A thermoplastic polyester elastomer composite and its preparation method and application

By compounding lubricants with different molecular weights and titanium dioxide in the thermoplastic polyester elastomer to form an ordered structure, the problem of high demoulding force and precipitation of the thermoplastic polyester elastomer material during the demoulding process is solved, and a solution suitable for Low demoulding force and no precipitation for parts with large aspect ratio.

CN116769283BActive Publication Date: 2024-10-22KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210240957.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-10-22
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

The thermoplastic polyester elastomer material has a large demoulding force during the demoulding process and the release agent is easy to precipitate, resulting in a greasy surface of the part, which limits its application in parts that come into contact with the human body and parts with a large aspect ratio.

Method used

The Montan wax lubricant with a smaller molecular weight is compounded with the silicone lubricant with a larger molecular weight, and combined with titanium dioxide, and processed through a twin-screw extruder to induce the thermoplastic polyester elastomer to form an ordered structure, reducing the Release force and avoid precipitation.

Benefits of technology

The low demoulding force and no precipitation characteristics of the thermoplastic polyester elastomer compound are achieved, which is suitable for the production of parts with large aspect ratio and meets the requirements of high demoulding performance and non-greasy surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003541633890000011
    Figure BDA0003541633890000011
  • Figure BDA0003541633890000021
    Figure BDA0003541633890000021
  • Figure BDA0003541633890000022
    Figure BDA0003541633890000022
Patent Text Reader

Abstract

The present invention discloses a thermoplastic polyester elastomer composite, a preparation method and an application thereof. The thermoplastic polyester elastomer composite comprises the following components calculated by weight: 90-99 parts of thermoplastic polyester elastomer; 1-5 parts of silicone lubricant; 0.3-1 parts of montan wax lubricant; 0.05-0.5 parts of titanium dioxide; and 0-30 parts of functional additives. The present invention obtains a thermoplastic polyester elastomer with small demoulding force and no precipitation by adding a specific amount of lubricant and titanium dioxide to the thermoplastic polyester elastomer, thereby overcoming the problems of large demoulding force and precipitation of demoulding agent of the existing thermoplastic polyester elastomer. The thermoplastic polyester elastomer composite can be used in the production of parts with large aspect ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyester elastomers, and more specifically, to a thermoplastic polyester elastomer composite and a preparation method and application thereof. Background Art

[0002] Thermoplastic polyester elastomer materials have excellent mechanical properties, chemical solvent resistance, fatigue resistance, and small variation in mechanical properties with temperature. They have been increasingly used in rail transit buffer gaskets, ski equipment, office seats, automotive pipelines and other fields.

[0003] Since thermoplastic polyester elastomer materials are highly polar materials with a certain degree of elasticity, they fit tightly to the inner surface of the mold after injection molding and have a relatively large interaction force with the inner surface of the mold, which can lead to various problems such as difficulty in demolding, damage to the parts during demolding, and complex mold structure, limiting their application.

[0004] The demoulding performance can be improved to a certain extent by adding release agents and other methods. For example, adding dimethyl silicone oil and ethylene bis stearamide to thermoplastic polyester elastomer can achieve the purpose of improving the wear resistance of TPEE, but in this scheme, the additives are easy to precipitate, resulting in greasy surface of the parts, which cannot be used for parts in contact with the human body; another example is the preparation of highly wear-resistant thermoplastic polyester elastomer by blending thermoplastic polyester elastomer with polytetrafluoroethylene, silica, silicone oil, etc., but due to the poor compatibility of silicone oil with thermoplastic polyester elastomer, silicone oil will precipitate on the surface of the parts, resulting in greasy surface of the parts, limiting its application in daily necessities. Summary of the invention

[0005] The primary purpose of the present invention is to overcome the problems of large demoulding force and release agent precipitation of the existing thermoplastic polyester elastomer, and to provide a thermoplastic polyester elastomer composite. The thermoplastic polyester elastomer composite provided by the present invention has small demoulding force and no precipitation, and can be used in the production of parts with large aspect ratio.

