A sulfur capture catalyst for diesel engine and preparation method thereof
By placing wall-flow sulfur capture catalyst upstream of the diesel engine post-treatment catalyst, using the combination of modified alumina and alkali metal salts, the problem of diesel engine catalysts being susceptible to sulfur poisoning is solved, and high-efficiency sulfide capture and The stability of the catalyst is improved and is suitable for high humidity and heat application scenarios.
Patent Information
- Application Number
- CN202310837761.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-07-10
AI Technical Summary
Diesel engine post-treatment catalysts are susceptible to sulfur poisoning, resulting in frequent failures. The prior art has shortcomings in improving sulfur resistance, especially after the SCR catalyst is moved forward, the problem of sulfur poisoning is more prominent.
The method of mixing uniform preparation of molecular sieve modified alumina, alkali metal salt, transition metal salt, extruder, pore-forming agent and inorganic strong acid glue solvent is adopted to obtain a wall-flow sulfur trapping catalyst through high-pressure vacuum extrusion molding, and the After high temperature calcination, a wall-flow integrated extrusion-forming sulfur trapping catalyst is formed, which is placed upstream of the post-treatment catalyst to trap gaseous sulfides.
It realizes efficient capture of gaseous sulfides, avoids downstream catalysts from being contaminated by sulfur, improves the high temperature stability and sulfur capacity of the catalyst, can work efficiently in high humidity and heat application scenarios, and realizes the reuse of the catalyst through a high-temperature regeneration scheme.
Smart Images

Figure CN116832856B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diesel engine post-treatment catalysts, and in particular relates to a sulfur capture catalyst for a diesel engine and a preparation method thereof. Background Art
[0002] Diesel engines have high fuel economy, good power, and a wide power range. They are the main power source for commercial vehicles, construction machinery, power generation equipment, ships, national defense equipment, and other fields, and are important products in my country's equipment manufacturing industry. In order to meet the increasingly stringent emission regulations, diesel engine exhaust is synergistically purified through post-treatment catalysts to achieve the purpose of reducing pollutant emissions. Since the implementation of the National VI emission regulations, diesel engine post-treatment catalysts have adopted the technical route of oxidation catalyst (DOC) + particulate filter (cDPF) + selective catalytic reduction (SCR) + ammonia slip catalyst (ASC) to meet the requirements of low temperature, high efficiency, high durability and full working condition coverage in the National VI stage. In order to ensure the efficient operation of the post-treatment catalyst, the National VI regulations require that the sulfur content of diesel must be less than 10ppm, and the sulfur content in the exhaust gas after combustion in the cylinder is 1~2ppm, but even at such a low sulfur content, long-term accumulation is bound to cause catalyst poisoning. Affected by regional differences, the use of non-compliant diesel has aggravated the occurrence of catalyst poisoning, and faulty parts caused by sulfur poisoning are common. In the future, in response to the National VII ultra-low emission requirements, catalysts such as close-coupled SCR (CC-SCR) and selective catalytic reduction filter (SDPF) are likely to be used in large quantities for diesel engine exhaust purification. However, as the SCR catalyst moves forward, the sulfur poisoning problem will become more prominent.
[0003] The National VI post-treatment catalysts for diesel engines mostly use metals such as Pt, Pd, and Cu as active species, and achieve the purpose of pollutant purification through efficient synergistic catalysis. However, the above-mentioned active metals have poor sulfur resistance. In the SO2 atmosphere, they are easily oxidized to form sulfates such as PtSO4, PdSO4, and CuSO4, causing irreversible deactivation of the catalyst. In addition, affected by the oxygen-rich and wet heat application conditions of diesel engines, sulfides are likely to cause corrosion to post-treatment stainless steel housings, engine cylinder heads and other components, generating composite sulfate ash such as FeSO4, ZnSO4, and CaSO4.
