A method for preparing a flexible graphene thermally conductive film

By introducing a cross-linking agent and controlling the heat treatment process in the preparation of the graphene thermally conductive film, the problem of expansion of the graphene thermally conductive film during heat treatment is solved, the preparation of a flexible graphene thermally conductive film with high toughness and high thermal conductivity is achieved, and the process is simplified process and reduce production costs.

CN116835984BActive Publication Date: 2024-10-25TAN KAH KEE INNOVATION LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310840237.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-10-25
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

The existing graphene thermally conductive film is gradually reduced due to the oxygen-containing functional groups during the heat treatment process, and the release of gas causes severe expansion, which limits large-scale coil production and increases production costs and resource waste.

Method used

By dispersing graphene oxide in a solvent and mixing it with a cross-linking agent, a graphene oxide slurry is formed. After coating to form a film, preheating, carbonization and graphitization are performed, and the temperature rise curve is controlled during the pressing process to fix the sheet. Reduce expansion and simplify the process.

Benefits of technology

The toughness and thermal conductivity of graphene thermal conductive film are improved, large-scale coil production is realized, production costs are reduced, and waste and complicated processes caused by hole making and toughening treatment are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004330809470000011
    Figure HDA0004330809470000011
  • Figure HDA0004330809470000012
    Figure HDA0004330809470000012
Patent Text Reader

Abstract

The present invention provides a method for preparing a flexible graphene thermal conductive film, comprising: A) dispersing graphene oxide in a solvent to obtain a graphene oxide dispersion; B) mixing the graphene oxide dispersion with a cross-linking agent to react to obtain a graphene oxide slurry; C) coating the graphene oxide slurry on a substrate, drying to form a film, and then separating the film from the substrate to obtain a graphene oxide film; D) preheating the graphene oxide film; E) carbonizing the film obtained in step D) under a protective atmosphere; F) graphitizing the film obtained in step E) under a protective atmosphere; G) pressing the film obtained in step F) to obtain a flexible graphene thermal conductive film. The method provided by the present invention not only simplifies the process, but also improves the toughness and thermal conductivity of the graphene thermal conductive film, and achieves large-scale winding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermally conductive films, and in particular to a method for preparing a flexible graphene thermally conductive film. Background Art

[0002] Graphene is a carbon atom in the form of sp 2 The two-dimensional carbon nanomaterial composed of hexagonal honeycomb lattices of hybrid orbitals has a theoretical thermal conductivity of 5300 W / (m·K) -1 ,, is one of the best thermally conductive materials known so far. Based on this characteristic, graphene thermal conductive film is widely used in thermal conduction and heat dissipation fields such as mobile phones, computers, 5G base stations, and military industry.

[0003] Graphene thermal conductive film usually uses graphene oxide as a precursor, and is prepared into graphene thermal conductive film through coating, carbonization, graphitization, pressing and other processes. While retaining the original hexagonal structure of graphene, graphene oxide contains a large number of functional groups such as hydroxyl, carboxyl, and epoxy groups on the surface and edges. These functional groups enable graphene oxide to maintain good dispersibility in solvents such as water, ethanol, and DMF, and improve its self-assembly performance in solvents, which is conducive to film formation.

[0004] The graphene oxide film produced by the existing process is stacked together by self-assembly layers, and the layers are attracted by van der Waals forces. During the heat treatment process, the oxygen-containing functional groups will be gradually reduced and release a large amount of gas, causing the graphene film to expand violently, resulting in cracking or even bursting during the coil preparation process, causing waste. Therefore, the existing graphene thermal conductive film products can only be produced in the form of small-scale coils or sheets, and it is difficult to achieve large-scale coil production. This will greatly limit the production efficiency of enterprises, cause waste of resources, and increase production costs, which is not conducive to the development of the industry.

[0005] Patent CN 115072709 A provides a method for preparing a large-scale graphene thermal conductive film coil, which is obtained by subjecting the graphene oxide film to pore-forming and toughening treatments and then rolling it up to obtain a porous graphene oxide film coil. The graphene thermal conductive film realizes batch preparation in the form of coils, which greatly improves the overall industrial production efficiency. However, this method adds two processes, pore-forming and toughening treatment, which is not only cumbersome, but also causes waste of raw materials due to pore-forming and reduces the strength of the film. Summary of the invention

[0006] In view of this, the present invention provides a method for preparing a flexible graphene thermally conductive film. The method provided by the present invention not only simplifies the process, but also improves the toughness and thermal conductivity of the graphene thermally conductive film.