[0006] Another object of the present invention is to provide a method for preparing the thermoplastic polyester elastomer compound.

[0007] Another object of the present invention is to provide application of the thermoplastic polyester elastomer compound.

[0008] The above-mentioned object of the present invention is achieved by the following technical solutions:

[0009] A thermoplastic polyester elastomer compound comprises the following components calculated by weight:

[0010]

[0011]

[0012] When using thermoplastic polyester elastomer to prepare parts with large aspect ratio, the demoulding performance is required to be very high. When using montan wax lubricants or other commonly used lubricants alone, a high proportion of addition is required, which is easy to cause lubricant precipitation. After many experiments, the inventors found that compounding thermoplastic polyester elastomer with a specific amount of montan wax lubricants with a small molecular weight and a fast migration speed and a specific amount of silicone lubricants with a large molecular weight and a slow migration speed can improve the defects of using a single lubricant with a large addition amount, which leads to precipitation. After further compounding with titanium dioxide, during the cooling process of the thermoplastic polyester elastomer melt in the mold cavity, titanium dioxide can induce the thermoplastic polyester elastomer molecules to form an ordered structure, and the size of the part shrinks, thereby further reducing the demoulding force.

[0013] Preferably, the thermoplastic polyester elastomer compound comprises the following components calculated in parts by weight:

[0014]

[0015] Preferably, the titanium dioxide is rutile titanium dioxide. The crystal size of rutile titanium dioxide matches the thermoplastic polyester elastomer, and can induce a more perfect crystal structure of the thermoplastic polyester elastomer.

[0016] Specifically, the titanium dioxide can be selected from one or more of R103, RCL-69, R350, and NCT-69P75.

[0017] More preferably, the rutile titanium dioxide is prepared by a chlorination process.

[0018] Conventional silicone lubricants in the art can be used in the present invention. Generally, the silicone lubricant is selected from silicone and / or silicone masterbatch.

[0019] Specifically, the silicone lubricant of the present invention can be selected from one or more of MB50-002, RM4-7081, HG-600, TEGOMER, and PD1090.

[0020] Conventional montan wax lubricants in the art can be used in the present invention. Generally, the montan wax lubricant is selected from one or more of LICOWAX E, LICOWAX OP, and LICOWAX WE4.

[0021] Preferably, the montan wax lubricant is LICOWAX E.

[0022] Preferably, the Shore hardness of the thermoplastic polyester elastomer is 60D-70D. Thermoplastic polyester elastomers within this hardness range have relatively balanced modulus and elastic properties and are suitable for making parts with a large aspect ratio.

[0023] It should be noted that the Shore hardness of the thermoplastic polyester elastomer is tested according to standard ISO 7619-1-2010.

[0024] The thermoplastic polyester elastomer composite provided by the present invention may also include other conventional functional additives in the art to obtain more excellent or new performance, and the types of various functional additives may be selected and adjusted according to actual needs.

[0025] Preferably, the other functional additives are one or more of antioxidants, anti-UV agents, flame retardants, and toners.

[0026] The antioxidant is selected from one or more of hindered phenol antioxidants, phosphite antioxidants, aniline antioxidants, and thioester antioxidants.

[0027] The anti-UV agent is selected from one or more of benzophenone anti-UV agents, benzotriazole anti-UV agents, and hindered amine anti-UV agents.

[0028] The flame retardant is selected from one or more of organic aluminum hypophosphite, inorganic aluminum hypophosphite, melamine cyanurate, brominated polystyrene, brominated epoxy resin, and red phosphorus.

[0029] The toner is selected from one or more of carbon black, zinc sulfide, titanium yellow and iron red.

[0030] The present invention also protects a method for preparing the thermoplastic polyester elastomer composite, comprising the following steps:

[0031] Thermoplastic polyester elastomer, silicone lubricant, montan wax lubricant, titanium dioxide and functional additives are uniformly mixed, extruded through a twin-screw extruder, and granulated to obtain a thermoplastic polyester elastomer compound.