[0004] In order to prevent the occurrence of sulfur poisoning, one idea is to improve the catalyst's ability to resist sulfur poisoning by improving the catalyst formula. Patent CN115555039A proposes to use Cu, Zn, Mn, and Ni to replace precious metal active species (Pt, Pd) as cDPF active components to reduce the occurrence of cDPF catalyst sulfur poisoning. Patent CN114534776A proposes that DOC adopts a partition coating method to improve the sulfur resistance of DOC catalyst by dispersing Pt and three non-precious metal active components (Ti, W, Mo, Ce) in the front zone and the fourth active component (Cu, Fe, Zn) in the rear zone. The above patent introduces non-precious metal elements and rare earth elements and adopts a method of partially replacing precious metal active species to improve the catalyst's sulfur resistance to a certain extent, but the non-precious metal catalyst has poor redox activity and thermal stability, which easily causes tail emissions to exceed the standard. Another idea is to reduce the occurrence of post-treatment catalyst poisoning by optimizing the catalyst combination and the whole machine control strategy. Patent CN1234473A proposes a method to optimize the calibration strategy of gasoline engines, using a combination of sulfur capture catalysts and NOx storage catalysts to achieve the storage and release cycle requirements of NOx and sulfur oxides by controlling the air-fuel ratio. The sulfur capture catalyst is an oxide of alkaline earth metals and rare earth elements doped in Mg / Al. Patent CN111255551A proposes a high-power diesel engine pollutant emission reverse flow catalytic conversion device with a sulfur trap, which integrates a sulfur trap and a particulate filter, wherein the sulfur capture catalyst comprises a straight-through silicon carbide carrier and a Pt / Ag-SiO2 catalyst coated thereon. The above patents provide a reference idea for solving catalyst sulfur poisoning, but do not mention the preparation method of the sulfur capture catalyst, the capture efficiency, the catalyst sulfur capacity, and the regeneration scheme. Summary of the invention
[0005] The purpose of the present invention is to make up for the deficiencies of the prior art and to provide a sulfur capture catalyst for a diesel engine and a preparation method thereof.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for preparing a sulfur capture catalyst for a diesel engine comprises the following steps: uniformly mixing molecular sieve: modified alumina: alkali metal salt: transition metal salt: extrusion aid: pore former: inorganic strong acid peptizer: H2O in a mass percentage of 33-40%: 8-13%: 3-5%: 1.5-3%: 2-4.5%: 0.5-1%: 2-6%: 27.5-50% to obtain a catalyst slurry; extruding the catalyst slurry into shape, drying and calcining the sulphur capture catalyst.
[0008] Furthermore, the molecular sieve is a powder material, including but not limited to one or a combination of two of OFF, 4A, 5A, and 13X.
[0009] Furthermore, the molecular sieve is a combination of one or two of Ca type, K type, Na type, and Na / K type; the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve is ≤10:1, wherein Ca, K, Na, and Na / K cations are coordinated with the framework Al, and the molar ratio of alkali metal elements to Al elements is ≤0.85:1.
[0010] Furthermore, the modified alumina has a boehmite crystal structure, a grain size of ≤1 μm, an alumina content of ≥95%, and NO3 - Content ≤5%.
[0011] Furthermore, the alkali metal salt is a nitrate obtained by adding an alkali metal element to nitric acid, and the purity of the nitrate is ≥95%; the alkali metal element is one or a combination of two of Ca, Mg, and Ba.
[0012] Furthermore, the transition metal salt is a nitrate obtained by adding a transition metal element to nitric acid, and the purity of the nitrate is ≥95%; the transition metal element is a combination of one or two of Fe, Co, Ce, and Ni.
[0013] Furthermore, the extrusion aid is one or a combination of two or more of hydrophilic carboxymethyl cellulose, starch, glycerol, and hydroxyethyl cellulose, and the viscosity of the extrusion aid is 1500-3000 mPa.s.
[0014] Furthermore, the pore-forming agent is one or a combination of two or more of polyethylene glycol, carbon powder, and polyvinyl alcohol, and the degree of polymerization of the pore-forming agent is 4000-6000.
[0015] Furthermore, the inorganic strong acid peptizing agent is concentrated nitric acid, concentrated hydrochloric acid or a mixture of both.