[0007] The present invention provides a method for preparing a flexible graphene thermally conductive film, comprising the following steps:

[0008] A) dispersing graphene oxide in a solvent to obtain a graphene oxide dispersion;

[0009] B) mixing the graphene oxide dispersion with a cross-linking agent to obtain a graphene oxide slurry;

[0010] C) coating the graphene oxide slurry on a substrate, drying to form a film, and then separating the film from the substrate to obtain a graphene oxide film;

[0011] D) preheating the graphene oxide film;

[0012] E) carbonizing the film obtained in step D) under a protective atmosphere;

[0013] F) graphitizing the film obtained in step E) under a protective atmosphere;

[0014] G) Pressing the film obtained in step F) to obtain a flexible graphene thermally conductive film.

[0015] Preferably, in step B), the crosslinking agent is at least one of polycarbodiimide, isocyanate curing agent, aziridine crosslinking agent, silicone crosslinking agent, polyethylene glycol, citric acid, glutaric acid, cellulose acetate, hydroxypropyl methylcellulose, hydroxyethyl cellulose, acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide and diacetone acrylamide.

[0016] Preferably, the amount of the cross-linking agent used in step B) is 0.1% to 50% of the mass of the graphene oxide in step A).

[0017] Preferably, in step D), the preheating treatment is carried out at a temperature of 200 to 300° C. for a time of 6 to 18 hours.

[0018] Preferably, in step E), the carbonization treatment is carried out at a temperature of 800 to 1500° C. and for a time of 60 to 240 min.

[0019] Preferably, in step F), the graphitization treatment is carried out by first heating the temperature to 1000-1200° C. at a high speed, then heating the temperature to 2600-3100° C. at a low speed and keeping the temperature;

[0020] The heating rate of the high-speed heating is 20-30°C / min; the heating rate of the low-speed heating is 5-8°C / min.

[0021] Preferably, in step F), the insulation time is 2 to 4 hours.

[0022] Preferably, in step G), the pressure of the pressing treatment is 40 to 120 MPa, and the holding time is 1 to 6 hours.

[0023] Preferably, in step A), the concentration of the graphene oxide dispersion is 1 to 60 mg / mL;

[0024] In step C), the drying temperature is 40-90°C.

[0025] Preferably, in step B), the coating thickness is 4 to 7 mm;

[0026] In step D), the preheating treatment is vacuum heat treatment;

[0027] In step E), the heating rate of the carbonization treatment is 3-8°C / min.

[0028] The preparation method of the flexible graphene thermal conductive film provided by the present invention is to first disperse graphene oxide in a solvent to prepare a graphene oxide dispersion, then introduce and add a cross-linking agent to mix and react, and obtain a graphene oxide slurry; afterwards, the graphene oxide slurry is coated on a substrate and dried to form a film; then, a series of heat treatments are performed on the film, including preheat treatment, carbonization treatment and graphitization treatment; finally, it is pressed to obtain a flexible graphene thermal conductive film. Wherein, a specific cross-linking agent is introduced in the process of preparing the slurry, which reacts with the oxygen-containing functional groups (hydroxyl, carboxyl and epoxy groups) on the graphene oxide, and each sheet of graphene oxide is connected by a cross-linking agent. The heating temperature during drying is used in the process of drying and forming the film, and the reaction is self-cross-linked, so that the graphene oxide is more closely connected, and a fixing effect is played during the heat treatment process, reducing the expansion caused by the release of gas; and a specific heating curve is used during the heat treatment process to control the impurity release rate and stage in the thermal conductive film. The above two aspects work together to effectively improve the toughness and thermal conductivity of the graphene oxide film, facilitate the winding operation in the production process, and achieve large-scale coiling. In addition, the method of the present invention does not require special pore-making and toughening treatments, simplifies the process, and reduces production costs.

