A thermoplastic polyester composite and its preparation method and application
Through the combination of thermoplastic polyester elastomer 1 and thermoplastic polyester elastomer 2 and the combination of styrene-glycidyl methacrylate copolymer and alumina, the thermoplastic polyester elastomer and nonwoven fabrics are solved at high temperatures The problem of poor adhesive strength has significantly improved the high-temperature adhesiveness between composites and non-woven fabrics, and is suitable for the production of medical protective clothing.
Patent Information
- Application Number
- CN202210222651.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-09
AI Technical Summary
The bonding strength of thermoplastic polyester elastomer materials and nonwovens in high temperature environments is poor, resulting in the easy debonding of medical protective clothing during disinfection and sterilization, resulting in waste products.
The thermoplastic polyester elastomer 1 and thermoplastic polyester elastomer 2 is used to combine the combination of styrene-glycidyl methacrylate copolymer and alumina, and prepare the thermoplastic polyester composite through the twin screw extrusion mechanism. , improve the high-temperature bonding between the composite and non-woven fabric.
The adhesive force between thermoplastic polyester composite and non-woven fabrics is significantly improved at high temperatures, ensuring the stability and service life of the composite film.
Smart Images

Figure BDA0003538081380000011 
Figure BDA0003538081380000021 
Figure BDA0003538081380000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of elastomers, and particularly relates to a thermoplastic polyester composite and a preparation method and application thereof. Background Art
[0002] Thermoplastic polyester elastomer materials have excellent mechanical properties, chemical solvent resistance, high moisture permeability and other characteristics, and have been increasingly used in clothing, jackets, outdoor tents and other fields. Especially in the field of medical protective clothing, the isolation layer made of thermoplastic polyester elastomer has the advantages of high moisture permeability, no microporous structure, and high virus barrier ability, and can be used in the field of infectious patient surgery.
[0003] Medical protective clothing is generally a multi-layer structure, with a non-woven outer layer and an isolation layer in the middle. The isolation layer and the non-woven fabric layer are bonded by glue or double-sided tape. The production process includes extrusion casting to produce non-woven fabrics, extrusion casting to produce thermoplastic polyester elastomer isolation membranes, applying glue or double-sided tape on the surface of non-woven fabrics, and laminating the non-woven fabric layer and the isolation layer. The production process has many steps, a long process, and cannot be produced continuously.
[0004] Non-woven fabrics are generally made of polypropylene, which is a non-polar material, while thermoplastic polyester elastomers are polar materials, and the two are not compatible. The cast film produced directly by multi-layer co-extrusion has no adhesion between the non-woven fabric layer and the isolation layer, resulting in the detachment of the two layers and the inability to form a composite film. In order to solve this problem, a common method is to apply glue or double-sided tape between the thermoplastic polyester elastomer and the non-woven fabric, and bond them by hot pressing. During the disinfection and sterilization process of protective clothing, in a high temperature environment, the thermoplastic polyester elastomer and the non-woven fabric are prone to debonding, resulting in waste. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a thermoplastic polyester composite and a preparation method and application thereof, so as to overcome the defect of poor adhesion between thermoplastic polyester elastomer material and non-woven fabric at high temperature in the prior art.
[0006] The present invention provides a thermoplastic polyester composite, wherein the composite components include, by weight:
[0007]
[0008] The thermoplastic polyester elastomer compound comprises a thermoplastic polyester elastomer 1 and a thermoplastic polyester elastomer 2 in a weight ratio of 5:1 to 1:5;
[0009] The thermoplastic polyester elastomer 1 is a copolymer of polyethylene glycol, terephthalic acid and 1,4-butanediol;
[0010] The thermoplastic polyester elastomer 2 is a copolymer of polyethylene glycol, terephthalic acid, isophthalic acid, neopentyl glycol and cyclohexanedimethanol.
[0011] Preferably, the composite components include, by weight:
[0012]
[0013] Preferably, the propylene-based elastomer is a semi-crystalline copolymer of propylene and ethylene.
[0014] Preferably, the styrene-glycidyl methacrylate copolymer or its compound is: styrene-glycidyl methacrylate copolymer 1 or / and styrene-glycidyl methacrylate copolymer 2.
[0015] Preferably, the mass fraction of glycidyl methacrylate in the styrene-glycidyl methacrylate copolymer 1 is 15-20%. The test standard for the mass fraction of glycidyl methacrylate is the hydrochloric acid-acetone method in GB / T 1677-2008.