[0016] The preparation method of the sulfur capture catalyst for diesel engine of the present invention comprises the following specific steps:
[0017] (1) Add molecular sieve, modified alumina, alkali metal salt, transition metal salt and extrusion aid into a mixer and continue dry mixing for 0.5-1h until uniform;
[0018] (2) adding an inorganic strong acid peptizing agent and H2O to the dry mix prepared in step (1) and wet mixing for 0.5-1h;
[0019] (3) After wet mixing in step (2), add a pore-forming agent and continue wet mixing for 1-1.5 hours to obtain a mud material, which is then put into a vacuum mud kneading machine and mixed 3-5 times under vacuum;
[0020] (4) placing the slurry prepared in step (3) into a high-pressure vacuum extruder for extrusion molding to obtain a blank, molding the blank with a mold, and then cutting it according to the required height to obtain a catalyst wet material;
[0021] (5) drying the catalyst wet material prepared in step (4) at 35-50° C. using a microwave to obtain a monolithic honeycomb ceramic catalyst;
[0022] (6) Asymmetrically plugging the inlet end face and the outlet end face of the monolithic honeycomb ceramic catalyst with a plugging material;
[0023] (7) The plugged integral honeycomb ceramic catalyst is calcined at 550-650° C. for 3-5 hours to obtain a wall-flow integral extrusion-molded sulfur capture catalyst.
[0024] Compared with the prior art, the method of the present invention has at least the following advantages:
[0025] (1) By preparing a high-capture wall-flow catalyst and placing it upstream of the post-treatment catalyst, the ultra-high specific surface area alkaline capture material can be used to capture gaseous / solid sulfides and avoid sulfur contamination of the downstream post-treatment catalyst.
[0026] (2) By coupling Ca-type, K-type, Na-type, Na / K-type OFF, 4A, 5A, 13X molecular sieve catalysts and alkaline oxides in a specific proportion, the sulfide is captured according to the reaction path of reaction → anchoring → capture. In addition, for ultra-low silicon-aluminum ratio molecular sieves, by adding transition metal elements, the doping effect of Ce or Fe or Co or Ni or bimetallic is fully utilized to increase the positive charge of Al atoms in the molecular sieve framework, reduce the Al-O electrostatic potential, increase the interaction between Al and adjacent framework O atoms, and form a stable Me(OH)2+-molecular sieve framework coordination structure, which effectively improves the stability of the framework Al, inhibits framework dealumination, and improves the high temperature stability of the catalyst.
[0027] (3) High sulfide capture wall-flow catalyst uses the porous effect of molecular sieve to achieve the maximum SO2 capture. At the same time, due to the semi-blocked pores at the outlet, the sulfate ash forms a terminal capture effect inside the catalyst. Through high-temperature calcination and high-pressure air gun purging, the sulfide desorption and sulfate ash removal effects can be met, achieving the purpose of reuse. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the capture principle of sulfur capture catalyst;
[0029] Figure 2 This is the XRD spectrum of the sulfur capture catalyst in Example 1 of the present invention;
[0030] Figure 3 It is a comparison chart of the sulfur capacity and the corresponding NOx conversion efficiency of the sulfur capture catalyst of Examples 1 to 5 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0031] The content of the present invention will be further described below in conjunction with the drawings and embodiments.
[0032] A method for preparing a sulfur trapping catalyst for a diesel engine, wherein the sulfur trapping catalyst is placed upstream of a post-treatment catalyst and is a wall-flow integrally extruded catalyst prepared by a wall-flow honeycomb ceramic carrier extrusion molding device. The wall-flow honeycomb ceramic carrier extrusion molding device is a prior art device.