[0032] Preferably, the extrusion temperature is 160-230°C.

[0033] Preferably, the length-to-diameter ratio of the twin-screw extruder used is 36-60 / 1, and the residence time of the mixed material in the screw is 40-90 seconds.

[0034] The invention also protects the use of the thermoplastic polyester elastomer compound in preparing a product with a large aspect ratio.

[0035] Generally, a part with an aspect ratio greater than 5 is called a large aspect ratio part. The large aspect ratio parts include but are not limited to toothbrush bristles, large-size display frame cushions, combs, etc.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The invention prepares a thermoplastic polyester elastomer composite by compounding a thermoplastic polyester elastomer with a montan wax lubricant having a small molecular weight and a fast migration speed, a silicone lubricant having a large molecular weight and a slow migration speed, and titanium dioxide. The obtained thermoplastic polyester elastomer composite can be processed and formed by injection molding and other processes, has a small demoulding force and no precipitation, and can be widely used in the production of parts with a large aspect ratio. DETAILED DESCRIPTION

[0038] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0039] The present invention will be further described below in conjunction with specific implementation modes.

[0040] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the present technical field.

[0041] The raw materials in the embodiments and comparative examples can be obtained from commercial sources, as follows:

[0042]

[0043] The thermoplastic polyester elastomer composites described in the embodiments and comparative examples are prepared by the following method:

[0044] The dried thermoplastic polyester elastomer, silicone lubricant, montan wax lubricant, titanium dioxide and functional additives are put into a high-speed mixer for mixing, and fed into a twin-screw extruder through loss-in-weight metering. After extrusion at 160-230° C., the thermoplastic polyester elastomer composite is obtained after granulation and drying.

[0045] The length-to-diameter ratio of the twin-screw extruder used is 36-60 / 1, and the residence time of the material in the screw is 40-90 seconds.

[0046] Examples 1 to 9

[0047] Examples 1 to 9 provide a thermoplastic polyester elastomer compound, and the amount of each raw material used is shown in Table 1.

[0048] Table 1 Amount of each raw material used in Examples 1 to 9 (parts by weight)

[0049]

[0050]

[0051] Embodiments 10 to 20

[0052] Examples 10 to 20 provide a thermoplastic polyester elastomer composite, and the amount of each raw material used is shown in Table 2.

[0053] Table 2 Amount of each raw material used in Examples 10 to 20 (parts by weight)

[0054]

[0055]

[0056] Comparative Examples 1 to 5

[0057] Comparative Examples 1 to 5 provide a thermoplastic polyester elastomer composite, and the amount of each raw material used is shown in Table 3.

[0058] Table 3 Comparative Examples 1 to 5 Amount of each raw material used (parts by weight)

[0059] 1 2 3 4 5 6 Thermoplastic Elastomer A 90 90 90 90 90 90 Silicone Lubricant A / 1 1 8 1 1 Montan wax lubricant A 0.3 / 0.3 0.3 2 0.3 Titanium Dioxide A 0.05 0.05 / 0.05 0.05 1

[0060] Performance Testing

[0061] The thermoplastic polyester elastomer composites prepared in the above examples and comparative examples were subjected to performance tests.

[0062] Demolding force test method: The thermoplastic polyester elastomer compound is injection molded into a cylindrical part, where the outer diameter of the cylinder is 50 mm, the wall thickness is 2 mm, and the height of the cylinder is 60 mm. Two pressure sensors are installed behind the demolding ejection device to measure the demolding force during the demolding process. The sum of the pressures measured by the two pressure sensors is used to evaluate the demolding force (unit: N).

[0063] Precipitation test method: Inject the thermoplastic polyester elastomer compound into a 100*100*1.5mm square plate, place it in an oven, bake it at 80℃ for 1 week, take it out and observe it with the naked eye. If oily or powdery substances appear on the surface, it is judged that precipitation exists. If the surface is dry and there is no oily or powdery substances, it is judged that there is no precipitation.

