A method for removing iron ions and recovering acid from high-concentration iron-containing waste liquid
By stirring the high-concentration iron ion solution with sodium salt under strong acid conditions and passing it into oxygen to generate iron sulfate, the problem of difficulty in removing high-concentration iron ion solution in the prior art is solved, and efficient iron ion removal and acid The recycling of the company reduces production costs and waste residue treatment problems.
Patent Information
- Application Number
- CN202310756827.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-25
AI Technical Summary
In the prior art, when treating high-concentration iron ion solutions, it is difficult to achieve efficient removal of iron ions under weak acid conditions, and a large number of alkaline substances are often required to adjust the pH, resulting in high production costs and difficulty in treating waste residues.
Under strong acidic conditions, by stirring the iron-containing solution with sodium salt and then passing oxygen into a pressure reactor, the reaction is to generate iron sulfate, and the removal of iron ions and the recovery of acid is achieved. Sodium sulfate is used as the sodium salt to generate The sulfuric acid can be reused.
It achieves a 90% iron ion removal rate under strong acid conditions, saves drug consumption, is low in production cost, is easy to remove iron slag, and can recycle residual acid, achieving green and environmental protection of resources.
Smart Images

Figure CN116770069B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for removing iron ions from a high-concentration iron-containing solution and recovering acid. Background Art
[0002] In the hydrometallurgical industry, sulfuric acid is often used as a leaching agent to leach the pre-recovered elements in the material, and then the leachate is purified and separated to obtain the final product. However, sulfuric acid, as a strong inorganic acid, can react with most metal elements and has poor leaching selectivity. Therefore, after separating the valuable elements, an acidic solution rich in low-value elements such as iron, magnesium, and manganese is often produced. In practice, chemical precipitation, resin adsorption, and other methods are often used to treat such solutions.
[0003] Conventional methods for removing iron ions from solutions mostly use alkaline substances such as lime, sodium hydroxide, and magnesium oxide to adjust the solution pH to 2.5-3.5, so that the iron ions are removed in the form of ferric hydroxide. If there are divalent iron ions in the solution, hydrogen peroxide, sodium hypochlorite, etc. must be added for pre-oxidation. This method requires a large amount of alkaline substances to neutralize the residual acid in the solution, which not only wastes the residual acid, but also produces a huge amount of iron-containing waste slag, increasing the treatment cost.
[0004] In the prior art, the divalent iron ions in the solution are oxidized to trivalent in advance, and an adsorption carrier is added, and then a metal oxide or metal carbonate is added to adjust the solution pH to 2.0-4.2, and the iron is removed in the form of iron hydroxide, and the iron removal slag is used as an adsorption material. The method achieves efficient removal and resource utilization of iron ions, but the method is only for solutions with iron ion concentrations below 5g / L, and is not suitable for treating high-content iron ion solutions. At the same time, this method requires the use of alkaline substances to adjust the solution pH, which has high production costs, and the reaction process is prone to form iron hydroxide colloidal substances, which affects the molding and application of adsorption materials.
[0005] There is also a method of pre-adjusting the acidity of the scandium-containing solution to 0.5-8 mol / L, then adding chloride ions to form complex anions with the iron ions in the solution, and then using chelating resin to adsorb and remove impurity ions such as iron and zirconium. This method removes iron ions under strong acidic conditions, but the method uses resin for adsorption treatment, and the iron ion concentration of the solution is 0.3-0.5 g / L, which is not suitable for treating high-concentration iron ion solutions. Summary of the invention
[0006] In view of the problem that the prior art needs to remove iron ions under weak acidic conditions, or the method for removing iron ions is complicated and requires the use of a large amount of reagents, the present invention provides a simple method for removing iron ions under strong acidic conditions.