[0033] The preparation method of the sulfur capture catalyst for diesel engine of the present invention is to mix molecular sieve: modified alumina: alkali metal salt: transition metal salt: extrusion aid: pore former: inorganic strong acid peptizer: H2O=33-40%: 8-13%: 3-5%: 1.5-3%: 2-4.5%: 0.5-1%: 2-6%: 27.5-50% by mass to obtain catalyst mud, extrude the catalyst mud into shape, dry and calcine to obtain the sulfur capture catalyst. The specific preparation method steps are as follows:
[0034] (1) Add molecular sieve, modified alumina, alkali metal salt, transition metal salt and extrusion aid into a mixer and continue dry mixing for 0.5-1h until uniform;
[0035] (2) adding an inorganic strong acid peptizing agent and H2O to the dry mix prepared in step (1) and wet mixing for 0.5-1h;
[0036] (3) After wet mixing in step (2), add a pore-forming agent and continue wet mixing for 1-1.5 hours to obtain a mud material, which is then put into a vacuum mud kneading machine and mixed 3-5 times under vacuum;
[0037] (4) placing the slurry prepared in step (3) into a high-pressure vacuum extruder for extrusion molding to obtain a blank, molding the blank with a mold, and then cutting it according to the required height to obtain a catalyst wet material;
[0038] (5) drying the catalyst wet material prepared in step (4) at 35-50° C. using a microwave to obtain a monolithic honeycomb ceramic catalyst;
[0039] (6) Use pore-blocking materials to asymmetrically block the inlet and outlet ends of the monolithic honeycomb ceramic catalyst. The so-called asymmetrical pore blocking means that if the inlet end is blocked, the corresponding outlet end will not be blocked; if the inlet end is not blocked, the corresponding outlet end must be blocked. The holes are not straight in and out, so that particulate matter, ash, and sulfate ash can be captured and not discharged into the air;
[0040] (7) The plugged integral honeycomb ceramic catalyst is calcined at 550-650° C. for 3-5 hours to obtain a wall-flow integral extrusion-molded sulfur capture catalyst.
[0041] In the above method, the molecular sieve is a powder material, including but not limited to a combination of one or two of OFF, 4A, 5A, and 13X, which are commonly used materials in the industry and can be purchased commercially. The molecular sieve is a combination of one or two of Ca type, K type, Na type, and Na / K type; the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve, i.e., the silicon-aluminum molar ratio is ≤10:1, wherein the Ca, K, Na, and Na / K elements are coordinated with the framework Al in the form of hydroxyl groups, and the molar ratio of alkali metal elements to Al elements is ≤0.85:1.
[0042] The hydrated alumina has a boehmite crystal structure, a grain size of ≤1 μm, an alumina content of ≥95%, and a NO3- content of ≤5%.
[0043] The alkali metal salt is a nitrate obtained by adding an alkali metal element to nitric acid, and the purity of the nitrate is ≥95%; the alkali metal element is one or a combination of two of Ca, Mg and Ba.
[0044] The transition metal salt is a nitrate obtained by adding a transition metal element to nitric acid, and the purity of the nitrate is ≥95%; the transition metal element is one or a combination of two of Fe, Co, Ce and Ni.
[0045] The extrusion aid is one or a combination of two or more of hydrophilic carboxymethyl cellulose, starch, glycerol, and hydroxyethyl cellulose, and these materials are all commercially available. The viscosity of the extrusion aid is 1500-3000 mPa.s.
[0046] The pore-forming agent is one or a combination of two or more of polyethylene glycol, carbon powder and polyvinyl alcohol, and these materials are all commercially available. The polymerization degree of the pore-forming agent is 4000-6000.
[0047] The inorganic strong acid peptizing agent is concentrated nitric acid, concentrated hydrochloric acid or a mixture of the two.
[0048] Figure 1 The figure shows the capture principle of sulfur capture catalyst. Figure 1 As shown, the inlet and outlet ends of the extruded honeycomb ceramic catalyst 4 are asymmetrically blocked with a plugging material 3. After the sulfur-containing gas (SO2 / SO3 gas) 2 passes through the porous sulfur capture catalyst, it undergoes a redox reaction with cations such as Na, K, Ca, and alkaline oxides in the catalyst, generating sulfate species 5 in the honeycomb pores of the catalyst. In addition, after the sulfate substance 1 in the sulfur-containing gas passes through the sulfur capture catalyst, it cannot pass through the plug 3 or the sulfur capture catalyst, and is captured in the integral honeycomb ceramic catalyst 4. Sulfide travels and is captured according to the reaction path 6 of reaction → anchoring → capture, and sulfur-free tail gas 7 is discharged.
