A piezoelectric ceramic material and its preparation method and use

By adjusting the composition of PZT-PZN-PNN material and adding specific additives, the lead oxide volatility problem and low output problems in high-temperature sintering are solved, and low-temperature sintering and high-performance piezoelectric ceramic materials are realized, suitable for high dielectric constants and high output piezoelectric actuators.

CN116813338BActive Publication Date: 2024-11-22KOSTER ELECTRONIC TECH (SHENZHEN) CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202310824025.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2024-11-22
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

Existing piezoelectric ceramic materials have problems with lead oxide volatility during high-temperature sintering, resulting in environmental pollution and unstable performance, and small output, which limits their wide application.

Method used

By adjusting the composition and ratio of the PZT-PZN-PNN quaternary material, adding specific contents of SrCO3, Li2CO3, Bi2O3 and ZnO as additives, reducing the sintering temperature and optimizing the material performance, forming a high dielectric constant and low dielectric loss piezoelectric ceramic material.

Benefits of technology

Low-temperature sintering is achieved, and the output of piezoelectric ceramic materials is improved. The dielectric constant reaches 3800~4200, the dielectric loss is ≤2%, and the piezoelectric strain constant d31 reaches 280~360pC/N. It is suitable for high-performance piezoelectric actuators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116813338B_ABST
    Figure CN116813338B_ABST
Patent Text Reader

Abstract

The present invention provides a piezoelectric ceramic material and a preparation method and use thereof. The piezoelectric ceramic material has a chemical formula of aPbZr x Ti 1‑x O 3 ‑bPbZn 1 / 3 Nb 2 / 3 O 3 ‑cPbNi 1 / 3 Nb 2 / 3 O 3 +d%SrCO 3 +e%Li 2 CO 3 +f%Bi 2 O 3 +g% ZnO; the present invention adjusts and optimizes the composition and ratio of the matrix material, and adopts a specific content of SrCO 3 , Li 2 CO 3 、Bi 2 O 3 And ZnO as additives, on the one hand, can greatly reduce the press sintering temperature, on the other hand, can effectively optimize the performance of the obtained piezoelectric ceramic material, so that the actuator formed by the piezoelectric ceramic material has a high dielectric constant of 3800-4200, while the dielectric loss can be ≤2%, and the piezoelectric strain constant d31 reaches 280-360pC / N, effectively improving the output.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of piezoelectric materials and relates to a piezoelectric ceramic material and a preparation method and application thereof. Background Art

[0002] Piezoelectric ceramics are functional materials that can realize the mutual conversion between mechanical energy and electrical energy. They are widely used in military, automotive, commercial and medical technology fields. At present, since the piezoelectric properties of lead-free piezoelectric ceramics are still quite different from those of lead zirconate titanate (PZT)-based piezoelectric ceramics, the production of piezoelectric ceramics is still concentrated on traditional PZT-based and its ternary and quaternary piezoelectric ceramics.

[0003] However, the content of lead oxide in PZT-based ceramics exceeds 60% of the total mass of the raw materials. Lead oxide is a volatile toxic substance. If you work in an environment with lead oxide for a long time, these lead oxides will accumulate in the human body, causing damage to the brain and nervous system. Therefore, achieving low-temperature sintering of PZT-based piezoelectric ceramics has important development value: it can reduce energy consumption; it can reduce the volatilization of lead oxide, avoid fluctuations in the components of piezoelectric ceramics and deviations from the designed composition, improve the qualified rate of products, and eliminate the environmental problems caused by the volatilization of lead oxide; there is no need for sealed sintering during the sintering process of piezoelectric ceramics, and the debinding sintering is completed at one time, which simplifies the process and reduces costs; in the preparation of multilayer piezoelectric devices, the sintering temperature is reduced to reduce the cost of multilayer piezoelectric devices.

[0004] Piezoelectric actuators (actuators or transducers) are devices that use the lateral expansion (d31 mode) or longitudinal expansion (d33 mode) of piezoelectric ceramics to apply an electric field in a certain direction to generate corresponding displacement and force. Due to its small size, good linearity, high displacement resolution, fast response speed, low energy consumption, and low heat generation, it has become an ideal micro-displacement drive device and is very suitable for applications in precision positioning, nano-machining, optical devices, aerospace, and other fields.

[0005] For example, in the prior art, a single piece of ceramic or a double piece of ceramic with the same polarity of a certain thickness is bonded to a substrate by epoxy resin. The thickness of the ceramic is generally above 0.1 mm. The circuit is connected in parallel, or two piezoelectric ceramic sheets with opposite polarities are glued together and connected in series in the circuit. The substrate constrains part of the ceramic. Under the excitation of the electric field, when one of the sheets stretches at a certain moment, the other shrinks, so that the vibration is converted into bending vibration. The actuator has a simple structure, but it has an obvious disadvantage of low output, generally within 0.5N, which limits its wider application and development.

[0006] CN101475373A discloses a piezoelectric ceramic material with a high-voltage electric strain constant d31 and a low piezoelectric voltage constant g31 and a preparation method thereof. The piezoelectric ceramic material has a new component composition and ratio, which can make d31 reach -388pC / N, but its preparation method requires sintering at a temperature as high as 1260 to 1320°C.

