C), the dropping temperature is 84-86°C (for example, it can be 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.), and the dropping time is 0.8-1.2h (for example, it can be 0.8h, 0.9h, 1h, 1.1h, 1.2h, etc.).
[0106] Preferably, in step (C), the aging temperature is 84-86°C (for example, 84°C, 84.5°C, 85°C, 85.5°C, 86°C, etc.), and the aging time is 0.8-1.2h (for example, 0.8h, 0.9h, 1h, 1.1h, 1.2h, etc.).
[0107] Preferably, in step (C), after the aging, the step further comprises: adding any one or a combination of at least two of a pH regulator, a preservative or a defoaming agent to the reaction solution.
[0108] Preferably, in step (C), a filtering step is further included after the aging.
[0109] In a third aspect, the present invention provides a use of the real stone paint emulsion as described in the first aspect in preparing a paint film having hydrophobic and UV-blocking functions.
[0110] Compared with the prior art, the present invention has the following beneficial effects:
[0111] (1) The present invention is mainly embodied in the introduction of nano anti-ultraviolet interlayer agent, through the first step of preparing nano anti-ultraviolet slurry, and then through the core-shell polymerization process design, the nano anti-ultraviolet interlayer agent is loaded on the surface of the latex particles, thereby playing the effect of shielding ultraviolet rays;
[0112] (2) The present invention effectively improves the weather resistance of styrene acrylic real stone paint emulsion, and at the same time, the shell layer introduces functional monomers to effectively improve the water resistance and hardness of the paint film;
[0113] (3) The present invention improves the adhesion of the paint film to the substrate, and the prepared real stone paint emulsion has the characteristics of excellent paint stability and the like. DETAILED DESCRIPTION
[0114] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0115] Generally, the nomenclature and its technology used in conjunction with cell and tissue culture, molecular biology, immunology, microbiology, genetics, and protein and nucleic acid chemistry and hybridization described herein are those well-known and commonly used in the art. Unless otherwise indicated, the methods and techniques of the present invention are generally carried out according to conventional methods as well-known in the art, and as described in various general and more specific references, which are cited and discussed throughout this specification. Enzymatic reactions and purification techniques are carried out according to the manufacturer's specifications, as generally achieved in the art, or as described herein. The nomenclature and its laboratory procedures and technology used in conjunction with analytical chemistry, synthetic organic chemistry, and medical and pharmaceutical chemistry described herein are those well-known and commonly used in the art.
[0116] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0117] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0118] The following are some sources of raw materials in the examples:
[0119]
[0120]
[0121] Example 1
[0122] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0123]
[0124] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0125] S1: Deionized water, sodium polycarboxylate, mineral oil defoamer, ammonia water, and kasonite preservative were added into the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0126] S2: Slowly add nano-rutile titanium dioxide into a dispersion tank and disperse it at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0127] Example 2
[0128] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0129]
[0130] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0131] S1: Add deionized water, sulfate, mineral oil defoamer, ammonia water, and kasson preservative into the dispersion tank in sequence, and stir at 200 rpm for 5 min until the dispersion is uniform;
[0132] S2: Slowly add nano-rutile titanium dioxide into a dispersion tank and disperse it at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0133] Example 3
[0134] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0135]
[0136] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0137] S1: Deionized water, sodium sulfonate, mineral oil defoamer, ammonia water, and kassonite preservative were added to the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0138] S2: Slowly add nano-rutile titanium dioxide into a dispersion tank and disperse it at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0139] Example 4
[0140] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0141]
[0142]
[0143] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0144] S1: Deionized water, sodium sulfonate, mineral oil defoamer, ammonia water, and kassonite preservative were added to the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0145] S2: Slowly add anatase titanium dioxide into a dispersion tank and disperse at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0146] Example 5
[0147] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0148]
[0149] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0150] S1: Deionized water, sodium sulfonate, mineral oil defoamer, ammonia water, and kassonite preservative were added to the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0151] S2: Slowly add anatase titanium dioxide into a dispersion tank and disperse at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0152] Example 6
[0153] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0154]
[0155]
[0156] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0157] S1: Deionized water, sodium polycarboxylate, mineral oil defoamer, ammonia water, and kasonite preservative were added into the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0158] S2: Slowly add nano-rutile titanium dioxide into a dispersion tank and disperse it at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0159] Example 7
[0160] This embodiment provides a slurry containing an ultraviolet blocking agent. The raw materials for preparing the slurry containing an ultraviolet blocking agent include the following components in parts by mass:
[0161]
[0162] The slurry containing the ultraviolet blocking agent is prepared by the following method:
[0163] S1: Deionized water, sodium polycarboxylate, mineral oil defoamer, ammonia water, and kasonite preservative were added into the dispersion tank in sequence, and stirred at 200 rpm for 5 min until the dispersion was uniform;
[0164] S2: Slowly add nano-rutile titanium dioxide into a dispersion tank and disperse it at a high speed of 800 rpm for 50 minutes to obtain a slurry containing a UV blocker.