[0049] The sulfur capture catalyst of the present invention can withstand high humidity and heat application scenarios of diesel engines, can efficiently capture SO2 and sulfates during vehicle operation, and can reach a sulfur capacity of 180-300g / cat, effectively preventing sulfur oxides from polluting post-treatment catalysts in different application scenarios. After the sulfur capture catalyst reaches the maximum sulfur capacity, it can be disassembled for high-temperature regeneration at 450-700°C for 1-1.5h, and a 450-600kPa portable air compressor is used for sulfate ash cleaning, and the catalyst can be reused.
[0050] The mixer, vacuum clay kneading machine, high-pressure vacuum extruder, drying and calcining kiln equipment used in the method of the present invention are all existing technical equipment.
[0051] Example 1
[0052] Add NaK / OFF (silicon-aluminum molar ratio = 7): modified alumina (wt% Al2O3 = 95%, wt% NO3- = 5%): Ba(NO3)2: Ce(NO3)3: hydroxyethyl cellulose = 33%: 10%: 5%: 2.5%: 2.5% to the mixer, and continue dry mixing until uniform. Add concentrated nitric acid solution (concentration 63%): H2O = 2%: 44.5% to the dry mix evenly and slowly into the mixer, and wet mix for 1 hour. After the wet material is mixed evenly, add 0.5% polyethylene glycol (polymerization degree 6000), continue wet mixing for 1.5 hours, and then put the mud into a vacuum mud kneading machine for mud kneading, vacuum mixing 3 times. The kneaded mud is placed in a high-pressure vacuum extruder for extrusion molding to obtain a blank, the blank is molded with a mold, and then cut into the required height to obtain a catalyst wet material, and the catalyst wet material is microwave-dried at 35°C for 8 hours to obtain a monolithic honeycomb ceramic catalyst. The inlet and outlet ends of the monolithic honeycomb ceramic catalyst were asymmetrically blocked with a blocking material and then calcined at 650° C. for 3 h to obtain a wall-flow integrally extruded sulfur capture catalyst, which was recorded as “Sample 1”.
[0053] Example 2
[0054] In the mixer, Na / 4A (silicon-aluminum molar ratio = 2): modified alumina (wt% Al2O3 = 96%, wt% NO3- = 4%): Mg(NO3)2: Ce(NO3)4: carboxymethyl cellulose = 38%: 8%: 3%: 1.0%: 2% are continuously dry mixed until uniform. Hydrochloric acid solution (concentration 38%): H2O = 3%: 44% is evenly and slowly added to the mixer, and wet mixed for 0.5h. After the wet material is mixed evenly, 1% polyvinyl alcohol (degree of polymerization 3000) is added, and wet mixed for 0.5h, the mud is put into a vacuum mud kneading machine for mud kneading, and vacuum kneading is performed 5 times. The kneaded mud is placed in a high-pressure vacuum extruder for extrusion molding to obtain a blank, the blank is molded with a mold, and then cut into the required height to obtain a catalyst wet material, and the catalyst wet material is microwave-dried and dried at 50°C for 5h to obtain a monolithic honeycomb ceramic catalyst. The inlet and outlet ends of the monolithic honeycomb ceramic catalyst were asymmetrically blocked with a blocking material and then calcined at 550° C. for 5 h to obtain a wall-flow integrally extruded sulfur capture catalyst, which was recorded as “Sample 2”.
