A polymer anti-corrosion composite cable tray
Through the preparation and combination technology of modified nylon materials, the corrosion resistance and low-temperature performance of cable trays in complex environments are solved, and the corrosion resistance and low-temperature toughness of polymer anti-corrosion composite cable trays are improved, satisfying a variety of Use requirements in the environment.
Patent Information
- Application Number
- CN202310675730.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-06-08
AI Technical Summary
The existing cable trays are insufficient in complex external environments, especially the high water absorption of nylon materials, resulting in a decrease in mechanical properties, which is difficult to meet the needs of use in various environments.
Using modified nylon as the substrate for the corrosion-resistant protective layer, a double bond-containing fluorinated monomer is prepared by the reaction of allyl chloride and trifluoroethanol, and polymerized with allyl glycidyl ether to form a copolymerization modifier, followed by React with liquid nylon ring opening, introduce fluorine-containing groups to form highly hydrophobic and toughened modified nylon, and combine with ultramicrofillers, flame retardants and antioxidants to form a buffer foam layer and a corrosion-resistant protective layer .
It achieves excellent corrosion resistance and low-temperature toughness of modified nylon-based materials, broadens the temperature range of cable trays, avoids damage to corrosion, and meets the use needs in various environments.
Smart Images

Figure BDA0004274530650000091 
Figure BDA0004274530650000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable bridges, and in particular relates to a polymer anti-corrosion composite cable bridge. Background Art
[0002] Cable trays use their own structural characteristics to attach and fix cables to buildings or independently support cables for passage in tunnels or caves, underground, in the air, etc., thereby supporting, protecting and managing the cables. Therefore, the structural stability of the cable tray will directly determine the safety of cable use; since the cable tray is in direct contact with the complex external environment, the cable tray must have good corrosion resistance.
[0003] There are two main types of cable trays in the prior art. One is the bare cable tray, which is mainly made of hot-dip galvanized steel, stainless steel and aluminum alloy. It has good corrosion resistance and simple production process. It is generally used for indoor cable laying. The other is the composite cable tray, which is coated with an anti-corrosion layer on the surface of the metal substrate to achieve the effect of isolation and protection. Generally, glass fiber modified epoxy resin protective coating is used more, but it is brittle and has poor weather resistance, and its protective performance for cable trays is average. Nylon has good corrosion resistance and wear resistance, and has excellent application prospects in anti-corrosion materials. However, nylon has high water absorption, which leads to a decrease in mechanical properties, especially in low temperature environments. Therefore, this application is based on nylon materials to prepare a polymer anti-corrosion composite cable tray. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a polymer anti-corrosion composite cable tray.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A polymer anti-corrosion composite cable bridge, comprising a load-bearing substrate, the surface of which is sequentially composited with a buffer foam layer and a corrosion-resistant protective layer;
[0007] The buffer foam layer is formed by foaming organic silicon foam;
[0008] The corrosion resistant protective layer comprises, by weight:
[0009] 100 parts of modified nylon, 1.8-2.5 parts of ultrafine filler, 3.2-4 parts of flame retardant and 0.6-0.9 parts of antioxidant.
[0010] The modified nylon is prepared by the following method:
[0011] Step A1: trifluoroethanol, triethylamine and acetone are mixed, and the mixture is kept constant at 5-10°C in an ice-water bath, and mechanically stirred at 240-360 rpm, and allyl chloride is slowly added, and triethylamine is used as an acid-binding agent, and allyl chloride and trifluoroethanol are substituted. The reaction time is controlled to be 5-7 hours. After the reaction is completed, low-boiling substances including acetone are removed by rotary evaporation, and deionized water is added for washing. The organic phase is taken and dried over anhydrous sodium sulfate to obtain a fluorinated monomer;
[0012] Furthermore, the usage ratio of trifluoroethanol, allyl chloride, triethylamine and acetone is 0.1 mol: 0.12-0.14 mol: 3.5-4.5 mL: 40-50 mL.