[0029] The test results show that the preparation method of the present invention enables the thermal conductivity of the graphene oxide thermal conductive film to be above 1405 W / mK and the tensile strength to be above 19 MPa, showing relatively high thermal conductivity and toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0031] Figure 1 This is a SEM image of the local interlayer crosslinking effect of the flexible graphene thermal conductive film obtained in Example 1;

[0032] Figure 2 This is a SEM image of the overall interlayer crosslinking effect of the flexible graphene thermal conductive film obtained in Example 1. DETAILED DESCRIPTION

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0034] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0035] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0036] Herein, when it comes to numerical ranges, unless otherwise specified, the numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0037] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 1-60 mg / mL means that the units of the left endpoint "1" and the right endpoint "60" are both mg / mL.

[0038] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0039] The present invention provides a method for preparing a flexible graphene thermally conductive film, comprising the following steps:

[0040] A) dispersing graphene oxide in a solvent to obtain a graphene oxide dispersion;

[0041] B) mixing the graphene oxide dispersion with a cross-linking agent to obtain a graphene oxide slurry;

[0042] C) coating the graphene oxide slurry on a substrate, drying to form a film, and then separating the film from the substrate to obtain a graphene oxide film;

[0043] D) preheating the graphene oxide film;

[0044] E) carbonizing the film obtained in step D) under a protective atmosphere;

[0045] F) graphitizing the film obtained in step E) under a protective atmosphere;

[0046] G) Pressing the film obtained in step F) to obtain a flexible graphene thermally conductive film.

[0047] About step A) :

[0048] A) dispersing graphene oxide in a solvent to obtain a graphene oxide dispersion.

[0049] In the present invention, the source of the graphene oxide is not particularly limited, and can be a conventional commercial product, such as conventional commercially available graphene oxide filter cake or graphene oxide. Graphene oxide itself has functional groups, including hydroxyl, carboxyl and epoxy groups.

[0050] In the present invention, the solvent includes but is not limited to at least one of water, DMF (N,N-dimethylformamide), NMP (N-methylpyrrolidone), ethanol and isopropanol.

[0051] The present invention has no special restrictions on the dispersion method, and the graphene oxide can be uniformly dispersed in the solvent according to the conventional dispersion method in the art. In the present invention, the amount of the graphene oxide and the solvent is preferably such that the concentration of the obtained graphene oxide dispersion reaches 1 to 60 mg / mL, specifically 1 mg / mL, 5 mg / mL, 10 mg / mL, 15 mg / mL, 20 mg / mL, 25 mg / mL, 30 mg / mL, 35 mg / mL, 40 mg / mL, 45 mg / mL, 50 mg / mL, 55 mg / mL, 60 mg / mL, more preferably 25 to 50 mg / mL.

[0052] About step B) :

[0053] B) mixing the graphene oxide dispersion with a cross-linking agent to obtain a graphene oxide slurry.

[0054] In the present invention, the crosslinking agent is preferably at least one of polycarbodiimide, isocyanate curing agent, aziridine crosslinking agent, silicone crosslinking agent, polyethylene glycol, citric acid, glutaric acid, cellulose acetate, hydroxypropyl methylcellulose, hydroxyethyl cellulose, acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide and diacetone acrylamide. Among them, the isocyanate curing agent is preferably at least one of water-based blocked isocyanate curing agent, isophorone diisocyanate and aliphatic isocyanate curing agent. The aziridine crosslinking agent is preferably at least one of aziridine, aziridine semi-blocked isocyanate crosslinking agent and aziridine modified isocyanate crosslinking agent. The silicone crosslinking agent is preferably at least one of water-based single-component silicone crosslinking agent and epoxy silane coupling agent. The polyethylene glycol is preferably polyethylene glycol with a number average molecular weight of less than 2000. If the molecular weight is too high, it is not conducive to coating and deteriorating film effect. In the present invention, the crosslinking agent is more preferably at least one of citric acid, acrylic acid and organosilicon crosslinking agent. The present invention introduces a crosslinking agent, which reacts with specific oxygen-containing functional groups on graphene oxide to connect the sheets and enhance the interlayer force, and can improve the toughness after film formation, improve the problem of severe expansion during heat treatment, and facilitate the winding operation during the production process.