[0064] The test results of Examples 1 to 20 are shown in Table 4.

[0065] Table 4 Test results of the thermoplastic polyester elastomer composites described in Examples 1 to 20.

[0066]

[0067] Table 4

[0068]

[0069]

[0070] The test results of Comparative Examples 1 to 6 are shown in Table 5 below.

[0071] Table 5 shows the test results of the thermoplastic polyester elastomer composites described in Comparative Examples 1 to 6.

[0072] 1 2 3 4 5 6 Surface precipitation No precipitation No precipitation No precipitation There is precipitation There is precipitation No precipitation Demolding force (N) 6670 6420 6460 3620 4590 5910

[0073] It can be seen from Table 4 that the demolding forces of the thermoplastic polyester elastomer composites described in Examples 1 to 20 of the present invention do not exceed 5500N, which can meet the injection molding requirements of parts with a large aspect ratio. They are injection molded into 100*100*1.5mm square plates, placed in an oven, and baked at 80°C for 1 week without precipitation.

[0074] From Example 1 and Examples 4 to 6, it can be seen that the titanium dioxide using rutile titanium dioxide has a lower demolding force. The reason is that the crystal size of rutile titanium dioxide matches the thermoplastic polyester elastomer and can induce a more perfect crystal structure of the thermoplastic polyester elastomer. The demolding force of rutile titanium dioxide prepared by the chlorination process can be further reduced.

[0075] From Example 1 and Examples 7 to 9, it can be seen that the amount of silicone lubricant used has a great influence on the demoulding force. When the amount of silicone lubricant added is 2 to 4 parts, the demoulding force is relatively low.

[0076] From Example 1 and Examples 10 to 12, it can be seen that the amount of montan wax lubricant used also has a great influence on the demoulding force. When the added amount of montan wax lubricant is 0.5 to 0.8 parts, the demoulding force is lower. From Example 1 and Examples 19 to 20, it can be seen that when the montan wax lubricant is LICOWAX E, the demoulding force is lower.

[0077] From Example 1 and Examples 13 to 15, it can be seen that the amount of titanium dioxide used has a great influence on the demoulding force. When the amount of titanium dioxide added is 0.1 to 0.3, the demoulding force is lower.

[0078] It can be seen from Table 5 that when the amount of silicone lubricant or montan wax lubricant is too much, although the demoulding force can meet the requirements, precipitation occurs after baking at 80°C for one week. When only a small amount of silicone lubricant or montan wax lubricant is added, although there is no precipitation, the demoulding force is greater than 5500N, which cannot meet the injection molding requirements of parts with a large aspect ratio.

[0079] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A thermoplastic polyester elastomer composite, characterized in that: The composition includes the following components calculated by weight:

2. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The composition includes the following components calculated by weight:

3. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The titanium dioxide is rutile titanium dioxide.

4. The thermoplastic polyester elastomer composite according to claim 3, characterized in that: The rutile titanium dioxide is prepared by a chlorination process.

5. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The silicone lubricant is selected from silicone and / or silicone masterbatch.

6. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The montan wax lubricant is selected from one or more of LICOWAX E, LICOWAX OP and LICOWAX WE4.

7. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The Shore hardness of the thermoplastic polyester elastomer is 60D-70D.

8. The thermoplastic polyester elastomer composite according to claim 1, characterized in that: The functional additive is selected from one or more of antioxidants, anti-UV agents, flame retardants, and color powders.

9. The method for preparing the thermoplastic polyester elastomer compound according to any one of claims 1 to 8, characterized in that: The steps include: Thermoplastic polyester elastomer, silicone lubricant, montan wax lubricant, titanium dioxide and functional additives are uniformly mixed, extruded and granulated to obtain a thermoplastic polyester elastomer compound.

10. Use of the thermoplastic polyester elastomer compound according to any one of claims 1 to 8 in the preparation of a product with a large aspect ratio.