[0013] Step A2: allyl glycidyl ether, fluorinated monomer and dioxane are mixed, the temperature is raised to 62-68° C., mechanical stirring is performed at 120-180 rpm, azobisisobutyronitrile is added intermittently, and the fluorinated monomer and allyl glycidyl ether are reacted under the initiation of azobisisobutyronitrile. The reaction time is controlled to be 1.5-2.2 hours. After the reaction is completed, the dioxane is removed by vacuum rotary evaporation to obtain a copolymer modifier;
[0014] Furthermore, the usage ratio of allyl glycidyl ether, fluorinated monomer, azobisisobutyronitrile and dioxane is 0.1 mol: 25-40 mmol: 0.1-0.14 g: 120-150 mL.
[0015] Step A3: Mix the copolymer modifier and the toluene solution of aluminum trifluoromethanesulfonate, heat to 45-50° C. and stir to activate for 10-15 minutes, then add liquid nylon and tetrahydrofuran, mix, continue to heat to 65-75° C. and reflux reaction, under the catalysis of aluminum trifluoromethanesulfonate, the epoxy groups in the copolymer modifier molecules and the amide structures in the nylon molecules undergo a ring-opening reaction, the reflux reaction time is controlled to be 2-3 hours, and after the reaction is completed, the tetrahydrofuran is removed by rotary evaporation to obtain modified nylon;
[0016] Furthermore, the usage ratio of liquid nylon, copolymer modifier, aluminum trifluoromethanesulfonate and tetrahydrofuran is 100g:18-25g:1.3-1.7g:150-200mL.
[0017] Furthermore, the ultrafine filler is selected from one or more of silicon dioxide, boron nitride and mica powder, and the fineness is not less than 1000 mesh.
[0018] Furthermore, the flame retardant is selected from melamine cyanurate.
[0019] Furthermore, the antioxidant is a mixture of the antioxidant 1010 and the antioxidant 168 .
[0020] A method for preparing a polymer anti-corrosion composite cable tray comprises the following steps:
[0021] Step S1: clean the supporting substrate, coat the surface with organic silicone foam, bake and foam to shape, and buffer the foam layer to obtain a prefabricated part;
[0022] Step S2: Evenly mix the modified nylon, ultrafine filler, flame retardant and antioxidant, apply them on the surface of the preform, place it in a vacuum oven, bake it at 60-70°C for 2-3h, and then send it into a molding machine, control the mold temperature to 95-110°C, the pressure to 1.2-1.5MPa, and maintain the pressure for 4-6min to form a corrosion-resistant protective layer to obtain a polymer anti-corrosion composite cable tray.
[0023] Beneficial effects of the present invention:
[0024] 1. The present invention provides a composite cable tray, which has no strict requirements on the corrosion resistance of the bearing substrate and does not require the use of expensive corrosion-resistant alloy materials. The buffer foam layer can disperse external impacts and avoid damage to the anti-corrosion layer. The corrosion-resistant protective layer uses modified nylon as the base material and shows excellent corrosion resistance and low-temperature toughness in the test, which can meet the use of the cable tray in most environments.