[0055] In the present invention, the amount of the cross-linking agent is preferably 0.1% to 50% of the mass of the graphene oxide in step A), specifically 0.1%, 0.5%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%.

[0056] In the present invention, the method of mixing the graphene oxide dispersion with the crosslinking agent is preferably: first dispersed by a disperser, and then ultrasonically dispersed. Wherein, the dispersion rate of the disperser is preferably 2000-3000r / min, specifically 2000r / min, 2100r / min, 2200r / min, 2300r / min, 2400r / min, 2500r / min, 2600r / min, 2700r / min, 2800r / min, 2900r / min, 3000r / min. The dispersion time of the disperser is preferably 30-60min, specifically 30min, 35min, 40min, 45min, 50min, 55min, 60min. The power of the ultrasonic dispersion is preferably 720W. The ultrasonic dispersion time is preferably 30 to 120 min, specifically 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, or 120 min.

[0057] In the present invention, after the above mixing, preferably a homogenization degassing treatment is further performed. In the present invention, the method of the homogenization degassing treatment is not particularly limited and can be a conventional method in the art.

[0058] In the present invention, after the above-mentioned homogenization and degassing treatment, the reaction is continued to obtain graphene oxide slurry. In the present invention, the temperature of the reaction is preferably 60 to 120°C, specifically 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C. In the present invention, the reaction time is preferably 1 to 6h, specifically 1h, 2h, 3h, 4h, 5h, 6h. Graphene oxide itself has functional groups (including hydroxyl, carboxyl and epoxy groups). The present invention introduces the above-mentioned cross-linking agent, which will react and cross-link with the above-mentioned functional groups on the graphene oxide, so that the graphene oxide sheets are closely connected to each other, the interlayer interaction force is enhanced, and the film toughness is improved.

[0059] About step C) :

[0060] C) coating the graphene oxide slurry on a substrate, drying to form a film, and then separating the film from the substrate to obtain a graphene oxide thin film.

[0061] In the present invention, the substrate is preferably a PP (polypropylene) substrate, a PI (polyimide) substrate or a PET (polyethylene terephthalate) substrate. In the present invention, the coating method of the graphene oxide slurry on the substrate is not particularly limited, and can be a conventional coating method in the art, such as blade coating. In the present invention, the coating thickness is preferably 4 to 7 mm, specifically 4 mm, 5 mm, 6 mm, 7 mm.

[0062] In the present invention, after coating, drying is performed to form a film. In the present invention, the drying temperature is preferably 40 to 90°C, specifically 40°C, 50°C, 60°C, 70°C, 80°C, 90°C. In the above-mentioned drying film-forming process, the cross-linking agent and graphene oxide react and self-crosslink by utilizing the heating temperature during drying, so that the graphene oxide is more tightly connected. In the present invention, after the above-mentioned drying, the formed film is separated from the substrate to obtain a graphene oxide film.

[0063] About step D) :

[0064] D) preheating the graphene oxide film.

[0065] In the present invention, the preheating treatment is preferably vacuum heat treatment, that is, heat treatment under vacuum conditions.

[0066] In the present invention, the temperature of the preheat treatment is preferably 200-300°C, specifically 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C. In the present invention, the time of the preheat treatment is preferably 6-18h, specifically 6h, 8h, 10h, 12h, 14h, 16h, 18h. Through the above preheat treatment, the moisture and part of the additives in the film are first removed. Due to the cross-linking effect, the thermal conductive film has better toughness at this stage and can be made into a coil, and the expansion degree of the heat treatment is reduced compared to the sample without adding a cross-linking agent.

[0067] About step E) :

[0068] E) Carbonizing the film obtained in step D) under a protective atmosphere.

[0069] In the present invention, there is no particular limitation on the type of gas providing the protective atmosphere, and it can be any conventional protective gas in the art, such as nitrogen or argon.

[0070] In the present invention, the heating rate of the carbonization treatment is preferably 3-8°C / min, specifically 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min. The temperature of the carbonization treatment is preferably 800-1500°C, specifically 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C. In the present invention, the holding time of the carbonization treatment is preferably 60-240min, specifically 60min, 120min, 180min, 240min. Through the above-mentioned carbonization treatment, the present invention reduces some oxygen-containing functional groups on graphene oxide, releases oxygen in the form of CO2 and CO, and further increases the carbon content.