[0007] Therefore, there is still a need to develop a new piezoelectric ceramic material that can achieve low temperature sintering and has high output performance. Summary of the invention

[0008] In view of the problems existing in the prior art, the object of the present invention is to provide a piezoelectric ceramic material and a preparation method and use thereof. The piezoelectric ceramic material has the chemical formula of aPbZr x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3O3+d%SrCO3+e%Li2CO3+f%Bi2O3+g%ZnO; The present invention adjusts and optimizes the composition and ratio of the matrix material, and adopts specific contents of SrCO3, Li2CO3, Bi2O3 and ZnO as additives. On the one hand, it can greatly reduce the sintering temperature of the piezoelectric ceramic material, and on the other hand, it can effectively optimize the performance of the obtained piezoelectric ceramic material, so that the actuator formed by the piezoelectric ceramic material has a high dielectric constant of 3800-4200, while the dielectric loss can be ≤2%, and the piezoelectric strain constant d31 reaches 280-360pC / N, effectively improving the output.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a piezoelectric ceramic material, characterized in that the piezoelectric ceramic material has a general chemical formula of:

[0011] aiZd x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3 O3+d%SrCO3+e%Li2CO3+f%Bi2O3+g%ZnO;

[0012] Among them: aPbZr x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3O3 is a matrix material, SrCO3, Li2CO3, Bi2O3 and ZnO are additives, and d%, e%, f% and g% respectively represent the mass percentage of the corresponding additives in the matrix material.

[0013] The piezoelectric ceramic material obtained by the present invention is a homogeneous solid solution formed by an additive and a base material. The present invention adjusts and optimizes the composition and ratio of the base material, and adopts a specific content of SrCO3, Li2CO3, Bi2O3 and ZnO as additives. On the one hand, the sintering temperature of the piezoelectric ceramic material can be greatly reduced, and on the other hand, the performance of the obtained piezoelectric ceramic material can be effectively optimized. Specifically, the base material of the present invention is a quaternary system PZT-PZN-PNN. The present invention effectively improves the dielectric constant of the PZT-PZN-PNN quaternary system material by adding strontium carbonate SrCO3 and slowly adjusts the Curie temperature of the material. The sintering temperature of the ceramic is quickly reduced by adding lithium carbonate Li2CO3 and bismuth oxide Bi2O3 low melting point compounds, and at the end of sintering, they are solid-dissolved into the perovskite lattice without forming a glass phase at the grain boundary, so the dielectric loss of the ceramic material does not increase. The addition of zinc oxide ZnO appropriately adjusts the performance of the ceramic material: the zinc ion is divalent and has a low valence state, but the ion radius is larger than the zirconium / titanium ion radius, which plays a role of neutral doping.

[0014] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0015] As a preferred technical solution of the present invention, in the piezoelectric ceramic material, 0.45≤x≤0.47, for example, 0 can be 0.45, 0.452, 0.454, 0.456, 0.458, 0.46, 0.462, 0.464, 0.466, 0.468 or 0.47, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0016] Preferably, 0.6≤a≤0.8, for example, it can be 0.6, 0.62, 0.64, 0.66, 0.68, 0.7, 0.72, 0.74, 0.76, 0.78 or 0.8, 0.05≤b≤0.15, for example, it can be 0.05, 0.07, 0.09, 0.11, 0.13 or 0.15, 0.15≤c≤0.25, for example, it can be 0.15, 0.17, 0.19, 0.21, 0.23 or 0.25, and a+b+c=1, but it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable.

[0017] Preferably, 0.2%≤d%≤0.3%, for example, it can be 0.2%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29% or 0.3%, etc., but it is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0018] Preferably, 0.3%≤e%≤0.5%, for example 0.3%, 0.32%, 0.34%, 0.36%, 0.38%, 0.4%, 0.42%, 0.44%, 0.46%, 0.48% or 0.5%, etc., but are not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0019] Preferably, 0.5%≤f%≤0.7%, for example 0.5%, 0.52%, 0.54%, 0.56%, 0.58%, 0.6%, 0.62%, 0.64%, 0.68% or 0.7%, etc., but are not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0020] Preferably, 0.05%≤g%≤0.15%, for example 0.05%, 0.07%, 0.09%, 0.11%, 0.13% or 0.15%, etc., but it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable.

[0021] Preferably, d%+e%+f%+g%≤1.5%, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%, etc., but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0022] In a second aspect, the present invention provides a method for preparing the piezoelectric ceramic material according to the first aspect, the preparation method comprising the following steps:

[0023] Prepare various raw materials according to the general chemical formula. First, mix the raw materials of the base material and SrCO3. After the first sintering, add Li2CO3, Bi2O3 and ZnO. After the second sintering, the piezoelectric ceramic material is obtained.

[0024] It should be noted that the raw materials used in the present invention are all pure crystalline solid powders of the corresponding substances.