[0025] 2. The present invention discloses a method for preparing modified nylon. A fluorinated monomer containing a double bond is prepared by a substitution reaction between allyl chloride and trifluoroethanol, and then the fluorinated monomer is polymerized with allyl glycidyl ether in azobisisobutyronitrile to form a copolymer modifier containing a chain olefin structure. At the same time, an active epoxy group is introduced into the side chain. Then, aluminum trifluoromethanesulfonate is used as a catalyst to perform a ring-opening reaction between the copolymer modifier and liquid nylon to introduce a fluorine-containing group between nylon molecular chains, thereby improving the hydrophobic and oil-repellent ability of nylon, improving the corrosion resistance of nylon, and reducing the water absorption rate of nylon. At the same time, the chain olefin structure toughens the nylon, greatly improving the low-temperature mechanical properties of the nylon-based corrosion-resistant protective layer, and broadening the use temperature range of the cable tray. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] This embodiment prepares a polymer anti-corrosion composite cable tray, and the specific implementation process is as follows:
[0029] 1) Preparation of modified nylon
[0030] 1.1. Take trifluoroethanol, triethylamine and acetone as feed materials, apply mechanical stirring to mix evenly, use ice water bath to control the temperature to be constant at 10°C, supplemented by 360rpm mechanical stirring, slowly and uniformly add allyl chloride within 2 hours, continue to stir and react at constant temperature after complete addition, and control the total addition reaction time of allyl chloride to be 5 hours, wherein the amount ratio of trifluoroethanol, allyl chloride, triethylamine and acetone is 0.1mol:0.14mol:4.5mL:50mL. After the reaction, remove the solvent acetone, excess allyl chloride and other low-boiling substances by rotary evaporation, then add deionized water twice the mass of the rotary evaporation substrate, stir and wash, take the organic phase, dry it with anhydrous sodium sulfate as a water absorbent, filter out the water absorbent, and obtain the fluorinated monomer.
[0031] 1.2. Take allyl glycidyl ether, fluorinated monomer and dioxane as feed materials, apply mechanical stirring to mix evenly, heat to 68°C, and stir mechanically at 180rpm. Add azobisisobutyronitrile intermittently in two times with an interval of 50min. After the addition is complete, continue to keep warm and stir to react. Control the total addition reaction time of azobisisobutyronitrile to be 1.5h. Among them, the amount ratio of allyl glycidyl ether, fluorinated monomer, azobisisobutyronitrile and dioxane is 0.1mol:40mmol:0.14g:150mL. After the reaction is completed, remove dioxane by reduced pressure rotary evaporation to obtain a copolymer modifier.
[0032] 1.3. Dissolve aluminum trifluoromethanesulfonate in toluene, stir and mix with the copolymer modifier, heat to 50°C and stir to activate for 10 min, then take liquid nylon (provided by Dongguan Baolimei Plastic Co., Ltd., the following examples use the same batch of raw materials) and tetrahydrofuran, add and mix, continue to heat to 75°C and reflux for 2h, wherein the amount ratio of liquid nylon, copolymer modifier, aluminum trifluoromethanesulfonate and tetrahydrofuran is 100g:25g:1.7g:200mL, and the reaction is completed by rotary evaporation to remove tetrahydrofuran to obtain modified nylon.
[0033] 2) Preparation of polymer anti-corrosion composite cable tray
[0034] 2.1. Take Q235 stamping profiled plate as the bearing substrate, degrease and ceramicize the surface in sequence, clean the surface, coat the surface with silicone foam (provided by Shanghai Mingchengjin Material Technology Co., Ltd., the following examples use the same batch of raw materials), place it in an oven, and foam it at a constant temperature of 65°C to form a buffer foam layer to obtain a prefabricated part.
[0035] 2.2. Mix nano silicon dioxide and 1200 mesh boron nitride powder in a weight ratio of 1:2 as ultrafine filler, and take 2.2 parts of ultrafine filler;
[0036] Take melamine cyanurate as a flame retardant, and take 3.2 parts of the flame retardant;
[0037] Take antioxidant 1010 and antioxidant 168 in a weight ratio of 3:1 as an antioxidant, and take 0.9 parts of antioxidant;
[0038] Take 100 parts of the modified nylon prepared above;
[0039] The above raw materials are mixed evenly, then coated on the surface of the preform, placed in a vacuum oven, and baked at 70°C for 2 hours. After that, it is sent to a molding machine, the mold temperature is controlled at 110°C, the pressure is 1.2MPa, and the pressure is maintained for 4 minutes to form a corrosion-resistant protective layer to obtain a polymer anti-corrosion composite cable tray.