[0016] Preferably, the mass fraction of glycidyl methacrylate in the styrene-glycidyl methacrylate copolymer 2 is 2-8%. The test standard for the mass fraction of glycidyl methacrylate is the hydrochloric acid-acetone method in GB / T 1677-2008.
[0017] Preferably, the styrene-glycidyl methacrylate copolymer compound comprises styrene-glycidyl methacrylate copolymer 1 and styrene-glycidyl methacrylate copolymer 2 in a weight ratio of 2-3:97-98.
[0018] Preferably, the number average molecular weight of the polyethylene glycol in the thermoplastic polyester elastomer 1 is 2000-8000.
[0019] Preferably, the number average molecular weight of the polyethylene glycol in the thermoplastic polyester elastomer 2 is 200-1800.
[0020] Preferably, the thermoplastic polyester elastomer 1 comprises, by weight percentage, 25-50% terephthalic acid residues, 48-70% polyethylene glycol residues, and 2-27% 1,4-butanediol residues. The weight percentage is obtained by nuclear magnetic resonance H spectrum.
[0021] Preferably, the preparation method of the thermoplastic polyester elastomer 1 comprises: subjecting 25-50% terephthalic acid, 48-70% polyethylene glycol and 2-27% 1,4-butanediol to an esterification reaction at 190-230° C. for 1-3 hours under normal pressure to negative pressure, heating to 235-260° C., and subjecting the reaction system to a polycondensation reaction at a pressure of less than 200 Pa for 2-5 hours, introducing high-purity nitrogen into the reaction system, extruding the melt through a mouth mold, and pelletizing to obtain the product, wherein the raw material percentage is the percentage of the raw material mass to the total raw material mass.
[0022] Preferably, the thermoplastic polyester elastomer 2 comprises, by weight percentage, 30-40% terephthalic acid residues, 2-10% isophthalic acid residues, 20-40% polyethylene glycol residues, 5-15% cyclohexanedimethanol residues, and 10-30% neopentyl glycol residues. The weight percentage is obtained by nuclear magnetic resonance H spectrum.
[0023] Preferably, the preparation method of the thermoplastic polyester elastomer 2 comprises: subjecting 30-40% of terephthalic acid, 2-10% of isophthalic acid, 20-40% of polyethylene glycol, 5-15% of cyclohexanedimethanol and 10-30% of neopentyl glycol to an esterification reaction at 180-210° C. for 1-3 hours under normal pressure to negative pressure, heating to 240-270° C., subjecting the reaction kettle system to a polycondensation reaction at a pressure less than 100 Pa, charging high-purity nitrogen into the reaction vessel system, extruding the melt through a mouth mold, and pelletizing to obtain the product, wherein the raw material percentage is the percentage of the raw material mass to the total raw material mass.
[0024] Preferably, the thermoplastic polyester compound further comprises 0-30 parts of additives.
[0025] Preferably, the additives include one or more of flame retardants, antioxidants, UV resistant agents, carbon black, pigments, dyes, and mineral powders.
[0026] Preferably, the flame retardant includes one or more of melamine cyanurate, inorganic aluminum hypophosphite, organic aluminum hypophosphite, brominated epoxy resin, and brominated polystyrene.
[0027] Preferably, the antioxidant includes one or more of hindered phenol antioxidants, phosphite antioxidants, aniline antioxidants, and thioester antioxidants.
[0028] Preferably, the UV-resistant agent includes one or more of benzophenone-based UV-resistant agents, benzotriazole-based UV-resistant agents, and hindered amine-based UV-resistant agents.
[0029] Preferably, the pigment includes one or more of titanium dioxide, zinc sulfide, and ultramarine blue.
[0030] Preferably, the dye includes one or more of azo yellow, isoindolinone yellow and phthalocyanine green.
[0031] Preferably, the mineral powder includes one or more of calcium carbonate, talc and montmorillonite.
[0032] The present invention also provides a method for preparing a thermoplastic polyester composite, comprising the following steps:
[0033] The components are mixed, and the obtained material is fed into a twin-screw extruder for extrusion, and then granulated and dried to obtain a thermoplastic polyester compound.
[0034] Preferably, the extrusion temperature is 160-230°C.
[0035] Preferably, the length-to-diameter ratio of the twin-screw extruder is 36 to 60:1.
[0036] Preferably, the material stays in the screw for 40 to 90 seconds.
[0037] The invention also provides application of the thermoplastic polyester composite in medical protective clothing.