[0071] About step F) :

[0072] F) graphitizing the film obtained in step E) under a protective atmosphere.

[0073] In the present invention, there is no particular limitation on the type of gas providing the protective atmosphere, and it can be any conventional protective gas in the art, such as nitrogen or argon.

[0074] In the present invention, the graphitization treatment is preferably a gradient heating treatment, preferably as follows: first high-speed heating to 1000-1200°C, then low-speed heating to 2600-3100°C and heat preservation. Among them, the heating rate of the high-speed heating is preferably 20-30°C / min, specifically 20°C / min, 21°C / min, 22°C / min, 23°C / min, 24°C / min, 25°C / min, 26°C / min, 27°C / min, 28°C / min, 29°C / min, 30°C / min. The above-mentioned first-stage target temperature of 1000-1200°C can be specifically 1000°C, 1050°C, 1100°C, 1150°C, 1200°C. The heating rate of the low-speed heating is preferably 5-8°C / min, specifically 5°C / min, 6°C / min, 7°C / min, 8°C / min. The second stage target temperature of 2600-3100°C can be specifically 2600°C, 2700°C, 2800°C, 2900°C, 3000°C, 3100°C. The insulation time is preferably 2-4h, specifically 2h, 3h, 4h. Through the above graphitization treatment, oxygen and other impurities can be further removed, and graphitization occurs.

[0075] After the graphitization treatment, the temperature is preferably lowered to room temperature. After the temperature is lowered, a fluffy and porous graphene oxide film is obtained, which can be called a graphene foam film.

[0076] About step G) :

[0077] G) Pressing the film obtained in step F) to obtain a flexible graphene thermally conductive film.

[0078] In the present invention, the pressing treatment can be performed using a hydraulic press. The pressure of the pressing treatment is preferably 40 to 120 MPa, specifically 40 MPa, 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, 100 MPa, 110 MPa, 120 MPa. The holding time of the pressing treatment is preferably 1 to 6 hours, specifically 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours. After the above pressing treatment, a flexible graphene thermal conductive film product is obtained.

[0079] The preparation method of the flexible graphene thermal conductive film provided by the present invention is to first disperse graphene oxide in a solvent to prepare a graphene oxide dispersion, then introduce and add a cross-linking agent to mix and react, and obtain a graphene oxide slurry; afterwards, the graphene oxide slurry is coated on a substrate and dried to form a film; then, a series of heat treatments are performed on the film, including preheat treatment, carbonization treatment and graphitization treatment; finally, it is pressed to obtain a flexible graphene thermal conductive film. Wherein, a specific cross-linking agent is introduced in the process of preparing the slurry, which reacts with the oxygen-containing functional groups (hydroxyl, carboxyl and epoxy groups) on the graphene oxide, and each sheet of graphene oxide is connected by a cross-linking agent. The heating temperature during drying is used in the process of drying and forming the film, and the reaction is self-cross-linked, so that the graphene oxide is more closely connected, and a fixing effect is played during the heat treatment process, reducing the expansion caused by the release of gas; and a specific heating curve is used during the heat treatment process to control the impurity release rate and stage in the thermal conductive film. The above two aspects work together to effectively improve the toughness and thermal conductivity of the graphene oxide film, facilitate the winding operation in the production process, and achieve large-scale coiling. In addition, the method of the present invention does not require special pore-making and toughening treatments, simplifies the process, and reduces production costs.

[0080] The test results show that the preparation method of the present invention enables the thermal conductivity of the graphene oxide thermal conductive film to be above 1405 W / mK and the tensile strength to be above 19 MPa, showing higher thermal conductivity and toughness.

[0081] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0082] Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available or can be prepared by known methods. The instruments are all conventionally selected in the art. The experimental methods without specific conditions in the examples are carried out according to conventional conditions, such as the conditions described in the literature, books or the methods recommended by the manufacturer.

[0083] Example 1

[0084] A) Graphene oxide is dispersed in deionized water as a solvent to prepare a graphene oxide dispersion with a concentration of 40 mg / mL.