[0165] Example 8
[0166] This embodiment provides a slurry containing an ultraviolet blocking agent, which is different from Embodiment 1 only in that the particle size of the titanium dioxide is 10 nm.
[0167] Example 9
[0168] This embodiment provides a slurry containing an ultraviolet blocking agent, which is different from the embodiment 1 only in that the particle size of the titanium dioxide is 100 nm.
[0169] Example 10
[0170] This embodiment provides a slurry containing an ultraviolet blocking agent, which is different from Embodiment 1 only in that rutile titanium dioxide is replaced by an equal mass of nano zinc oxide.
[0171] Embodiment 11
[0172] This embodiment provides a slurry containing a UV blocking agent, which is different from Embodiment 1 only in that the mineral oil defoamer is replaced with an organosilicon defoamer of equal mass.
[0173] Example 12
[0174] This embodiment provides a slurry containing an ultraviolet blocking agent, which is different from Embodiment 1 only in that rutile titanium dioxide is replaced with an equal mass of a polyether-modified defoaming agent.
[0175] Embodiment 13
[0176] This embodiment provides a slurry containing a UV blocking agent, which is different from the embodiment 1 only in that, in the preparation process, mixing is not performed in steps, but in one step, and the mixing time is prolonged;
[0177] The slurry containing the ultraviolet blocking agent is prepared by the following method: deionized water, sodium polycarboxylate, mineral oil defoamer, ammonia water, kasonite preservative, and nano-rutile titanium dioxide are slowly added into a dispersion tank in sequence, and dispersed at a high speed of 800 rpm for 2 hours to obtain the slurry containing the ultraviolet blocking agent.
[0178] Test Example 1
[0179] Stability test
[0180] Test sample: slurry containing UV blocker prepared in Examples 1 to 13;
[0181] Test method: Take a small amount of slurry in a centrifuge test tube and put it in a centrifuge for centrifugal separation. Generally, they are centrifuged at the same speed for the same time and then taken out and observed. If the emulsion cannot be separated at the maximum speed of the centrifuge, you can dilute the emulsion and test its stability. Usually the slurry is divided into two layers, the upper layer is the liquid layer, and the lower layer is the white precipitate. Calculate the precipitation rate of the precipitation amount of the lower layer. The smaller the precipitation rate, the better the stability.
[0182] The sedimentation rate (%) is calculated according to the following formula:
[0183]
[0184] Where: Q1—emulsion precipitation mass; Q2—actual solid mass of emulsion;
[0185] The test results are shown in Table 1 below:
[0186] Table 1
[0187]
[0188] From the test data in Table 1, it can be seen that the sedimentation rate of the slurry containing the UV blocker prepared by the present invention is below 0.1%, and the stability is excellent. Among them, from the comparison of Examples 1-3, it can be seen that the slurry containing the UV blocker with the best stability is the dispersing wetting agent of sodium sulfonate. From the comparison of Examples 3-5, it can be seen that the addition ratio of 40-50% nano titanium dioxide is more stable.