[0040] Example 2
[0041] This embodiment prepares a polymer anti-corrosion composite cable tray, and the specific implementation process is as follows:
[0042] 1) Preparation of modified nylon
[0043] 1.1. Take trifluoroethanol, triethylamine and acetone as feed materials, apply mechanical stirring to mix evenly, use ice water bath to control the temperature to be constant at 5°C, supplemented by 240rpm mechanical stirring, slowly and uniformly add allyl chloride within 3 hours, continue to stir and react at constant temperature after complete addition, and control the total addition reaction time of allyl chloride to be 7 hours, wherein the amount ratio of trifluoroethanol, allyl chloride, triethylamine and acetone is 0.1mol:0.12mol:3.5mL:40mL. After the reaction, remove the solvent acetone, excess allyl chloride and other low-boiling substances by rotary evaporation, then add deionized water twice the mass of the rotary evaporation substrate, stir and wash, take the organic phase, dry it with anhydrous sodium sulfate as a water absorbent, filter out the water absorbent, and obtain the fluorinated monomer.
[0044] 1.2. Take allyl glycidyl ether, fluorinated monomer and dioxane as feed materials, apply mechanical stirring to mix evenly, raise the temperature to 62°C, and stir mechanically at 120rpm. Add azobisisobutyronitrile intermittently in 3 times with an interval of 30min. After the addition is complete, continue to keep warm and stir to react. The total addition reaction time of azobisisobutyronitrile is controlled to be 2.2h. Among them, the amount ratio of allyl glycidyl ether, fluorinated monomer, azobisisobutyronitrile and dioxane is 0.1mol:25mmol:0.1g:120mL. After the reaction is completed, remove dioxane by reduced pressure rotary evaporation to obtain a copolymer modifier.
[0045] 1.3. Dissolve aluminum trifluoromethanesulfonate in toluene, and then stir and mix with the copolymer modifier. Heat to 45°C and stir to activate for 15 minutes. Then, add liquid nylon and tetrahydrofuran and mix. Continue to heat to 65°C and reflux for 3 hours. The amount ratio of liquid nylon, copolymer modifier, aluminum trifluoromethanesulfonate and tetrahydrofuran is 100g:18g:1.3g:150mL. After the reaction, remove tetrahydrofuran by rotary evaporation to obtain modified nylon.
[0046] 2) Preparation of polymer anti-corrosion composite cable tray
[0047] 2.1. Take Q235 stamping special-shaped plate as the bearing substrate, degrease and ceramicize the surface in turn, clean the surface, coat the surface with silicone foam, place it in an oven, and foam it at a constant temperature of 65°C to form a buffer foam layer to obtain a prefabricated part.
[0048] 2.2. Mix nano silicon dioxide and mica powder with a fineness of 1000 mesh in a weight ratio of 1:1 as ultrafine filler, and take 1.8 parts of ultrafine filler;
[0049] Take melamine cyanurate as a flame retardant, and take 4 parts of the flame retardant;
[0050] Take antioxidant 1010 and antioxidant 168 in a weight ratio of 3:1 as an antioxidant, and take 0.7 parts of antioxidant;
[0051] Take 100 parts of the modified nylon prepared above;
[0052] The above raw materials are mixed evenly, then coated on the surface of the preform, placed in a vacuum oven, and baked at 60°C for 3 hours. After that, it is sent to a molding machine, the mold temperature is controlled at 95°C, the pressure is 1.5MPa, and the pressure is maintained for 6 minutes to form a corrosion-resistant protective layer to obtain a polymer anti-corrosion composite cable tray.
[0053] Example 3
[0054] This embodiment prepares a polymer anti-corrosion composite cable tray, and the specific implementation process is as follows:
[0055] 1) Preparation of modified nylon
[0056] 1.1. Take trifluoroethanol, triethylamine and acetone as feed materials, apply mechanical stirring to mix evenly, use ice water bath to control the temperature to be constant at 5°C, supplemented by 360rpm mechanical stirring, slowly and uniformly add allyl chloride within 2.5h, continue to stir and react at constant temperature after complete addition, and control the total addition reaction time of allyl chloride to be 6h, wherein the amount ratio of trifluoroethanol, allyl chloride, triethylamine and acetone is 0.1mol:0.13mol:4.2mL:50mL. After the reaction, remove the solvent acetone, excess allyl chloride and other low-boiling substances by rotary evaporation, then add deionized water twice the mass of the rotary evaporation substrate, stir and wash, take the organic phase, dry it with anhydrous sodium sulfate as a water absorbent, filter out the water absorbent, and obtain the fluorinated monomer.