[0085] B) adding citric acid to the graphene oxide dispersion (the amount of citric acid is 1% of the amount of graphene oxide in step A), first dispersing it in a disperser at 2000 r / min for 60 min, then dispersing it in an ultrasonic disperser at 720 W for 30 min, then homogenizing and degassing, and reacting it at 80 ° C for 2 h to obtain a graphene oxide slurry.

[0086] C) The graphene oxide slurry was scraped onto the PP fiber cloth with a thickness of 5 mm, and the slurry was placed in an oven at 60° C. for 10 h. Then, the film was separated from the PP fiber cloth substrate to obtain a graphene oxide film.

[0087] D) The graphene oxide film was placed in a vacuum drying oven at 230° C. for 6 h.

[0088] E) In a nitrogen atmosphere, the temperature was raised to 1500°C at a rate of 30°C / min and maintained at that temperature for 1 h.

[0089] F) In an argon atmosphere, the temperature was first raised from room temperature to 2200°C at a high speed of 10°C / min, and then further raised to 3000°C at a low speed of 5°C / min, and kept at that temperature for 2 hours. Then, the temperature was cooled to room temperature to obtain a fluffy and porous graphene oxide film.

[0090] G) The graphene oxide film obtained in step F) is pressed by a hydraulic press at 50 MPa for 3 hours to obtain a flexible graphene thermal conductive film.

[0091] Characterization:

[0092] The interlayer structure of the obtained flexible graphene thermal conductive film was characterized by scanning electron microscopy. Figures 1-2 As shown, Figure 1 This is a SEM image of the local interlayer crosslinking effect of the flexible graphene thermal conductive film obtained in Example 1. Figure 2 This is a SEM image of the overall interlayer crosslinking effect of the flexible graphene thermal conductive film obtained in Example 1.

[0093] Example 2

[0094] A) Graphene oxide is dispersed in deionized water as a solvent to prepare a graphene oxide dispersion with a concentration of 40 mg / mL.

[0095] B) Adding acrylic acid to the graphene oxide dispersion (the amount of acrylic acid is 0.5% of the amount of graphene oxide in step A), first dispersing it in a disperser at 1800 r / min for 60 min, then dispersing it in an ultrasonic disperser at 720 W for 30 min, then homogenizing and degassing, and reacting it at 90° C. for 2 h to obtain a graphene oxide slurry.

[0096] C) The graphene oxide slurry was scraped onto the PP fiber cloth with a thickness of 5 mm, and the slurry was placed in an oven at 60° C. for 10 h. Then, the film was separated from the PP fiber cloth substrate to obtain a graphene oxide film.

[0097] D) The graphene oxide film was placed in a vacuum drying oven at 230° C. for 6 h.

[0098] E) In a nitrogen atmosphere, the temperature was raised to 1500°C at a rate of 30°C / min and maintained at that temperature for 1 h.

[0099] F) In an argon atmosphere, the temperature was first raised from room temperature to 2400°C at a high speed of 15°C / min, and then further raised to 3100°C at a low speed of 5°C / min, and kept at that temperature for 2 hours. Then, the temperature was cooled to room temperature to obtain a fluffy and porous graphene oxide film.

[0100] G) The graphene oxide film obtained in step F) is pressed by a hydraulic press at 50 MPa for 3 hours to obtain a flexible graphene thermal conductive film.

[0101] Example 3

[0102] A) Graphene oxide is dispersed in deionized water as a solvent to prepare a graphene oxide dispersion with a concentration of 40 mg / mL.

[0103] B) Add an aqueous one-component silicone crosslinker to the graphene oxide dispersion (the amount of the silicone crosslinker is 0.1% of the amount of graphene oxide in step A), first disperse it in a disperser at 2000 r / min for 90 min, then disperse it in an ultrasonic disperser at 720 W for 20 min, then homogenize and degas, and react at room temperature (25° C.) for 1 h to obtain a graphene oxide slurry.

[0104] C) The graphene oxide slurry was scraped onto the PP fiber cloth with a thickness of 5 mm, and the slurry was placed in an oven at 45° C. for 10 h. Then, the film was separated from the PP fiber cloth substrate to obtain a graphene oxide film.

[0105] D) The graphene oxide film was placed in a vacuum drying oven at 230° C. for 6 h.