[0189] Embodiment 14
[0190] This embodiment provides a real stone paint emulsion, and the raw materials for preparing the real stone paint emulsion include the following components in parts by mass:
[0191]
[0192]
[0193] The real stone paint emulsion is prepared by the following method:
[0194] Preparation of S1 pre-emulsion: Stir 2 / 3 of anionic emulsifier, water and acrylamide for 10 minutes at room temperature and pressure;
[0195] Preparation of S2 mixed monomer: Styrene, butyl acrylate and acrylic acid were mixed and stirred for 10 minutes at room temperature and pressure for later use;
[0196] Preparation of S3 pre-emulsion: Add S2 to S1 at room temperature and stir at high speed for 30 minutes for later use;
[0197] Preparation of S4 initiator solution: at room temperature and pressure, add deionized water and ammonium persulfate according to the formula, stir until the initiator is completely dissolved for later use;
[0198] At room temperature and pressure, add deionized water according to the formula to the reactor of S5, raise the temperature to 85°C, add 1% S3 solution and 1 / 5 S4 solution, react for 15 minutes, and wait until the temperature stabilizes at 85±1°C, then start to drip the remaining S3 and S4, and drip the remaining materials for 3.5 hours. When the dripping time is 2.5 hours, stop dripping S3 and S4, and start keeping warm for 30 minutes. Add nano UV slurry and triethyltrimethoxysilane to S3, stir for 20 minutes and continue to drip. After the dripping is completed for 1 hour, then keep warm and mature for 1 hour to ensure the yield of the monomer, then cool to below 45°C, add ammonia water, Kathon preservative, and mineral oil defoaming agent, stir for 10 minutes, and filter the material to obtain the real stone paint emulsion.
[0199] Embodiment 15
[0200] This embodiment provides a real stone paint emulsion, and the raw materials for preparing the real stone paint emulsion include the following components in parts by mass:
[0201]
[0202]
[0203] The real stone paint emulsion is prepared by the following method:
[0204] Preparation of S1 pre-emulsion: Stir 2 / 3 of anionic emulsifier, water and acrylamide for 10 minutes at room temperature and pressure;
[0205] Preparation of S2 mixed monomer: Styrene, butyl acrylate and acrylic acid were mixed and stirred for 10 minutes at room temperature and pressure for later use;
[0206] Preparation of S3 pre-emulsion: Add S2 to S1 at room temperature and stir at high speed for 30 minutes for later use;
[0207] Preparation of S4 initiator solution: at room temperature and pressure, add deionized water and ammonium persulfate according to the formula, stir until the initiator is completely dissolved for later use;
[0208] At room temperature and pressure, add deionized water according to the formula to the reactor of S5, raise the temperature to 85°C, add 1% S3 solution and 1 / 5 S4 solution, react for 15 minutes, and wait until the temperature stabilizes at 85±1°C, then start to drip the remaining S3 and S4, and drip the remaining materials for 3.5 hours. When the dripping time is 2.5 hours, stop dripping S3 and S4, and start keeping warm for 30 minutes. Add nano UV slurry and triethyltrimethoxysilane to S3, stir for 20 minutes and continue to drip. After the dripping is completed for 1 hour, then keep warm and mature for 1 hour to ensure the yield of the monomer, then cool to below 45°C, add ammonia water, Kathon preservative, and mineral oil defoaming agent, stir for 10 minutes, and filter the material to obtain the real stone paint emulsion.