[0055] Example 3
[0056] In the mixer, continue to dry mix until uniform according to the ratio of Na / Ca-13X (silicon-aluminum molar ratio = 5): modified alumina (wt% Al2O3 = 97.5%, wt% NO3- = 2.5%): Ca(NO3)2: Fe(NO3)4: starch = 34%: 9%: 3.75%: 2.5%: 1%. Add concentrated hydrochloric acid solution (concentration 36%): H2O = 2%: 47% to the dry mix evenly and slowly into the mixer, and wet mix for 0.5h. After the wet material is mixed evenly, add 0.75% polyethylene glycol (degree of polymerization 3000), continue wet mixing for 0.5h, and then put the mud into the vacuum mud kneading machine for mud kneading, and vacuum mix 4 times. The prepared clay was put into a high-pressure vacuum extruder for extrusion molding to obtain a blank, which was molded with a mold and then cut into the required height to obtain a catalyst wet material, which was microwave-dried at 60°C for 6 hours to obtain a monolithic honeycomb ceramic catalyst. The inlet and outlet ends of the monolithic honeycomb ceramic catalyst were asymmetrically plugged with a plugging material and then calcined at 550°C for 4 hours to obtain a wall-flow integral extrusion molding sulfur capture catalyst, which was recorded as "Sample 3".
[0057] Example 4
[0058] In the mixer, according to the ratio of Ca / 5A (silicon-aluminum molar ratio = 3): modified alumina (wt% Al2O3 = 99%, wt% NO3- = 1%): Ca(NO3)2: Co(NO3)4: field sesbania powder = 36%: 10%: 3%: 2%: 2%, continue to dry mix until uniform. In the dry mix, according to the ratio of concentrated nitric acid solution (concentration 63%): H2O = 2%: 44.75%, add it to the mixer evenly and slowly, and wet mix for 0.5h. After the wet material is mixed evenly, 0.25% polyvinyl alcohol (polymerization degree 4000) is added, and after continuous wet mixing for 2h, the mud is put into a vacuum mud machine for mud training, and vacuum mixing is performed 4 times. The trained mud is placed in a high-pressure vacuum extruder for extrusion molding to obtain a blank, the blank is molded with a mold, and then cut into the required height to obtain a catalyst wet material, and the catalyst wet material is microwave-dried at 70°C for 4.5h to obtain a monolithic honeycomb ceramic catalyst. The inlet and outlet ends of the monolithic honeycomb ceramic catalyst were asymmetrically blocked with a blocking material and then calcined at 550° C. for 4.5 h to obtain a wall-flow integrally extruded sulfur capture catalyst, which was recorded as “Sample 4”.
[0059] Example 5
[0060] In the mixer, continue to dry mix until uniform according to the ratio of Ca / 5A (silicon aluminum molar ratio = 3): Na / OFF (silicon aluminum molar ratio = 5): modified alumina (wt% Al2O3 = 95%, wt% NO3- = 5%): Ca(NO3)2: Ni(NO3)2: field sesbania powder = 14%: 24%: 11%: 4%: 1.5%: 2%. Add concentrated nitric acid solution (concentration 63%): concentrated hydrochloric acid: H2O = 1.5%: 0.5%: 41% to the dry mix evenly and slowly into the mixer, and wet mix for 0.5h. After the wet material is mixed evenly, add 0.5% polyethylene glycol (polymerization degree 4000), continue wet mixing for 2h, and then put the mud into the vacuum mud kneading machine for mud kneading, and vacuum mix 4 times. The prepared clay was put into a high-pressure vacuum extruder for extrusion molding to obtain a blank, which was molded with a mold and then cut into the required height to obtain a catalyst wet material, which was microwave-dried at 70°C for 4.5 hours to obtain a monolithic honeycomb ceramic catalyst. The inlet and outlet ends of the monolithic honeycomb ceramic catalyst were asymmetrically plugged with a plugging material and then calcined at 550°C for 4.5 hours to obtain a wall-flow integral extrusion molding sulfur capture catalyst, which was recorded as "Sample 5".
[0061] Comparative Example 1
[0062] The sulfur capture catalyst was prepared according to the sulfur capture catalyst preparation method of CN1234473A.