[0106] E) In a nitrogen atmosphere, the temperature was raised to 1500°C at 30°C / min and maintained at this temperature for 2 h.

[0107] F) In an argon atmosphere, the temperature was first raised from room temperature to 2200°C at a high speed of 15°C / min, and then further raised to 3100°C at a low speed of 5°C / min, and kept at that temperature for 2 hours. Then, the temperature was cooled to room temperature to obtain a fluffy and porous graphene oxide film.

[0108] G) The graphene oxide film obtained in step F) is pressed by a hydraulic press at 50 MPa for 3 hours to obtain a flexible graphene thermal conductive film.

[0109] Example 4

[0110] A) Graphene oxide is dispersed in deionized water as a solvent to prepare a graphene oxide dispersion with a concentration of 40 mg / mL.

[0111] B) adding an aqueous blocked isocyanate curing agent to the graphene oxide dispersion (the amount of the aqueous blocked isocyanate curing agent is 1% of the amount of graphene oxide in step A), first dispersing it in a disperser at 2000 r / min for 60 min, then dispersing it in an ultrasonic disperser at 720 W for 30 min, then homogenizing and degassing, and reacting it at 80 ° C for 2 h to obtain a graphene oxide slurry.

[0112] C) The graphene oxide slurry was scraped onto the PP fiber cloth with a thickness of 5 mm, and the slurry was placed in an oven and dried at 80° C. for 10 h. Then, the film was separated from the PP fiber cloth substrate to obtain a graphene oxide film.

[0113] D) The graphene oxide film was placed in a vacuum drying oven at 230° C. for 6 h.

[0114] E) In a nitrogen atmosphere, the temperature was raised to 1500°C at a rate of 30°C / min and maintained at that temperature for 1 h.

[0115] F) In an argon atmosphere, the temperature was first raised from room temperature to 2200°C at a high speed of 10°C / min, and then further raised to 3000°C at a low speed of 5°C / min, and kept at that temperature for 2 hours. Then, the temperature was cooled to room temperature to obtain a fluffy and porous graphene oxide film.

[0116] G) The graphene oxide film obtained in step F) is pressed by a hydraulic press at 50 MPa for 3 hours to obtain a flexible graphene thermal conductive film.

[0117] Comparative Example 1

[0118] A) Graphene oxide is dispersed in deionized water as a solvent to prepare a graphene oxide dispersion with a concentration of 40 mg / mL.

[0119] B) The graphene oxide slurry was scraped onto the PP fiber cloth with a thickness of 5 mm, and the slurry was placed in an oven at 60° C. for 10 h. Then, the film was separated from the PP fiber cloth substrate to obtain a graphene oxide film.

[0120] C) The graphene oxide film was placed in a vacuum drying oven at 230° C. for 6 h.

[0121] D) In ​​a nitrogen atmosphere, the temperature was raised to 1500°C at 30°C / min and maintained for 1 h.

[0122] E) In an argon atmosphere, the temperature was first raised from room temperature to 2200°C at a high speed of 15°C / min, and then further raised to 3000°C at a low speed of 5°C / min, and kept at that temperature for 2 hours. Then, the temperature was cooled to room temperature to obtain a fluffy and porous graphene oxide film.

[0123] F) The graphene oxide film obtained in step E) is pressed by a hydraulic press at 60 MPa for 3 h to obtain a flexible graphene thermal conductive film.

[0124] Comparative Example 2

[0125] The process is carried out in accordance with Example 1, except that in step E), the target temperature for heating is 700°C; in step F), the target temperature for the first stage is 800°C, and the target temperature for the second stage is 2400°C.

[0126] Comparative Example 3

[0127] The process is carried out in accordance with Example 1, except that in step E), the target temperature for heating is 1800°C; in step F), the target temperature for the first stage is 1400°C, and the target temperature for the second stage is 3000°C.

[0128] Comparative Example 4

[0129] The method was carried out in accordance with Example 1, except that the cross-linking agent citric acid in step B) was replaced by polyethylene glycol with a number average molecular weight of 2000.

[0130] Performance Test:

[0131] The graphene oxide thermal conductive films obtained in each embodiment and comparative example were subjected to various performance tests, and the results are shown in Table 1. Among them, the tensile strength test was tested with reference to the national standard GB / T 1040.1-2018 Test method for determining tensile properties of plastics.