[0025] As a preferred technical solution of the present invention, the temperature of the first sintering is 920-980°C, for example, 920°C, 925°C, 930°C, 935°C, 940°C, 945°C, 950°C, 955°C, 960°C, 965°C, 970°C, 975°C or 980°C, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0026] Preferably, the holding time of the first sintering is 2 to 4 h, for example 2 h, 2.2, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.8 h or 4 h, but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0027] Preferably, the second sintering temperature is 900-940°C, for example 900°C, 905°C, 910°C, 915°C, 920°C, 925°C, 930°C, 935°C or 940°C, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0028] Preferably, the holding time of the second sintering is 3 to 5 h, for example 2 h, 2.2, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.8 h, 4 h, 4.2 h, 4.4 h, 4.8 h or 5 h, but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0029] Preferably, after adding Li2CO3, Bi2O3 and ZnO, fine grinding is first performed and then a second sintering is performed.

[0030] Preferably, after the fine grinding, a forming process is performed, and then a second sintering is performed.

[0031] Preferably, the molding process comprises a tape casting process.

[0032] In a third aspect, the present invention provides a piezoelectric ceramic actuator, comprising an electrode layer and a piezoelectric layer formed of the piezoelectric ceramic material described in the first aspect.

[0033] As a preferred technical solution of the present invention, the piezoelectric ceramic actuator is a transverse piezoelectric ceramic actuator.

[0034] Preferably, the transverse piezoelectric ceramic actuator is composed of the piezoelectric layer and the electrode layer stacked on each other.

[0035] Preferably, the thickness of the electrode layer is 2 to 4 μm, for example 2.2 μm, 2.4 μm, 2.6 μm, 2.8 μm, 3 μm, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm or 4 μm, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0036] Preferably, the thickness of the piezoelectric layer is 20 to 70 μm, for example 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm or 70 μm, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0037] Preferably, the thickness of the lateral piezoelectric ceramic actuator is 700-900 μm, for example, 700 μm, 720 μm, 740 μm, 760 μm, 780 μm, 800 μm, 820 μm, 840 μm, 860 μm, 880 μm or 900 μm, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0038] Preferably, the number of piezoelectric layers in the lateral piezoelectric ceramic actuator is 16 to 24 layers, for example 16 layers, 17 layers, 18 layers, 19 layers, 20 layers, 21 layers, 22 layers, 23 layers or 24 layers, etc., but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0039] Preferably, the transverse piezoelectric ceramic actuator is divided into a first part and a second part along a thickness direction, and the polarization direction of the piezoelectric layer in the first part is opposite to that of the piezoelectric layer in the second part.

[0040] Preferably, the number of piezoelectric layers in the first portion is the same as the number of piezoelectric layers in the second portion.

[0041] Preferably, a protective layer is disposed at an end of the first part farthest from the second part, at an end of the second part farthest from the first part, and between the first part and the second part.

[0042] Preferably, the protection layer comprises the piezoelectric ceramic material.

[0043] Preferably, in the first part, the electrode layer includes a first electrode layer and a common electrode layer, and the first electrode layer and the common electrode layer are arranged alternately in sequence along the thickness direction of the first part; the first electrode layer extends to the outer surface of the piezoelectric ceramic actuator to form a first electrode.

[0044] In the second part, the electrode layer includes a second electrode layer and a common electrode layer, and the second electrode layer and the common electrode layer are arranged alternately in sequence along the thickness direction of the second part; the second electrode layer extends to the outer surface of the piezoelectric ceramic actuator to form a second electrode.

[0045] The common electrode layer in the first part and the second part extends to the outer surface of the piezoelectric ceramic actuator to form a common electrode.

[0046] Preferably, the dielectric constant of the lateral piezoelectric ceramic actuator is 3800 to 4200, for example, 3800, 3850, 3900, 3950, 4000, 4050, 4100, 4150 or 4200, etc., the dielectric loss is ≤2%, for example, it can be 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2%, etc., and the piezoelectric strain constant d31 is -280 to -360 pC / N, for example, -280 pC / N , -285pC / N, -290pC / N, -295pC / N, -300pC / N, -305pC / N, -310pC / N, -315pC / N, -320pC / N, -325pC / N, -330pC / N, -335pC / N, -340pC / N, -345pC / N, -350pC / N, -355pC / N or -360pC / N, but are not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0047] The low-temperature sintered piezoelectric ceramic material obtained by the present invention is particularly suitable for lateral actuators. It is made by stacking and co-sintering low-temperature co-fired piezoelectric ceramics. The thickness of a single layer of ceramic is 20 μm or more and 70 mm or less. The output of the obtained lateral actuator is relatively large and can be used in the field of optical lens dimming.

[0048] In a fourth aspect, the present invention provides a method for manufacturing the piezoelectric ceramic actuator according to the third aspect, the manufacturing method comprising the following steps:

[0049] (1) preparing various raw materials according to the general chemical formula, first mixing the raw materials of the matrix material and SrCO3, adding Li2CO3, Bi2O3 and ZnO after the first sintering, fine grinding, and then performing a molding process to obtain a diaphragm as a piezoelectric layer;

[0050] (2) preparing an electrode layer on the first piezoelectric layer, stacking a second piezoelectric layer, and preparing an electrode layer on the second piezoelectric layer, and alternately stacking piezoelectric layers and preparing electrode layers until a target number of layers is reached, thereby obtaining a composite;

[0051] (3) The composite is subjected to a second sintering and then polarized to obtain a piezoelectric ceramic actuator.