[0063] Weigh 500g of γ-Al2O3 and dissolve it in deionized water. After stirring evenly, add 1182g of MgO to the suspension. After stirring for 30min, add 1150g of Al2O3 powder. After the suspension is stirred evenly, pre-calcine at 550℃ for 4 hours. Using the impregnation method, the above dispersion is impregnated on a cordierite carrier with a honeycomb structure according to a loading amount of 170g / L, dried at 120℃, and calcined at 500℃ for 2h. The coated honeycomb ceramic is impregnated in tetraammine platinum nitrate, dried, and calcined in air at 500℃ for 2h to obtain a sulfur capture catalyst, which is recorded as "Sample 6".
[0064] After the above samples 1 to 6 were completely packaged and weighed, they were installed on a National VI 4L diesel engine test bench, where the sulfur trap was placed 10 cm in front of the DOC. The test bench used fuels with different sulfur contents of 2000ppm, 1500ppm, 350ppm, 50ppm, and 10ppm. The sulfur trap catalyst was placed upstream of the National VI post-treatment catalyst. According to the requirements of the "Heavy Duty Diesel Vehicle Pollutant Emission Limits and Measurement Methods (China Phase VI)" (GB 17691-2018), the WHTC cycle test was carried out. The exhaust gas at the rear end of the ASC was connected to an analyzer to collect the concentration of SO2 and other gaseous pollutants. When the SO2 concentration exceeded 20ppm, the engine was stopped, the sulfur trap was removed, and the engine was kept at 100℃ in an oven for 30min before weighing.
[0065] Remove the post-treatment catalyst, use National VI standard 0# diesel, connect the tail pipe to the analyzer, and follow the requirements of "Emission Limits and Measurement Methods of Pollutants for Heavy-Duty Diesel Vehicles (China Phase VI)" (GB 17691-2018). After the WHTC-H cycle test, perform weighted calculation of source NOx emissions (g / kWh) in accordance with regulatory requirements.
[0066] After the source emission test, the post-treatment catalyst is installed, and the National VI standard 0# diesel is used. The analyzer is connected to the tail pipe at the rear end of the ASC catalyst. According to the requirements of the "Emission Limits and Measurement Methods of Pollutants for Heavy-Duty Diesel Vehicles (China Phase VI)" (GB17691-2018), after the WHTC-H cycle condition test hot cycle test is completed, the weighted calculation of tail NOx emissions (g / kWh) is carried out in accordance with the regulations.
[0067] The catalysts obtained in Examples 1 to 5 and Comparative Example 1 were subjected to cycle emission tests and sulfur capacity calculations, respectively, and the specific methods are as follows:
[0068] 1) The catalyst sulfur capacity is calculated according to the following formula:
[0069] .
[0070] Wherein, m1 represents the mass after sulfur accumulation (g), m0 represents the initial mass of the catalyst (g), and V represents the volume of the sulfur capture catalyst (L);
[0071] 2) The NOx conversion efficiency of the catalyst is calculated according to the following formula:
[0072] .
[0073] Among them, NOx tail emission and NOx source emission respectively represent the engine tail emission and source emission NOx emissions (g / kWh) under the WHTC-H cycle.
[0074] Figure 2 The XRD result of the sulfur capture catalyst prepared in Example 1 of the present invention shows that the sulfur capture catalyst prepared in Example 1 has a typical hexagonal alkaline OFF diffraction peak, and no Ba and Ce metal species are detected, which indicates that the Ba and Ce metal species are highly dispersed in the OFF crystal, or the XRD detection limit is not reached. The OFF pore size is 7Å×7Å, with 12 circular rings and barrier-free macropores, which provide abundant reaction sites for SO2, SO3 to react with framework cations Na+, K+, and alkaline oxides, thereby improving the sulfide capture efficiency.
[0075] Figure 3 The NOx conversion efficiency and sulfur capacity of the catalysts in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 1 of the present invention are shown in Table 1. Figure 1 By comparison, it can be seen that by placing an efficient sulfur capture catalyst device upstream of the catalyst, the catalyst uses a large-pore molecular sieve as a carrier, and alkaline earth metals and transition metals as active ingredients. The catalyst sulfur capacity can be as high as 180-300g / cat, with a long service life, and can efficiently capture SO2 and sulfate species, effectively preventing sulfur oxides from polluting post-treatment catalysts in different application scenarios. The use of Na-type, Ca-type, K-type, Na / K-type OFF, 4A, 5A, and 13X porous molecular sieve materials can efficiently utilize large-pore molecular sieve channels and active single sites, double sites, and triple sites to combine sulfur oxides to achieve the purpose of capturing sulfur oxides. The catalyst sulfur capacity of Comparative Example 1 can only reach about 100g / cat.