[0038] In the present invention, thermoplastic polyester elastomer 1 is a crystalline polymer, which can give the composite good mechanical strength. Under high temperature conditions, the dimensional change caused by crystallization will produce large internal stress at the interface between the composite and the non-woven fabric, resulting in low adhesion. Thermoplastic polyester elastomer 2 is an amorphous polymer, which is easily deformed when heated at high temperatures, resulting in low adhesion. Thermoplastic polyester elastomer 1 and thermoplastic polyester elastomer 2 are used in combination. Under high temperature conditions, the crystalline thermoplastic polyester elastomer 1 can provide a higher adhesion, and the amorphous thermoplastic polyester elastomer 2 can reduce the internal stress at the interface between the composite and the non-woven fabric through its own deformation, thereby obtaining good adhesion at high temperatures.
[0039] The aluminum oxide in the present invention has a high thermal conductivity. During the bonding process of the thermoplastic polyester composite and the non-woven fabric, the heat released by the aluminum oxide helps the interface of the thermoplastic polyester composite and the non-woven fabric to maintain a high temperature state for a longer time, thereby improving the bonding effect. Aluminum oxide is an inorganic substance, and the resin composite is an organic material. The two have poor compatibility, and uneven dispersion is easily produced during the mixing process, resulting in the heat in the aluminum oxide not being evenly released to the interface between the composite and the non-woven fabric, affecting the bonding effect. The glycidyl methacrylate in the styrene-glycidyl methacrylate copolymer can produce a strong interaction with the surface of aluminum oxide, helping aluminum oxide to be better dispersed in the composite, so that the heat in the aluminum oxide can be more evenly released to the interface between the composite and the non-woven fabric, thereby improving the bonding strength at high temperature. When styrene-glycidyl methacrylate copolymer 1 and styrene-glycidyl methacrylate copolymer 2 are used in combination, the dispersion effect of aluminum oxide in the composite can be optimized.
[0040] Beneficial Effects
[0041] The present invention uses a compound of thermoplastic polyester elastomer 1 and thermoplastic polyester elastomer 2 to improve the bonding strength between the composite and the non-woven fabric at high temperatures. The compound of styrene-glycidyl methacrylate copolymer or its compound and aluminum oxide can further improve the bonding strength between the composite and the non-woven fabric at high temperatures. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0043] Source of reagents:
[0044] Thermoplastic polyester elastomer 1:
[0045] Thermoplastic polyester elastomer 1-1: a copolymer of polyethylene glycol, terephthalic acid and 1,4-butanediol, the preparation method of which is as follows: 25% terephthalic acid (BP), 48% polyethylene glycol (PEG-6000, the number average molecular weight of polyethylene glycol is 6000, Sinopharm Group) and 27% 1,4-butanediol (BASF) are put into a reactor, stirred evenly at 190°C and normal pressure, the pressure is gradually reduced to 70kPa, and the reaction is continued for 3 hours to carry out esterification reaction, the temperature is raised to 235°C within 1 hour, the pressure is gradually reduced to 30Pa, and the polycondensation reaction is carried out for 4 hours. After the polycondensation reaction is completed, high-purity nitrogen is filled into the reactor, the melt is extruded from the reactor through the mouth mold, and pelletized to obtain the product, wherein the raw material percentage is the percentage of the raw material mass to the total raw material mass;
[0046] Thermoplastic polyester elastomer 1-2: a copolymer of polyethylene glycol, terephthalic acid and 1,4-butanediol, the preparation method of which is based on the thermoplastic polyester elastomer 1-1, and the difference from the thermoplastic polyester elastomer 1-1 is that the number average molecular weight of polyethylene glycol is 1000, PEG-1000, purchased from Sinopharm Group, and the rest is the same as the preparation method of the thermoplastic polyester elastomer 1-1;
[0047] Thermoplastic polyester elastomer 2:
[0048] Thermoplastic polyester elastomer 2-1: a copolymer of polyethylene glycol, terephthalic acid, isophthalic acid, neopentyl glycol and cyclohexanedimethanol, the preparation method of which is as follows: 30% of terephthalic acid (BP), 2% of isophthalic acid (Sinopharm Group), 30% of polyethylene glycol (PEG-1000, number average molecular weight of 1000, Sinopharm Group), 15% of cyclohexanedimethanol (SK) and 23% of neopentyl glycol (Sinopharm Group) are put into a reactor, stirred evenly at 180°C, the pressure is gradually reduced to 80 kPa, the reaction is continued for 2.5 hours, the temperature is increased to 240°C within 1 hour, the pressure is reduced to 30 Pa, the polycondensation reaction is continued for 4 hours, high-purity nitrogen is charged into the reactor system, the melt is extruded through a mouth mold, and pelletized to obtain the product, wherein the raw material percentage is the percentage of the raw material mass to the total raw material mass;
[0049] Thermoplastic polyester elastomer 2-2: a copolymer of polyethylene glycol, terephthalic acid, isophthalic acid, neopentyl glycol and cyclohexanedimethanol, the preparation method of which is based on the thermoplastic polyester elastomer 2-1, and the difference from the thermoplastic polyester elastomer 2-1 is that the number average molecular weight of polyethylene glycol is 11000, PEG-11000, purchased from Sinopharm Group, and the rest is the same as the preparation method of thermoplastic polyester elastomer 2-1;
[0050] Propylene-based elastomer: semi-crystalline copolymer of propylene and ethylene, Vistamaxx 3020FL, ExxonMobil;
[0051] Styrene-Glycidyl Methacrylate Copolymer:
[0052] Styrene-glycidyl methacrylate copolymer was prepared as follows:
[0053] Under the protection of high-purity nitrogen, add the measured toluene solution of styrene (commercially available) and glycidyl methacrylate monomer (commercially available) into the reactor, stir and cool to 0°C, slowly drop a small amount of n-butyl lithium, continue stirring and react for 5 hours, add methanol to terminate the reaction, evaporate the solvent to dryness, and wash with ethanol to obtain styrene-glycidyl methacrylate copolymer. Adjust the ratio of added styrene and glycidyl methacrylate to obtain copolymers with different glycidyl methacrylate contents. (The following styrene-glycidyl methacrylate copolymers are all synthesized according to the above method)
[0054] Styrene-Glycidyl Methacrylate Copolymer 1:
[0055] Styrene-glycidyl methacrylate copolymer 1-1: the mass fraction of glycidyl methacrylate is 20%. During the preparation of the copolymer, the amount of styrene added is 795 g, and the amount of glycidyl methacrylate monomer added is 200 g;
[0056] Styrene-methacrylate glycidyl copolymer 1-2: The mass fraction of glycidyl methacrylate is 14%. During the preparation of the copolymer, the amount of styrene added is 855 g, and the amount of glycidyl methacrylate monomer added is 140 g; Styrene-methacrylate glycidyl copolymer 2:
[0057] Styrene-glycidyl methacrylate copolymer 2-1: the mass fraction of glycidyl methacrylate is 5%. During the preparation of the copolymer, the amount of styrene added is 930 g, and the amount of glycidyl methacrylate monomer added is 50 g;
[0058] Styrene-glycidyl methacrylate copolymer 2-2: the mass fraction of glycidyl methacrylate is 1%. During the preparation of the copolymer, the amount of styrene added is 990 g, and the amount of glycidyl methacrylate monomer added is 10 g;
[0059] Ethylene-acrylate-glycidyl methacrylate copolymer: glycidyl methacrylate mass fraction is 8%, brand AX 8900, from Arkema;
[0060] Alumina: Brand DC3-ML2, produced by Xinjiang Sanruibaide;
[0061] Additives: Antioxidant: Hindered phenol antioxidant, commercially available;
[0062] The additives (antioxidants) used in the examples and comparative examples are the same commercially available products.
[0063] The preparation method of the thermoplastic polyester composite is as follows:
[0064] According to the proportions in Table 1, Table 2 and Table 3, each component is put into a high-speed mixer and mixed evenly, and the obtained material is fed into a twin-screw extruder through a loss-in-weight metering scale for extrusion, and granulated and dried to obtain a thermoplastic polyester composite. The extrusion temperature is 160-230°C; the aspect ratio of the twin-screw extruder is 36-60:1; and the residence time of the material in the screw is 40-90s.
[0065] Performance Test:
[0066] Adhesion test: The thermoplastic polyester elastomer compound and non-woven fabric special material (PP T30S, Sinopec) were co-extruded in two layers to prepare a composite film, wherein the extrusion temperature of PP T30S was 210°C and the film thickness was 0.6mm, and the extrusion temperature of the thermoplastic polyester elastomer compound was 220°C and the film thickness was 0.5mm. The composite film was cut into a width of 50mm and tested for 180-degree peel strength at 115°C using a universal testing machine Zwick / Roell Z020 with a displacement speed of 200mm / min.