[0052] The present invention combines the preparation process of piezoelectric ceramic materials with the manufacturing process of actuators, and uses the "diaphragm" obtained after the piezoelectric ceramic material is formed and before the second sintering to form an actuator structure (composite), and then the composite is uniformly sintered for the second time. At this time, the second sintering is the co-sintering process of all the diaphragms in the composite, so that the final actuator device can be formed while the piezoelectric ceramic material is formed. It should also be emphasized that since the present invention optimizes the piezoelectric ceramic material, its sintering temperature is greatly reduced, so the co-sintering of the composite can be carried out at a lower temperature to achieve "low temperature sintering".

[0053] As a preferred technical solution of the present invention, the manufacturing method uses the piezoelectric ceramic material diaphragm as a protective layer, and step (2) of the manufacturing method includes the following steps:

[0054] A first piezoelectric layer is arranged on a protective layer, an electrode layer is prepared on the first piezoelectric layer, a second piezoelectric layer is superimposed, an electrode layer is prepared on the second piezoelectric layer, and piezoelectric layers are superimposed and electrode layers are prepared alternately until the n-th piezoelectric layer and the n-th electrode layer in the first part are reached, a protective layer is arranged on the n-th electrode layer, an n+1-th piezoelectric layer is arranged thereon, an electrode layer is prepared on the n+1-th piezoelectric layer, an n+2-th piezoelectric layer is superimposed, an electrode layer is prepared on the n+2-th piezoelectric layer, and piezoelectric layers are superimposed and electrode layers are prepared alternately until the n+m-th piezoelectric layer and the n+m-th electrode layer in the second part are reached, and a protective layer is arranged on the n+m-th electrode layer to form a composite.

[0055] As a preferred technical solution of the present invention, the manufacturing method comprises the following steps:

[0056] (1) Prepare the membrane:

[0057] aiZd x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3O3+d%SrCO3+e%Li2CO3+f%Bi2O3+g%ZnO, 0.45≤x≤0.47; 0.6≤a≤0.8, 0.05≤b≤0.15, 0.15≤c≤0.25, and a+b+c=1, 0.2%≤d%≤0.3%, 0.3%≤e%≤0.5%, 0.5%≤f%≤0.7%, 0.05%≤g%≤0.15%, prepare various raw materials according to the above chemical formula, first mix the raw materials of the matrix material and SrCO3, after the first sintering at 920~980℃ for 2~4h, add Li2CO3, Bi2O3 and ZnO and grind them finely, then perform tape casting to obtain a diaphragm, which is used as a piezoelectric layer and a protective layer at the same time;

[0058] (2) providing a first piezoelectric layer on a protective layer;

[0059] A first electrode layer is prepared on the first piezoelectric layer, a second piezoelectric layer is superimposed, and a common electrode layer is prepared on the second piezoelectric layer, and the piezoelectric layers are superimposed and the electrode layers are prepared alternately, and the first electrode layer and the common electrode layer are arranged in turn, until the nth piezoelectric layer and the nth electrode layer are reached, where n is an even number between 8 and 12, to form a first part;

[0060] Disposing a protective layer on the nth electrode layer;

[0061] Arranging the n+1th piezoelectric layer on the protective layer arranged on the nth electrode layer, preparing the second electrode layer on the n+1th piezoelectric layer, superimposing the n+2th piezoelectric layer, preparing the common electrode layer on the n+2th piezoelectric layer, alternately superimposing the piezoelectric layers and preparing the electrode layers, and making the second electrode layer and the common electrode layer arranged in turn in sequence until reaching the n+mth piezoelectric layer and the n+mth electrode layer, n+m is an even number between 16 and 24 and n=m, to form a second part;

[0062] Disposing a protective layer on the n+m-th electrode layer to form a composite body;

[0063] The first electrode layer extends to the outer surface of the composite body to form a first electrode; the second electrode layer extends to the outer surface of the composite body to form a second electrode; the common electrode layer in the first part and the second part extends to the outer surface of the composite body to form a common electrode;

[0064] (3) After the composite is subjected to a second sintering at 900-940° C. for 3-5 hours, the first electrode is used as the positive electrode, the common electrode is used as the negative electrode, and an external power supply is connected for polarization; the second electrode is used as the negative electrode, the common electrode is used as the positive electrode, and an external power supply is connected for polarization; after polarization, the polarization directions of the piezoelectric layers in the first part and the second part are opposite, thereby obtaining a lateral piezoelectric ceramic actuator.

[0065] In a fifth aspect, the present invention provides a use of the piezoelectric ceramic actuator described in the third aspect or the piezoelectric ceramic actuator obtained by the manufacturing method described in the fourth aspect, and the uses include textile machinery drive plates, buzzer plates, piezoelectric pumps and optical lenses.