[0057] 1.2. Take allyl glycidyl ether, fluorinated monomer and dioxane as feed materials, apply mechanical stirring to mix evenly, heat to 65°C, and stir mechanically at 180rpm. Add azobisisobutyronitrile intermittently in 3 times with an interval of 30min. After adding completely, continue to keep warm and stir to react. Control the total addition reaction time of azobisisobutyronitrile to be 2h. Among them, the dosage ratio of allyl glycidyl ether, fluorinated monomer, azobisisobutyronitrile and dioxane is 0.1mol:35mmol:0.13g:150mL. After the reaction, remove dioxane by reduced pressure rotary evaporation to obtain a copolymer modifier.
[0058] 1.3. Dissolve aluminum trifluoromethanesulfonate in toluene, and then stir and mix with the copolymer modifier. Heat to 50°C and stir to activate for 12 minutes. Then, add liquid nylon and tetrahydrofuran and mix. Continue to heat to 68°C and reflux for 2.4 hours. The amount ratio of liquid nylon, copolymer modifier, aluminum trifluoromethanesulfonate and tetrahydrofuran is 100g:22g:1.5g:200mL. After the reaction, remove tetrahydrofuran by rotary evaporation to obtain modified nylon.
[0059] 2) Preparation of polymer anti-corrosion composite cable tray
[0060] 2.1. Take Q235 stamping special-shaped plate as the bearing substrate, degrease and ceramicize the surface in turn, clean the surface, coat the surface with silicone foam, place it in an oven, and foam it at a constant temperature of 65°C to form a buffer foam layer to obtain a prefabricated part.
[0061] 2.2. Take 1000 mesh boron nitride powder and mica powder in a weight ratio of 1:2 as ultrafine filler, and take 2.5 parts of ultrafine filler;
[0062] Take melamine cyanurate as a flame retardant, and take 3.6 parts of the flame retardant;
[0063] Take antioxidant 1010 and antioxidant 168 in a weight ratio of 3:1 as an antioxidant, and take 0.6 parts of antioxidant;
[0064] Take 100 parts of the modified nylon prepared above;
[0065] The above raw materials are mixed and coated on the surface of the preform, placed in a vacuum oven, and baked at 65°C for 2.2 hours. Then, it is sent to a molding machine, the mold temperature is controlled at 105°C, the pressure is 1.3MPa, and the pressure is maintained for 6 minutes to form a corrosion-resistant protective layer to obtain a polymer anti-corrosion composite cable tray.
[0066] Comparative Example
[0067] The implementation process of this comparative example is the same as that of Example 3, except that the modified nylon is replaced by the same weight of liquid nylon.
[0068] In order to verify the corrosion resistance of the cable tray prepared as above, samples were cut from the finished products prepared in Examples 1 to 3 and the comparative example, and the samples were subjected to corrosion resistance tests, as shown in Table 1:
[0069] Table 1
[0070]
[0071] It can be seen from the data in Table 1 that the cable tray prepared by the present invention has good resistance to salt spray, oil, acid and alkali corrosion, and shows good acid resistance compared to the existing nylon coating.
[0072] In order to facilitate the detection of the comprehensive performance of the corrosion-resistant protective layer, the raw materials of the corrosion-resistant protective layer in Example 3 and the comparative example were mixed and extruded into a die groove with a specification of 200×100×2 mm, and cured according to the parameters of Example 3. Samples were taken for relevant performance tests, as shown in Table 2:
[0073] Table 2
[0074]
[0075] It can be seen from the data in Table 2 that the corrosion-resistant protective layer of the cable tray prepared by the present invention has a lower water absorption rate than the existing nylon protective layer, has excellent low-temperature toughness, and can meet the use of the cable tray in a wider temperature range.