[0209] Example 16
[0210] This embodiment provides a real stone paint emulsion, and the raw materials for preparing the real stone paint emulsion include the following components in parts by mass:
[0211]
[0212] The real stone paint emulsion is prepared by the following method:
[0213] Preparation of S1 pre-emulsion: Stir 2 / 3 of anionic emulsifier, water and acrylamide for 10 minutes at room temperature and pressure;
[0214] Preparation of S2 mixed monomer: Styrene, butyl acrylate and acrylic acid were mixed and stirred for 10 minutes at room temperature and pressure for later use;
[0215] Preparation of S3 pre-emulsion: Add S2 to S1 at room temperature and stir at high speed for 30 minutes for later use;
[0216] Preparation of S4 initiator solution: at room temperature and pressure, add deionized water and ammonium persulfate according to the formula, stir until the initiator is completely dissolved for later use;
[0217] At room temperature and pressure, add deionized water according to the formula to the reactor of S5, raise the temperature to 85°C, add 1% S3 solution and 1 / 5 S4 solution, react for 15 minutes, and wait until the temperature stabilizes at 85±1°C, then start to drip the remaining S3 and S4, and drip the remaining materials for 3.5 hours. When the dripping time is 2.5 hours, stop dripping S3 and S4, and start keeping warm for 30 minutes. Add nano UV slurry and triethyltrimethoxysilane to S3, stir for 20 minutes and continue to drip. After the dripping is completed for 1 hour, then keep warm and mature for 1 hour to ensure the yield of the monomer, then cool to below 45°C, add ammonia water, Kathon preservative, and mineral oil defoaming agent, stir for 10 minutes, and filter the material to obtain the real stone paint emulsion.
[0218] Embodiment 17
[0219] This embodiment provides a real stone paint emulsion, which is different from Example 13 only in that the nano anti-UV slurry prepared in Example 4 is replaced by the nano anti-UV slurry prepared in Example 10 (the UV blocker is nano zinc oxide).
[0220] Embodiment 18
[0221] This embodiment provides a real stone paint emulsion, which is different from Example 13 only in that no acrylic acid is added and the acrylamide content is increased to 4 parts.
[0222] Embodiment 19
[0223] This embodiment provides a real stone paint emulsion, which is different from Example 13 only in that acrylamide is not added and the acrylic acid content is increased to 4 parts.
[0224] Embodiment 20
[0225] This embodiment provides a real stone paint emulsion, which is different from Embodiment 13 only in that 2 parts of acrylic acid are replaced by 2 parts of glyceryl methacrylate.
[0226] Embodiment 21
[0227] This embodiment provides a real stone paint emulsion, which is different from Embodiment 13 only in that 2 parts of acrylamide are replaced by 2 parts of glyceryl methacrylate.
[0228] Embodiment 22
[0229] This embodiment provides a real stone paint emulsion, which is different from Example 13 only in that 1 part of triethyltrimethoxysilane is replaced by 1 part of γ-(methacryloyloxy)propyltrimethoxysilane.
[0230] Embodiment 23
[0231] This embodiment provides a real stone paint emulsion, which is different from embodiment 13 only in that S5 directly reacts S3 and S4 solutions without pre-seed solution reaction;
[0232] That is, at room temperature and pressure, deionized water is added to the reactor according to the amount of the formula, the temperature is raised to 85°C, and the remaining S3 and S4 are added dropwise. After 2.5 hours of addition, the addition of S3 and S4 is stopped, and the temperature is kept warm for 30 minutes. Nano-UV slurry and triethyltrimethoxysilane are added to S3 and stirred for 20 minutes and then continued to be added dropwise. After the addition is completed for 1 hour, the mixture is kept warm for 1 hour to ensure the yield of the monomer, and then the temperature is lowered to below 45°C, ammonia water, Kathon preservative, and mineral oil defoaming agent are added, and after stirring for 10 minutes, the material is filtered to obtain a real stone paint emulsion.
[0233] Comparative Example 1
[0234] This comparative example provides a real stone paint emulsion, which differs from Example 14 only in that no nano anti-UV slurry is added.