[0066] Compared with the prior art solutions, the present invention has at least the following beneficial effects:

[0067] The present invention adjusts and optimizes the composition and ratio of the matrix material in the piezoelectric ceramic material, and adopts specific contents of SrCO3, Li2CO3, Bi2O3 and ZnO as additives. On the one hand, the sintering temperature of the piezoelectric ceramic material can be greatly reduced to achieve low-temperature sintering of the piezoelectric ceramic and the actuator containing the piezoelectric ceramic. On the other hand, the performance of the obtained piezoelectric ceramic material can be effectively optimized, so that the actuator formed by the piezoelectric ceramic material has a high dielectric constant of 3800 to 4200, while the dielectric loss can be ≤2%, and the piezoelectric strain constant d31 reaches 280 to 360 pC / N, effectively improving the output. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 is a schematic diagram of the layer structure of the lateral piezoelectric ceramic actuator obtained in Application Example 1;

[0069] Figure 2-Figure 4 is a schematic diagram of the lateral piezoelectric ceramic actuator obtained in Application Example 1 in different viewing directions;

[0070] Figure 5 is a schematic diagram of the shapes of the first electrode layer, the second electrode layer and the common electrode layer in Application Example 1;

[0071] Figure 6 is a schematic diagram of the installation and use status of the obtained transverse piezoelectric ceramic actuator;

[0072] In the figure: 1-piezoelectric layer, 2-first electrode layer, 21-first electrode, 3-common electrode layer, 31-common electrode, 4-second electrode layer, 41-second electrode, 5-protective layer. DETAILED DESCRIPTION

[0073] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0074] Example 1

[0075] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. The piezoelectric ceramic material has a general chemical formula of:

[0076] 0.7PbZr 0.46 Ti0.54 O3-0.1PbZn 1 / 3 Nb 2 / 3 O3-0.2PbNi 1 / 3 Nb 2 / 3 O3+0.25%SrCO3+0.4%Li2CO3+0.6%Bi2O3+0.1%ZnO;

[0077] The preparation method is:

[0078] Prepare the various raw materials according to the above chemical formula. First, mix the raw materials of the matrix material and SrCO3. After the first sintering at 950°C for 3 hours, add Li2CO3, Bi2O3 and ZnO and grind them finely. Then, perform tape casting. Finally, perform the second sintering at 920°C for 4 hours to obtain the piezoelectric ceramic material.

[0079] Example 2

[0080] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. 0.46 Ti 0.54 O3 adjusted to PbZr 0.45 Ti 0.55 O3, that is, the chemical formula of the piezoelectric ceramic material is:

[0081] 0.7PbZr 0.45 Ti 0.55 O3-0.1PbZn 1 / 3 Nb 2 / 3 O3-0.2PbNi 1 / 3 Nb 2 / 3 O3+0.25%SrCO3+0.4%Li2CO3+0.6%Bi2O3+0.1%ZnO;

[0082] Except for the different amounts of raw materials, other conditions of the preparation method are exactly the same as those of Example 1.

[0083] Example 3

[0084] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. x0.46 Ti 0.54 O3 adjusted to PbZr 0.47 Ti 0.53 O3, that is, the chemical formula of the piezoelectric ceramic material is:

[0085] 0.7PbZr 0.47 Ti 0.53 O3-0.1PbZn 1 / 3 Nb 2 / 3 O3-0.2PbNi1 / 3 Nb 2 / 3 O3+0.25%SrCO3+0.4%Li2CO3+0.6%Bi2O3+0.1%ZnO;

[0086] Except for the different amounts of raw materials, other conditions of the preparation method are exactly the same as those of Example 1.

[0087] Except for the different amounts of raw materials, other conditions of the preparation method are exactly the same as those of Example 1.

[0088] Example 6

[0089] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of SrCO3 in the additive of the piezoelectric ceramic material is adjusted from 0.25% to 0.2%, other conditions are exactly the same as those in Embodiment 1.

[0090] Example 7

[0091] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of SrCO3 in the additive of the piezoelectric ceramic material is adjusted from 0.25% to 0.3%, other conditions are exactly the same as those in Embodiment 1.

[0092] Example 8

[0093] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of Li2CO3 in the additive of the piezoelectric ceramic material is adjusted from 0.4% to 0.3%, other conditions are exactly the same as those in Embodiment 1.

[0094] Example 9

[0095] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of Li2CO3 in the additive of the piezoelectric ceramic material is adjusted from 0.4% to 0.5%, other conditions are exactly the same as those in Embodiment 1.

[0096] Example 10

[0097] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of Bi2O3 in the additive of the piezoelectric ceramic material is adjusted from 0.6% to 0.5%, other conditions are exactly the same as those in Embodiment 1.

[0098] Embodiment 11

[0099] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of Bi2O3 in the additive of the piezoelectric ceramic material is adjusted from 0.6% to 0.7%, other conditions are exactly the same as those in Embodiment 1.

[0100] Example 12

[0101] This embodiment provides a piezoelectric ceramic material and a preparation method thereof. Except that the amount of ZnO in the additive of the piezoelectric ceramic material is adjusted from 0.1% to 0.05%, other conditions are exactly the same as those in Embodiment 1.

[0102] Comparative Example 1

[0103] This comparative example provides a piezoelectric ceramic material and a preparation method thereof. The preparation method does not use any additives, that is, the chemical formula of the obtained piezoelectric ceramic material is:

[0104] 0.7PbZr 0.46 Ti 0.54 O3-0.1PbZn 1 / 3 Nb 2 / 3 O3-0.2PbNi 1 / 3 Nb 2 / 3 O3;

[0105] The preparation method is completely the same as Example 1 except that no additives are used.