[0007] Specifically, the present invention provides the following technical solutions:
[0008] A method for removing iron ions and recovering acid from a high-concentration iron-containing solution, comprising:
[0009] Step S1, pouring the iron-containing solution and an appropriate amount of sodium salt into a stirring tank and stirring evenly;
[0010] Step S2, adding the uniformly stirred iron-containing solution into a pressure reactor, and continuously introducing oxygen during the reaction process to react;
[0011] Step S3: After the reaction is completed, the reaction slurry is discharged into a sedimentation tank. After standing for a period of time, the filter residue sinks to the bottom of the tank, and the supernatant is discharged through the discharge port for recycling.
[0012] Optionally, in step S1, the iron-containing solution is obtained by using sulfuric acid as a leaching agent, and the solution after valuable elements are extracted is concentrated, and the anion is mainly sulfate; the iron content is 50-75 g / L (Fe 2+ :40~60g / L、Fe 3+ : 10-15 g / L) solution pH = 0-0.1.
[0013] Optionally, in step S1, the sodium salt is selected from one or more of sodium sulfate, sodium sulfite, sodium nitrate or sodium bisulfate, preferably sodium sulfate; the amount of sodium salt added is 15 to 35 g / L. The solution of the present invention comes from a sulfuric acid system, and the use of sodium sulfate has the advantages of being cheap and having low production costs; sodium sulfate is added to remove iron, and the corresponding product generated is sulfuric acid, and no other impurities are introduced, and the solution after iron removal can be reused.
[0014] Optionally, in step S2, the reaction temperature is 140-180° C., the reaction time is 1-2 h, the oxygen pressure is 1.2-1.5 MPa, and the reaction process is:
[0015] 12FeSO4+3O2+2Na2SO4+18H2O=4NaFe3(SO4)2(OH)6+6H2SO4
[0016] 3Fe2(SO4)3+Na2SO4+12H2O=2NaFe3(SO4)2(OH)6+6H2SO4
[0017] Optionally, in step S3, the standing time is 10 to 30 min, there are no suspended particles in the supernatant, the iron ion concentration is 3 to 6 g / L, and the hydrogen ion concentration is 2 to 2.5 mol / L.
[0018] The beneficial effects brought about by the technical solution provided by the present invention include at least:
[0019] 1) The invention can remove iron ions under strong acidic conditions, with an iron removal rate of up to 90%. It does not require the addition of additional alkaline substances to adjust the pH, thus saving reagent consumption and having low production costs.
[0020] 2) The invention removes iron in the range of solution pH = 0 to 0.1, and the acidity of the reaction system is relatively high (the acidity at the reaction end point can reach 2.0 to 2.5 mol / L), which can effectively prevent the remaining ions from entering the iron removal slag phase, and the iron removal slag is easy to handle and use.
[0021] 3) In the process of iron removal, new sulfuric acid is generated. After iron removal, the hydrogen ion concentration in the solution can reach 2.0-2.5 mol / L. This part of the residual acid can be recycled, which is green and environmentally friendly.
[0022] 4) The iron removal slag obtained by the invention has large particles and a fast sedimentation rate, and solid-liquid separation can be achieved without filter press equipment.