[0067] Table 1 Example ratio (parts by weight)
[0068]
[0069]
[0070] Table 2 Examples (parts by weight)
[0071]
[0072]
[0073] Table 3 Comparative Example Proportions (parts by weight)
[0074]
[0075] As shown in Tables 1-3, in Comparative Example 1, only thermoplastic polyester elastomer 1 is added without thermoplastic polyester elastomer 2, and in Comparative Example 2, only thermoplastic polyester elastomer 2 is added without thermoplastic polyester elastomer 1, and the bonding strength of Comparative Examples 1 and 2 is significantly less than that of Example 1. The weight ratio of thermoplastic polyester elastomer 1 to thermoplastic polyester elastomer 2 in Comparative Examples 3 and 4 is not within the scope of the present invention, and the bonding strength of Comparative Examples 3 and 4 is less than that of Example 1. It can be seen that the present invention adopts thermoplastic polyester elastomer 1 and thermoplastic polyester elastomer 2 to compound and add them in proportion, which can significantly improve the bonding strength between the composite and the non-woven fabric at high temperature.
[0076] Comparative Example 5 does not add styrene-glycidyl methacrylate copolymer, Comparative Example 6 does not add aluminum oxide, and Comparative Example 7 adds ethylene-glycidyl methacrylate. The bonding strength of Comparative Examples 5-7 is less than that of Example 1. It can be seen that the bonding strength between the composite and the non-woven fabric at high temperature can be further improved by using a compound of styrene-glycidyl methacrylate copolymer or its compound and aluminum oxide.
Claims
1. A thermoplastic polyester composite, characterized in that: The composite components include, by weight: 60-90 parts of thermoplastic polyester elastomer compound; 10-40 parts of propylene-based elastomer; 2-10 parts of styrene-glycidyl methacrylate copolymer or its compound; Alumina 5-30 parts; The thermoplastic polyester elastomer compound comprises a thermoplastic polyester elastomer 1 and a thermoplastic polyester elastomer 2 in a weight ratio of 5:1 to 1:5; The thermoplastic polyester elastomer 1 is a copolymer of polyethylene glycol, terephthalic acid and 1,4-butanediol; The thermoplastic polyester elastomer 2 is a copolymer of polyethylene glycol, terephthalic acid, isophthalic acid, neopentyl glycol and cyclohexanedimethanol; The propylene-based elastomer is a semi-crystalline copolymer of propylene and ethylene.
2. The thermoplastic polyester composite according to claim 1, characterized in that The composite components include, by weight: 66-84 parts of thermoplastic polyester elastomer compound; 15-35 parts of propylene-based elastomer; 4-8 parts of styrene-glycidyl methacrylate copolymer or its compound; Alumina 8-25 parts.
3. The thermoplastic polyester composite according to claim 1, characterized in that The styrene-glycidyl methacrylate copolymer or its composite is: styrene-glycidyl methacrylate copolymer 1 or / and styrene-glycidyl methacrylate copolymer 2; the mass fraction of glycidyl methacrylate in the styrene-glycidyl methacrylate copolymer 1 is 15-20%; the mass fraction of glycidyl methacrylate in the styrene-glycidyl methacrylate copolymer 2 is 2-8%.
4. The thermoplastic polyester composite according to claim 3, characterized in that The styrene-glycidyl methacrylate copolymer compound comprises styrene-glycidyl methacrylate copolymer 1 and styrene-glycidyl methacrylate copolymer 2 in a weight ratio of 2-3:97-98.
5. The thermoplastic polyester composite according to claim 1, characterized in that The number average molecular weight of the polyethylene glycol in the thermoplastic polyester elastomer 1 is 2000-8000; the number average molecular weight of the polyethylene glycol in the thermoplastic polyester elastomer 2 is 200-1800.
6. The thermoplastic polyester composite according to claim 1, characterized in that The thermoplastic polyester compound further comprises 0-30 parts of additives; the additives comprise one or more of flame retardants, antioxidants, UV resistant agents, carbon black, pigments, dyes and mineral powders.
7. A method for preparing the thermoplastic polyester composite according to any one of claims 1 to 6, comprising the following steps: The components are mixed, and the obtained material is fed into a twin-screw extruder for extrusion, and then granulated and dried to obtain a thermoplastic polyester compound.
8. The preparation method according to claim 7, characterized in that: The extrusion temperature is 160-230° C.; the length-to-diameter ratio of the twin-screw extruder is 36-60:1; and the residence time of the material in the screw is 40-90 seconds.
9. Use of the thermoplastic polyester composite according to any one of claims 1 to 6 in medical protective clothing.