[0106] Application Example 1

[0107] The diaphragm obtained after tape casting and before the second sintering in the embodiment and the comparative example is made into a transverse piezoelectric ceramic actuator by the following manufacturing method. The layer structure schematic diagram of the transverse piezoelectric ceramic actuator is shown in FIG. Figure 1 As shown, the manufacturing method is:

[0108] (1) preparing a diaphragm so that it serves as a piezoelectric layer 1 and also as a protective layer 5;

[0109] (2) a first piezoelectric layer 1 is provided on a protective layer 5;

[0110] A first electrode layer 2 is prepared on the first piezoelectric layer 1, and a second piezoelectric layer 1 is superimposed. A common electrode layer 3 is prepared on the second piezoelectric layer 1. The piezoelectric layers 1 are superimposed and the electrode layers are prepared alternately, and the first electrode layer 2 and the common electrode layer 3 are arranged in turn in sequence until the tenth piezoelectric layer 1 and the tenth electrode layer are reached, and the first electrode layer is the common electrode layer 3, forming a first part;

[0111] A protective layer 5 is provided on the tenth electrode layer;

[0112] The 11th piezoelectric layer 1 is arranged on the protective layer 5 arranged on the 10th electrode layer, the second electrode layer 4 is prepared on the 11th piezoelectric layer 1, the 12th piezoelectric layer 1 is superimposed, and the common electrode layer 3 is prepared on the 12th piezoelectric layer 1, and the piezoelectric layers 1 and the electrode layers are superimposed and prepared alternately, and the second electrode layer 4 and the common electrode layer 3 are arranged in turn in sequence until the 20th piezoelectric layer 1 and the 20th electrode layer are reached, and the 20th electrode layer is the common electrode layer 3, forming the second part;

[0113] A protective layer 5 is provided on the 20th electrode layer to form a composite body;

[0114] In this application example, the shapes of the first electrode layer 2, the second electrode layer 4 and the common electrode layer 3 are as follows: Figure 5 as shown; Figure 2 and Figure 4 As shown, the small rectangular portion on the right side of the first electrode layer 2 extends to the outer surface of the composite body to form a first electrode 21, and the small rectangular portion on the right side of the second electrode layer 4 extends to the outer surface of the composite body to form a second electrode 41; Figure 2 and Figure 3 As shown, the small rectangular portion in the upper part of the common electrode layer 3 in the first part and the second part extends to the outer surface of the composite body to form a common electrode 31, and the small rectangular portion in the lower part is not exposed;

[0115] (3) After the composite is subjected to a second sintering at 920° C. for 4 hours, the first electrode 21 is used as the positive electrode, the common electrode 31 is used as the negative electrode, and an external power source is connected for polarization; the second electrode 41 is used as the negative electrode, the common electrode 31 is used as the positive electrode, and an external power source is connected for polarization; after the polarization is completed, the polarization directions of the piezoelectric layers 1 in the first part and the second part are opposite, and a lateral piezoelectric ceramic actuator is obtained;

[0116] In this application example, the thickness of the piezoelectric layer 1 is 32 μm, the thickness of the first electrode layer 2, the second electrode layer 4 and the common electrode layer 3 are all 3.2 μm, and the size of the obtained lateral piezoelectric ceramic actuator is 20*8*0.8 (mm 3 ).

[0117] It should be noted that in some embodiments, the shapes of the first electrode layer 2 and the second electrode layer 4 in Application Example 1 can be interchangeable; the lower small rectangular portion of the common electrode layer 3 can be extended to the outer surface of the composite to form a common electrode 31, so that the upper small rectangle is hidden or not set, or the upper small rectangle and the lower small rectangle are respectively extended to the outer surface of the composite to form a common electrode 31.

[0118] Application Example 2

[0119] The diaphragm obtained in Example 1 after tape casting and before the second sintering is made into a lateral piezoelectric ceramic actuator by the following manufacturing method, wherein in step (2), the number of piezoelectric layers 1 in the first part and the second part is adjusted from 10 layers to 6 layers. Apart from this, other conditions are exactly the same as those in Application Example 1.

[0120] The transverse piezoelectric ceramic actuators obtained in Application Example 1-2 were tested. Figure 6 As shown, one end of the obtained transverse piezoelectric ceramic actuator is clamped, as shown in Figure 6 As shown by the arrow on the right, the other end remains free, the first electrode 21 and the second electrode 41 are connected as one pole, the common electrode 31 is used as the other pole, and an external AC power source is connected for driving. Then the bending vibration direction and the output direction of the free end are as follows: Figure 6 The results are shown in Table 1.

[0121] Table 1

[0122]

[0123] It can be seen from the above results that an appropriate amount of strontium carbonate can improve the dielectric constant of ceramics; the addition of too much bismuth oxide will rapidly increase the dielectric loss of ceramic materials and reduce the performance of ceramic materials; when the layer thickness of the piezoelectric ceramic material in the actuator remains unchanged, the output of the actuator decreases as the number of layers decreases; since Comparative Example 1 only has the raw materials of the base material and does not contain additives during preparation, it is impossible to obtain piezoelectric ceramic materials at the first and second sintering temperatures of Example 1, and its applicable sintering temperature should be 1260-1280°C, so the material obtained in Comparative Example 1 cannot be used to make an actuator, and " / " in Table 1 represents no result. It can be seen that the present invention uses specific contents of SrCO3, Li2CO3, Bi2O3 and ZnO as additives, which can greatly reduce the sintering temperature of the piezoelectric ceramic material on the one hand, and can effectively optimize the performance of the obtained piezoelectric ceramic material on the other hand.