[0076] The above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments identical or equivalent to the contents of the present invention obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a sulfur capture catalyst for a diesel engine, characterized in that: The molecular sieve: modified alumina: alkali metal salt: transition metal salt: extrusion aid: pore former: inorganic strong acid peptizer: H2O=33-40%: 8-13%: 3-5%: 1.5-3%: 2-4.5%: 0.5-1%: 2-6%: 27.5-50% are mixed uniformly in mass percentage to obtain a catalyst slurry, and the catalyst slurry is extruded into shape, dried, and calcined to obtain a sulfur capture catalyst; the molecular sieve is a combination of one or two of the following: Ca type, K type, Na type, and Na / K type; the molar ratio of silicon dioxide to alumina in the molecular sieve is ≤10:1, wherein Ca, K, Na, and Na / K cations are coordinated with the framework Al, and the molar ratio of alkali metal elements to Al elements is ≤0.85:1; the alkali metal salt is a nitrate obtained by adding an alkali metal element to nitric acid; and the transition metal salt is a nitrate obtained by adding a transition metal element to nitric acid.
2. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The molecular sieve is a powder material, including but not limited to one or a combination of two of OFF, 4A, 5A, and 13X.
3. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The modified alumina has a boehmite crystal structure, a grain size of ≤1 μm, an alumina content of ≥95wt%, and NO3 - Content ≤5wt%.
4. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The purity of the nitrate is ≥95%; the alkali metal element is one or a combination of two of Ca, Mg and Ba.
5. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The purity of the nitrate is ≥95%; the transition metal element is one or a combination of two of Fe, Co, Ce and Ni.
6. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The extrusion aid is one or a combination of two or more of hydrophilic carboxymethyl cellulose, starch, glycerol and hydroxyethyl cellulose, and the viscosity of the extrusion aid is 1500-3000 mPa·s.
7. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The pore-forming agent is one or a combination of two or more of polyethylene glycol, carbon powder and polyvinyl alcohol, and the polymerization degree of the pore-forming agent is 4000-6000.
8. The method for preparing a sulfur capture catalyst for a diesel engine according to claim 1, characterized in that: The inorganic strong acid peptizing agent is concentrated nitric acid, concentrated hydrochloric acid or a mixture of the two.
9. The method for preparing a sulfur capture catalyst for a diesel engine according to any one of claims 1 to 8, characterized in that: The preparation steps are as follows: (1) Add molecular sieve, modified alumina, alkali metal salt, transition metal salt and extrusion aid into a mixer and continue dry mixing for 0.5-1h until uniform; (2) adding an inorganic strong acid peptizing agent and H2O to the dry mix prepared in step (1) and wet mixing for 0.5-1h; (3) After wet mixing in step (2), add a pore-forming agent and continue wet mixing for 1-1.5 hours to obtain a mud material, which is then put into a vacuum mud kneading machine and mixed 3-5 times under vacuum; (4) placing the slurry prepared in step (3) into a high-pressure vacuum extruder for extrusion molding to obtain a blank, molding the blank with a mold, and then cutting it according to the required height to obtain a catalyst wet material; (5) drying the catalyst wet material prepared in step (4) at 35-50° C. using a microwave to obtain a monolithic honeycomb ceramic catalyst; (6) Asymmetrically plugging the inlet end face and the outlet end face of the monolithic honeycomb ceramic catalyst with a plugging material; (7) The plugged integral honeycomb ceramic catalyst is calcined at 550-650° C. for 3-5 hours to obtain a wall-flow integral extrusion-molded sulfur capture catalyst.