[0235] Comparative Example 2
[0236] This comparative example provides a real stone paint emulsion, which differs from Example 14 only in that acrylic acid and acrylamide are not added, and the content of triethyltrimethoxysilane is increased to 5 parts.
[0237] Comparative Example 3
[0238] This comparative example provides a real stone paint emulsion, which differs from Example 14 only in that triethyltrimethoxysilane is not added, the acrylic acid content is increased to 2.5 parts, and the acrylamide content is increased to 2.5 parts.
[0239] Comparative Example 4
[0240] This comparative example provides a real stone paint emulsion, which is different from Example 14 only in that the nano anti-ultraviolet slurry prepared in Example 4 is directly polymerized during the preparation of S5; the specific steps are as follows: S5 is added with deionized water according to the amount of the formula to the reactor at room temperature and pressure, the temperature is raised to 85°C, 1% S3 solution and 1 / 5 S4 solution are added, and the reaction is carried out for 15 minutes. When the temperature is stabilized at 85±1°C, the remaining S3, S4 and nano ultraviolet slurry are added dropwise, and the remaining materials are added dropwise for 3.5 hours. When the addition is continued for 2.5 hours, the addition of S3 and S4 is stopped, and then the mixture is kept warm and matured for 1 hour to ensure the yield of the monomer, and then the temperature is lowered to below 45°C, ammonia water, Kathon preservative, and mineral oil defoaming agent are added, and after stirring for 10 minutes, the material is filtered to obtain the real stone paint emulsion.
[0241] Test Example 2
[0242] Pulp physiochemical testing
[0243] Test samples: the real stone paint emulsions provided in Examples 14-23 and the real stone paint emulsions provided in Comparative Examples 1-4;
[0244] The test items and corresponding test instruments are as follows:
[0245]
[0246] The test results are shown in Table 2 below:
[0247] Table 2
[0248] Group Particle size (nm) Solid content% MFFT(℃) Gel volume (%) Embodiment 14 108 48.20% 20 0.08% Embodiment 15 109 48.30% 21 0.15% Example 16 105 48.50% 22 0.12% Embodiment 17 105 48.30% 22 0.80% Embodiment 18 105 48.20% 22 0.60% Embodiment 19 108 48.21% 22 0.45% Embodiment 20 110 48.30% 22 0.60% Embodiment 21 114 48.20% 22 0.40% Embodiment 22 105 48.20% 22 0.18% Embodiment 23 100 48.15% 22 0.80% Comparative Example 1 106 48.40% 21 0.26% Comparative Example 2 120 48.20% 22 1.50% Comparative Example 3 104 48.0% 23 0.60% Comparative Example 4 110 48.30% 22 1.60%
[0249] From the test data in Table 2, it can be seen that the particle size of the real stone paint emulsion provided by the present invention is 100-110nm, the solid content is 48.2-48.5%, the MFFT is 20-22%, and the gel content is less than 0.1%. Among them, in terms of gel content, Example 14 is the best and the polymerization is the most stable.
[0250] Test Example 3
[0251] Application Testing
[0252] Test samples: the real stone paint emulsions provided in Examples 14-23 and the real stone paint emulsions provided in Comparative Examples 1-4;
[0253] Test method:
[0254] 1. The test method for the initial water whitening resistance of the emulsion is to make a film on a glass plate using a 50μm wet film former, dry it in an oven with air blast at 50℃ for 30 minutes, take it out and cool it to room temperature, soak it in water, observe the water whitening resistance of the emulsion film, and record the experimental phenomena.
[0255] 2. The bonding strength test method shall be carried out in accordance with 7.17 of standard JG / T24-2018.
[0256] 3. The water resistance test method shall be carried out in accordance with 7.13 of standard JG / T24-2018.
[0257] 4. The test method for resistance to artificial aging shall be carried out in accordance with the provisions of cycle A in standard GB / T1865-2009, and the evaluation of the results shall be carried out in accordance with GB / T1766.
[0258] 5. Alkali resistance test method: test according to 7.14 of standard JG / T24-2018.