[0124] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0125] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0126] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0127] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A piezoelectric ceramic actuator, characterized in that: A piezoelectric layer comprising an electrode layer and a piezoelectric ceramic material; the thickness of the piezoelectric layer is 20-70 μm; The general chemical formula of the piezoelectric ceramic material is: <h2 style=";text-align:left;direction:ltr">aPbZr<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> Ti<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> O3-bPbZn<h2 style=";text-align:left;direction:ltr"> 1 / 3 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 2 / 3 <h2 style=";text-align:left;direction:ltr"> O3-cPbNi<h2 style=";text-align:left;direction:ltr"> 1 / 3 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 2 / 3 <h2 style=";text-align:left;direction:ltr"> O3+d%SrCO3+e%Li2CO3+f%Bi2O3+g%ZnO; Among them: aPbZr x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3 O3 is the matrix material, SrCO3, Li2CO3, Bi2O3 and ZnO are additives, d%, e%, f% and g% respectively represent the mass percentage of the corresponding additive in the matrix material; 0.45≤x≤0.47; 0.6≤a≤0.8, 0.05≤b≤0.15, 0.15≤c≤0.25, and a+b+c=1; 0.2%≤d%≤0.3%; 0.3%≤e%≤0.5%; 0.5%≤f%≤0.7%; 0.05%≤g%≤0.15%; d%+e%+f%+g%≤1.5%.

2. The piezoelectric ceramic actuator according to claim 1, characterized in that: The piezoelectric ceramic material is obtained by the following method, which comprises the following steps: Prepare various raw materials according to the general chemical formula, first mix the raw materials of the base material and SrCO3, add Li2CO3, Bi2O3 and ZnO after the first sintering, and obtain the piezoelectric ceramic material after the second sintering; The temperature of the first sintering is 920-980°C; the temperature of the second sintering is 900-940°C.

3. The piezoelectric ceramic actuator according to claim 2, characterized in that: The holding time of the first sintering is 2 to 4 hours; the holding time of the second sintering is 3 to 5 hours; after adding Li2CO3, Bi2O3 and ZnO, fine grinding is first performed, and then the second sintering is performed; after the fine grinding, a molding process is performed, and then the second sintering is performed; the molding process includes a tape casting molding process.

4. The piezoelectric ceramic actuator according to claim 1, characterized in that: The piezoelectric ceramic actuator is a transverse piezoelectric ceramic actuator.

5. The piezoelectric ceramic actuator according to claim 4, characterized in that: The transverse piezoelectric ceramic actuator is composed of the piezoelectric layer and the electrode layer stacked on each other.

6. The piezoelectric ceramic actuator according to claim 1, characterized in that: The thickness of the electrode layer is 2-4 μm.

7. The piezoelectric ceramic actuator according to claim 4, characterized in that: The thickness of the lateral piezoelectric ceramic actuator is 700-900 μm.

8. The piezoelectric ceramic actuator according to claim 4, characterized in that: The number of piezoelectric layers in the transverse piezoelectric ceramic actuator is 16 to 24.

9. The piezoelectric ceramic actuator according to claim 4, characterized in that: The transverse piezoelectric ceramic actuator is divided into a first part and a second part along a thickness direction, and the polarization direction of the piezoelectric layer in the first part is opposite to that of the piezoelectric layer in the second part.

10. The piezoelectric ceramic actuator according to claim 9, characterized in that: The number of piezoelectric layers in the first portion is the same as the number of piezoelectric layers in the second portion.

11. The piezoelectric ceramic actuator according to claim 9, characterized in that: A protective layer is disposed at one end of the first part farthest from the second part, at one end of the second part farthest from the first part, and between the first part and the second part.

12. The piezoelectric ceramic actuator according to claim 11, characterized in that: The protection layer includes the piezoelectric ceramic material.

13. The piezoelectric ceramic actuator according to claim 9, characterized in that: In the first part, the electrode layer includes a first electrode layer and a common electrode layer, and the first electrode layer and the common electrode layer are arranged alternately in sequence along the thickness direction of the first part; the first electrode layer extends to the outer surface of the piezoelectric ceramic actuator to form a first electrode; In the second part, the electrode layer includes a second electrode layer and a common electrode layer, and the second electrode layer and the common electrode layer are arranged alternately in sequence along the thickness direction of the second part; the second electrode layer extends to the outer surface of the piezoelectric ceramic actuator to form a second electrode; The common electrode layer in the first part and the second part extends to the outer surface of the piezoelectric ceramic actuator to form a common electrode.

14. The piezoelectric ceramic actuator according to claim 1, characterized in that: The dielectric constant of the piezoelectric ceramic actuator is 3800-4200, the dielectric loss is ≤2%, and the piezoelectric strain constant d31 is 280-360 pC / N.