[0076] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0077] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A polymer anti-corrosion composite cable tray, characterized in that: It comprises a load-bearing substrate, the surface of which is compounded with a buffer foaming layer and a corrosion-resistant protective layer in sequence; The corrosion-resistant protective layer comprises, by weight: 100 parts of modified nylon, 1.8-2.5 parts of ultrafine filler, 3.2-4 parts of flame retardant and 0.6-0.9 parts of antioxidant; The modified nylon is prepared by the following method: Step A1: trifluoroethanol, triethylamine and acetone are mixed, and allyl chloride is slowly added under constant temperature of 5-10°C and stirring. The reaction time is controlled to be 5-7h. After the reaction is completed, the mixture is rotary evaporated, washed with deionized water, and the organic phase is dried to obtain a fluorinated monomer; Step A2: allyl glycidyl ether, fluorinated monomer and dioxane are mixed, the temperature is raised to 62-68° C., azobisisobutyronitrile is added intermittently under stirring, the reaction time is controlled to be 1.5-2.2 hours, and after the reaction is completed, vacuum rotary evaporation is performed to obtain a copolymer modifier; Step A3: Mix the copolymer modifier and the toluene solution of aluminum trifluoromethanesulfonate, heat to 45-50°C, stir and activate for 10-15 minutes, then add liquid nylon and tetrahydrofuran, mix, continue to heat to 65-75°C, reflux reaction for 2-3 hours, and rotary evaporate after the reaction to obtain modified nylon; The ultrafine filler is one or more of silicon dioxide, boron nitride and mica powder, and the fineness is not less than 1000 meshes.
2. The polymer anti-corrosion composite cable tray according to claim 1, characterized in that: The usage ratio of trifluoroethanol, allyl chloride, triethylamine and acetone is 0.1 mol: 0.12-0.14 mol: 3.5-4.5 mL: 40-50 mL.
3. The polymer anti-corrosion composite cable tray according to claim 2 is characterized in that: The usage ratio of allyl glycidyl ether, fluorinated monomer, azobisisobutyronitrile and dioxane is 0.1 mol: 25-40 mmol: 0.1-0.14 g: 120-150 mL.
4. The polymer anti-corrosion composite cable tray according to claim 3 is characterized in that: The dosage ratio of liquid nylon, copolymer modifier, aluminum trifluoromethanesulfonate and tetrahydrofuran is 100g:18-25g:1.3-1.7g:150-200mL.
5. The polymer anti-corrosion composite cable tray according to claim 1, characterized in that: The flame retardant is melamine cyanurate.
6. The polymer anti-corrosion composite cable tray according to claim 1, characterized in that: The antioxidant is a mixture of antioxidant 1010 and antioxidant 168.
7. The method for preparing a polymer anti-corrosion composite cable tray according to claim 1, characterized in that: The steps include: Step S1: cleaning the supporting substrate, coating the surface with organic silicon foam glue, baking and foaming to form a buffer foam layer, and obtaining a prefabricated part; Step S2: Evenly mix the modified nylon, ultrafine filler, flame retardant and antioxidant, apply them on the surface of the preform, vacuum bake at 60-70°C for 2-3h, and then put them into a molding machine, control the mold temperature to 95-110°C, the pressure to 1.2-1.5MPa, and maintain the pressure for 4-6min to form a corrosion-resistant protective layer to obtain a polymer anti-corrosion composite cable tray.
Citation Information
Patent Citations
High-performance reinforced toughened glass fiber nylon and preparation method thereof
CN112920594A
High-resistance composite hose and production process thereof
CN115773409A
Etching-resistant waterproof putty and preparation method thereof
CN115873441A
High-toughness epoxy sealant and preparation method thereof
CN116376491A