[0023] The invention can effectively remove iron ions from a high-concentration iron-containing solution, and can also recycle the residual acid, thereby having low production cost, being green and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 This is the XRD diagram of the iron removal slag prepared in the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] Comparative Example 1
[0028] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and a pH of 0.05 (hydrogen ion concentration of 0.9 mol / L), add 2 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0029] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 170°C, the oxygen pressure to 1.2MPa (saturated vapor pressure to 0.85MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0030] S3, the reaction slurry poured out from S2 was allowed to stand for 10 minutes, and the supernatant was taken for analysis and testing. The iron ion content in the obtained supernatant was 25.5g / L and the hydrogen ion concentration was 1.8mol / L. (This comparative example shows that the amount of sodium sulfate added was insufficient and the iron removal rate was very low)
[0031] Comparative Example 2
[0032] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and a pH of 0.05 (hydrogen ion concentration of 0.9 mol / L), add 10 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0033] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 140°C, the oxygen pressure to 1.2MPa (saturated vapor pressure to 0.45MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0034] S3, the reaction slurry poured out from S2 was allowed to stand for 10 minutes, and the supernatant was taken for analysis and testing. The iron ion content in the obtained supernatant was 17.5g / L and the hydrogen ion concentration was 2.01mol / L. (This comparative example shows that the reaction temperature is not enough and the iron removal rate of the solution is not enough)
[0035] Comparative Example 3
[0036] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and a pH of 0.05 (hydrogen ion concentration of 0.9 mol / L), add 10 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0037] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 170°C, the oxygen pressure to 0.90MPa (saturated vapor pressure to 0.85MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0038] S3, the reaction slurry poured out of S2 was allowed to stand for 10 minutes, and the supernatant was taken for analysis and testing. The iron ion content in the obtained supernatant was 14.6g / L and the hydrogen ion concentration was 1.97mol / L. (This comparative example shows that the oxygen pressure of the reaction is insufficient, that is, the oxygen pressure is insufficient, and the iron removal rate of the solution is insufficient)
[0039] Example 1
[0040] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and a pH of 0.05 (hydrogen ion concentration of 0.9 mol / L), add 10 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0041] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 170°C, the oxygen pressure to 1.2MPa (saturated vapor pressure to 0.85MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0042] S3. The reaction slurry poured out from S2 was allowed to stand for 10 min, and the supernatant was taken for analysis. The iron ion content in the obtained supernatant was 5.5 g / L, and the hydrogen ion concentration was 2.3 mol / L.
[0043] Example 2
[0044] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and a pH of 0.05 (hydrogen ion concentration of 0.9 mol / L), add 10 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0045] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 180°C, the oxygen pressure to 1.2MPa (saturated vapor pressure to 0.95MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0046] S3. The reaction slurry poured out from S2 was allowed to stand for 10 min, and the supernatant was taken for analysis. The iron ion content in the obtained supernatant was 3.5 g / L, and the hydrogen ion concentration was 2.6 mol / L.
[0047] Example 3
[0048] S1. Take 300 ml of a solution with an iron ion concentration of 55 g / L and pH = 0 (hydrogen ion concentration of 1 mol / L), add 10 g of sodium sulfate and stir at room temperature (25° C.) for 10 min to obtain a mixed solution.
[0049] S2. Pour the mixed solution of S1 into a pressure reactor for reaction. Set the reaction temperature to 170°C, the oxygen pressure to 1.2MPa (saturated vapor pressure to 0.85MPa), and the reaction time to 1.5h. After the reaction is completed, close the oxygen valve and pour out the reaction slurry.
[0050] S3. The reaction slurry poured out from S2 was allowed to stand for 10 min, and the supernatant was taken for analysis. The iron ion content in the obtained supernatant was 8.5 g / L, and the hydrogen ion concentration was 2.05 mol / L.
[0051] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for removing iron ions and recovering acid from a high concentration iron-containing solution, characterized in that: include: Step S1, pouring the iron-containing solution and an appropriate amount of sodium salt into a stirring tank and stirring evenly; Step S2, adding the uniformly stirred iron-containing solution into a pressure reactor, and continuously introducing oxygen during the reaction process to react; Step S3: After the reaction is completed, the reaction slurry is discharged into a sedimentation tank, and after standing for a period of time, the filter residue sinks to the bottom of the tank, and the supernatant is discharged through the discharge port for recycling; in: In step S1, the anions in the iron-containing solution are mainly sulfate; the solution pH is 0-0.1, and the sodium salt is sodium sulfate; In step S2, the reaction temperature is 170-180°C, the reaction time is 1-2h, and the oxygen pressure is 1.2-1.5MPa; In step S3, the standing time is 10 to 30 minutes, there are no suspended particles in the supernatant, and the hydrogen ion concentration is 2 to 2.5 mol / L.
2. The method according to claim 1, characterized in that In step S1, the iron content is 50-75 g / L.
3. The method according to claim 1, characterized in that In step S1, the amount of sodium salt added is 15-35 g / L.
4. The method according to claim 1, characterized in that: The iron ion concentration in the supernatant in step S3 is 3-6 g / L.