15. A method for manufacturing a piezoelectric ceramic actuator according to any one of claims 1 to 14, characterized in that: The manufacturing method comprises the following steps: (1) preparing various raw materials according to the general chemical formula, first mixing the raw materials of the matrix material and SrCO3, adding Li2CO3, Bi2O3 and ZnO after the first sintering, fine grinding, and then performing a molding process to obtain a diaphragm as a piezoelectric layer; (2) preparing an electrode layer on the first piezoelectric layer, stacking a second piezoelectric layer, and preparing an electrode layer on the second piezoelectric layer, and alternately stacking piezoelectric layers and preparing electrode layers until the target number of layers is reached, thereby obtaining a composite; (3) The composite is subjected to a second sintering and then polarized to obtain a piezoelectric ceramic actuator.

16. The method for manufacturing a piezoelectric ceramic actuator according to claim 15, characterized in that: The manufacturing method uses the diaphragm as a protective layer, and step (2) of the manufacturing method comprises the following steps: A first piezoelectric layer is arranged on a protective layer, an electrode layer is prepared on the first piezoelectric layer, a second piezoelectric layer is superimposed, an electrode layer is prepared on the second piezoelectric layer, and piezoelectric layers are superimposed and electrode layers are prepared alternately until the n-th piezoelectric layer and the n-th electrode layer in the first part are reached, a protective layer is arranged on the n-th electrode layer, an n+1-th piezoelectric layer is arranged thereon, an electrode layer is prepared on the n+1-th piezoelectric layer, an n+2-th piezoelectric layer is superimposed, an electrode layer is prepared on the n+2-th piezoelectric layer, and piezoelectric layers are superimposed and electrode layers are prepared alternately until the n+m-th piezoelectric layer and the n+m-th electrode layer in the second part are reached, and a protective layer is arranged on the n+m-th electrode layer to form a composite.

17. The method for manufacturing a piezoelectric ceramic actuator according to claim 15 or 16, characterized in that: The manufacturing method comprises the following steps: (1) Prepare the diaphragm: aiZd x Ti 1-x O3-bPbZn 1 / 3 Nb 2 / 3 O3-cPbNi 1 / 3 Nb 2 / 3 O3+d%SrCO3+e%Li2CO3+f%Bi2O3+g%ZnO, 0.45≤x≤0.47; 0.6≤a≤0.8, 0.05≤b≤0.15, 0.15≤c≤0.25, and a+b+c=1, 0.2%≤d%≤0.3%, 0.3%≤e%≤0.5%, 0.5%≤f%≤0.7%, 0.05%≤g%≤0.15%, prepare each raw material according to the above chemical formula, first mix the raw material of the matrix material and SrCO3, after the first sintering at 920~980℃ for 2~4h, add Li2CO3, Bi2O3 and ZnO and grind them finely, then perform tape casting to obtain a diaphragm, which is used as a piezoelectric layer and a protective layer at the same time; (2) providing a first piezoelectric layer on a protective layer; A first electrode layer is prepared on the first piezoelectric layer, a second piezoelectric layer is superimposed, and a common electrode layer is prepared on the second piezoelectric layer, and the piezoelectric layers are superimposed and the electrode layers are prepared alternately, and the first electrode layer and the common electrode layer are arranged in turn, until the nth piezoelectric layer and the nth electrode layer are reached, where n is an even number between 8 and 12, to form a first part; Disposing a protective layer on the nth electrode layer; Arranging the n+1th piezoelectric layer on the protective layer arranged on the nth electrode layer, preparing the second electrode layer on the n+1th piezoelectric layer, superimposing the n+2th piezoelectric layer, and preparing the common electrode layer on the n+2th piezoelectric layer, alternately superimposing the piezoelectric layers and preparing the electrode layers, and making the second electrode layer and the common electrode layer arranged in turn in sequence until reaching the n+mth piezoelectric layer and the n+mth electrode layer, n+m is an even number between 16 and 24 and n=m, to form a second part; Disposing a protective layer on the n+m-th electrode layer to form a composite body; The first electrode layer extends to the outer surface of the composite body to form a first electrode; The second electrode layer extends to the outer surface of the composite body to form a second electrode; the common electrode layer in the first part and the second part extends to the outer surface of the composite body to form a common electrode; (3) After the composite is subjected to a second sintering at 900-940° C. for 3-5 hours, the first electrode is used as the positive electrode, the common electrode is used as the negative electrode, and an external power supply is connected for polarization; the second electrode is used as the negative electrode, the common electrode is used as the positive electrode, and an external power supply is connected for polarization; after the polarization is completed, the polarization directions of the piezoelectric layers in the first part and the second part are opposite, thereby obtaining a lateral piezoelectric ceramic actuator.

18. Use of the piezoelectric ceramic actuator according to any one of claims 1 to 14 or the piezoelectric ceramic actuator obtained by the manufacturing method according to any one of claims 15 to 17, characterized in that: The applications include textile machinery drive sheets, buzzer sheets, piezoelectric pumps and optical lenses.

Citation Information

Patent Citations

  • High piezoelectric strain constant d31, low piezoelectric strain constant g31 piezoelectric ceramic material and preparation thereof

    CN101475373A

  • Addition for reducing piezoelectric ceramics sintering temperature of electro-acoustic conversion device

    CN101386536A

  • Additive and application thereof for reducing sintering temperature of piezoceramic

    CN102531638A

  • Annular multilayer piezoelectric motor ceramic chip of monolithic structure

    CN103441213A

  • Zinc niobium and nickel niobium lead zirconate titanate piezoelectric ceramic

    CN103467089A