[0259] 6. The water absorption test shall be carried out in accordance with the provisions of Appendix A of JG / T157-2009, and the immersion time shall be 2 hours.
[0260] The test results are shown in Table 3 below:
[0261] Table 3
[0262]
[0263]
[0264] It can be seen from the data in Table 3 that the overall indicators are better than the control samples in terms of water resistance, water absorption rate and bonding strength, especially in terms of resistance to artificial aging. Therefore, by introducing anti-UV nano-slurry into emulsion polymerization, and then through special process design and particle size structure design, the real stone paint emulsion is finally prepared. It effectively improves the yellowing resistance and poor weather resistance of styrene acrylic real stone paint. From the perspective of product economic benefits, it has far-reaching development value.
[0265] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a real stone paint emulsion, characterized in that: The preparation method is: Preparation of a slurry containing a UV blocker: (1) stirring and mixing water and a dispersing wetting agent to obtain a dispersion; (2) stirring and mixing a UV blocker and the above dispersion to obtain a slurry containing a UV blocker; The raw materials for preparing the slurry containing the ultraviolet blocker include the following components by weight: 40-70 parts of ultraviolet blocker, 0.05-1 parts of dispersing and wetting agent, and 30-60 parts of water; the ultraviolet blocker includes nano-grade titanium dioxide; Preparation of mixed monomer solution: (a) stirring and mixing an emulsifier and water to obtain a pre-emulsion; stirring and mixing a hard monomer, a soft monomer, and a functional monomer to obtain a mixed monomer; (b) stirring and mixing the pre-emulsion and the mixed monomer to obtain a pre-emulsion containing the monomer; Preparation of initiator solution: Mix the initiator and part of water in the raw materials for preparing the real stone paint emulsion to obtain an initiator solution; Preparation of real stone paint emulsion: (A) After heating water, mix it with 0.5-3% of the total mass of the pre-emulsion containing monomers and 15-25% of the total mass of the initiator solution to react and obtain an initial reaction solution; (B) mix the above initial reaction solution, 0.5-3% of the total mass of the pre-emulsion containing monomers and 5-15% of the total mass of the initiator solution to react and keep warm to form the latex particle core of the real stone paint emulsion to obtain a polymerization reaction solution; (C) mix the slurry containing ultraviolet blocker with the remaining pre-emulsion containing monomers, and then mix it with the above polymerization reaction solution to react and mature to form a shell layer to obtain a real stone paint emulsion with a core-shell structure; The real stone paint emulsion has a core-shell structure; the shell layer of the core-shell structure includes an ultraviolet blocker and a functional monomer; the functional monomer includes a functional monomer having a hydrophobic group and a functional monomer having a hydrophilic group; The raw materials for preparing the real stone paint emulsion include the following components by weight: 1-10 parts of slurry containing ultraviolet blocker, 1-10 parts of functional monomer, 15-25 parts of hard monomer, 15-25 parts of soft monomer, 0.1-5 parts of emulsifier, 0.05-1 parts of initiator, and 40-55 parts of water; Wherein, the functional monomers having hydrophilic groups include acrylic acid and acrylamide; the functional monomers having hydrophobic groups include triethyltrimethoxysilane and / or γ -(methacryloyloxy)propyltrimethoxysilane; the hard monomer is styrene; and the soft monomer is butyl acrylate.
2. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The particle size of the nano-scale titanium dioxide is 10-100 nm.
3. The method for preparing the real stone paint emulsion according to claim 2, characterized in that: The particle size of the nano-scale titanium dioxide is 15-50 nm.
4. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The nano-scale titanium dioxide includes rutile nano-titanium dioxide and / or anatase nano-titanium dioxide.
5. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The mass ratio of the functional monomer having a hydrophobic group to the functional monomer having a hydrophilic group in the functional monomer is (3-5):
1.
6. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The emulsifier includes any one of anionic emulsifier, nonionic emulsifier or anionic and nonionic emulsifier or a combination of at least two of them.
7. The method for preparing the real stone paint emulsion according to claim 6, characterized in that: The anionic emulsifier includes any one of sodium fatty alcohol polyoxyethylene ether sulfate, sodium modified alkyl alcohol sulfonate, sodium dodecylbenzene sulfonate or sodium dodecyl sulfate, or a combination of at least two thereof.
8. The method for preparing the real stone paint emulsion according to claim 6, characterized in that: The nonionic emulsifier includes any one of polyoxyethylene ether, propylene oxide block copolymer or polyol fatty acid ester or a combination of at least two thereof.
9. The method for preparing the real stone paint emulsion according to claim 6, characterized in that: The anionic nonionic emulsifier includes any one of polyoxyethylene nonylphenol succinate disodium, ethoxylated alcohol sulfosuccinate disodium or polyoxyethylene nonylphenol ether, or a combination of at least two thereof.
10. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The initiator includes any one of sodium persulfate, ammonium persulfate or potassium persulfate, or a combination of at least two of them.
11. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts of a defoaming agent.
12. The method for preparing the real stone paint emulsion according to claim 11, characterized in that: The defoamer includes any one of an organosilicon defoamer, a mineral oil defoamer or a polyether modified defoamer, or a combination of at least two of them.
13. The method for preparing the real stone paint emulsion according to claim 12, characterized in that: The organosilicon defoamer includes any one of trimethyl silicone oil, dimethyl polysiloxane, silicone paste or polysiloxane, or a combination of at least two thereof.
14. The method for preparing the real stone paint emulsion according to claim 12, characterized in that: The mineral oil defoamer includes any one of white oil, liquid wax or naphthenic oil or a combination of at least two of them.
15. The method for preparing the real stone paint emulsion according to claim 12, characterized in that: The polyether-modified defoaming agent includes polyether-modified polysiloxane.
16. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts of preservatives.
17. The method for preparing the real stone paint emulsion according to claim 16, characterized in that: The preservatives include Kathon and / or BIT.
18. The method for preparing the real stone paint emulsion according to claim 17, characterized in that: The BIT includes BIT10 and / or BIT20.
19. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the real stone paint emulsion also include 0.05-0.5 parts of a pH regulator.
20. The method for preparing the real stone paint emulsion according to claim 19, characterized in that: The pH adjuster is an alkaline pH adjuster.
21. The method for preparing the real stone paint emulsion according to claim 20, characterized in that: The pH regulator is any one of ammonia water, AMP-95 or triethanolamine, or a combination of at least two of them.
22. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The water is deionized water, and the conductivity of the deionized water is less than 10 μS / cm.
23. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In the raw materials for preparing the slurry containing the ultraviolet blocking agent, the dispersing wetting agent is selected from any one of sulfate wetting agents, polycarboxylate wetting agents or sulfonate wetting agents, or a combination of at least two thereof.
24. The method for preparing the real stone paint emulsion according to claim 23, characterized in that: The dispersing wetting agent is a sulfonate wetting agent.
25. The method for preparing the real stone paint emulsion according to claim 23, characterized in that: The sulfate ester wetting agent is selected from any one of sodium lauryl sulfate, sodium polyoxyethylene fatty alcohol ether sulfate or sodium polyoxyethylene fatty amine sulfate, or a combination of at least two thereof.
26. The method for preparing the real stone paint emulsion according to claim 23, characterized in that: The polycarboxylate wetting agent is selected from any one of sodium polyacrylate, sodium polymethacrylate or maleic acid-sodium acrylate or a combination of at least two thereof.
27. The method for preparing the real stone paint emulsion according to claim 23, characterized in that: The sulfonate wetting agent is selected from any one of sodium dodecylbenzenesulfonate, sodium butylnaphthalenesulfonate or sodium aminobenzenesulfonate or a combination of at least two thereof.
28. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.1-0.2 parts of a defoaming agent.
29. The method for preparing the real stone paint emulsion according to claim 28, characterized in that: The defoamer includes any one of an organosilicon defoamer, a mineral oil defoamer or a polyether modified defoamer, or a combination of at least two of them.
30. The method for preparing the real stone paint emulsion according to claim 29, characterized in that: The organosilicon defoamer includes any one of trimethyl silicone oil, dimethyl polysiloxane, silicone paste or polysiloxane, or a combination of at least two thereof.
31. The method for preparing the real stone paint emulsion according to claim 29, characterized in that: The mineral oil defoamer includes any one of white oil, liquid wax or naphthenic oil or a combination of at least two of them.
32. The method for preparing the real stone paint emulsion according to claim 29, characterized in that: The polyether-modified defoaming agent includes polyether-modified polysiloxane.
33. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.05-0.1 parts of preservatives.
34. The method for preparing the real stone paint emulsion according to claim 33, characterized in that: The preservatives include Kathon and / or BIT.
35. The method for preparing the real stone paint emulsion according to claim 34, characterized in that: The BIT includes BIT10 and / or BIT20.
36. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The raw materials for preparing the slurry containing the ultraviolet blocking agent also include 0.1-0.2 parts of a pH regulator.
37. The method for preparing the real stone paint emulsion according to claim 36, characterized in that: The pH adjuster is an alkaline pH adjuster.
38. The method for preparing the real stone paint emulsion according to claim 37, characterized in that: The pH regulator is any one of ammonia water, AMP-95 or triethanolamine, or a combination of at least two of them.
39. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (1), any one of a defoaming agent, a preservative or a pH adjuster or a combination of at least two thereof is also added.
40. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (1), the stirring and mixing speed is 200-300 rpm, and the stirring and mixing time is 4-6 min.
41. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (2), the stirring and mixing speed is 800-1000 rpm, and the stirring and mixing time is 40-60 min.
42. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (a), the water accounts for 40-50% of the total mass of water in the raw materials for preparing the real stone paint emulsion.
43. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (a), the rotation speed of the stirring and mixing is independently 100-200 rpm, and the time of the stirring and mixing is independently 5-15 min.
44. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (b), the stirring and mixing speed is 500-600 rpm, and the stirring and mixing time is 20-40 min.
45. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: The initiator solution is prepared by the following steps: The water accounting for 4-6% of the total mass of water in the raw materials for preparing the real stone paint emulsion and the initiator are mixed and stirred with a glass rod to dissolve and then set aside to obtain the initiator solution.
46. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (A), the heating temperature is 84-86°C; In step (A), the reaction temperature is 84-86° C., and the reaction time is 10-20 min.
47. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (B), after the temperature of the initial reaction liquid is stabilized at 84-86° C., the pre-emulsion containing the monomer and the initiator solution are added dropwise to the initial reaction liquid; In step (B), the reaction temperature is 84-86° C., and the reaction time is 2-3 h; the insulation temperature is 84-86° C., and the insulation time is 20-40 min.
48. The method for preparing the real stone paint emulsion according to claim 1, characterized in that: In step (C), the slurry containing the UV blocker is added to the remaining pre-emulsion containing the monomer and stirred for 15-25 minutes, and then continued to be added dropwise to the above polymerization reaction solution; And / or, in step (C), the temperature of the dropping is 84-86°C, and the time of the dropping is 0.8-1.2 h; And / or, in step (C), the aging temperature is 84-86°C, and the aging time is 0.8-1.2 h; And / or, in step (C), after the aging, the step further comprises: adding any one or a combination of at least two of a pH regulator, a preservative or a defoaming agent to the reaction solution; And / or, in step (C), the aging further includes a filtering step.
49. Use of the real stone paint emulsion prepared according to the method according to any one of claims 1 to 48 in preparing a paint film having hydrophobic and UV-blocking functions.