[0132] Table 1: Properties of graphene oxide thermal conductive films obtained in various examples and comparative examples

[0133] Dry film thickness / μm <![CDATA[Density / (g / cm 3 )]]> Thermal conductivity / (W / mK) Tensile strength / MPa Example 1 191 2.08 1405.6 19 Example 2 168 2.11 1497.6 35 Example 3 172 2.07 1506.3 27 Example 4 164 2.15 1503.2 29 Comparative Example 1 247 1.97 1167.9 12 Comparative Example 2 251 2.03 1246.5 15 Comparative Example 3 223 2.07 1278.4 18 Comparative Example 4 201 2.07 1320.5 16

[0134] Note: Dry film thickness refers to the thickness of the wet film after drying, not the thickness of the final product.

[0135] It can be seen from the test results in Table 1 that the dry film thickness of the graphene oxide thermal conductive film obtained in Examples 1 to 4 of the present invention is below 191 μm (under the condition of 5 mm coating thickness), the thermal conductivity is above 1405 W / mK, and the tensile strength reaches above 19 MPa, showing a lower degree of thermal expansion, higher thermal conductivity and toughness. Compared with Example 1, the dry film thickness of Comparative Example 1 is significantly increased, and the thermal conductivity and tensile strength are significantly decreased. It is proved that the introduction of a cross-linking agent in the present invention can fix the sheet layer, inhibit the expansion during the heat treatment process, and is conducive to the orderly arrangement of the GO (lamellar two-dimensional structure) sheet layers, reduce the defects generated during the expansion process, and improve the thermal conductivity and strength of the thermal conductive film. Compared with Example 1, the thermal conductivity and tensile strength of Comparative Examples 2 to 3 are also reduced, which proves that the present invention adopts a specific heat treatment method, which is conducive to improving the thermal conductivity and strength of the thermal conductive film. Compared with Example 4, the dry film thickness of Comparative Example 4 is increased, and the thermal conductivity and tensile strength are also reduced, which proves that the use of a certain cross-linking agent in the present invention is conducive to film formation and improving the performance of the film product.

[0136] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for preparing a flexible graphene thermally conductive film, characterized in that: The following steps are involved: A) dispersing graphene oxide in a solvent to obtain a graphene oxide dispersion; the concentration of the graphene oxide dispersion is 1-60 mg / mL; B) mixing the graphene oxide dispersion with a cross-linking agent to react to obtain a graphene oxide slurry; the cross-linking agent is at least one of an isocyanate curing agent, an organosilicon cross-linking agent, and acrylic acid; the reaction temperature is 60-120° C.; the amount of the cross-linking agent is 0.1%-1% of the mass of the graphene oxide in step A); C) coating the graphene oxide slurry on a substrate, drying to form a film, and then separating the film from the substrate to obtain a graphene oxide film; D) preheating the graphene oxide film; the preheating temperature is 200-300° C. and the time is 6-18 h; E) carbonizing the film obtained in step D) under a protective atmosphere; F) graphitizing the film obtained in step E) under a protective atmosphere; the graphitization treatment is performed by firstly heating the film to 1000-1200° C. at a high speed, then heating the film to 2600-3100° C. at a low speed and keeping the temperature; The heating rate of the high-speed heating is 20-30 °C / min; the heating rate of the low-speed heating is 5-8 °C / min; G) Pressing the film obtained in step F) to obtain a flexible graphene thermal conductive film.

2. The preparation method according to claim 1, characterized in that: In step E), the carbonization treatment is carried out at a temperature of 800-1500° C. and for a time of 60-240 min.

3. The preparation method according to claim 1, characterized in that: In step F), the insulation time is 2 to 4 hours.

4. The preparation method according to claim 1, characterized in that: In step G), the pressure of the pressing treatment is 40-120 MPa, and the holding time is 1-6 h.

5. The preparation method according to claim 1, characterized in that: In step A) and step C), the drying temperature is 40-90°C.

6. The preparation method according to claim 1, characterized in that: In step B), the coating thickness is 4 to 7 mm; In step D), the preheating treatment is vacuum heat treatment; In step E), the heating rate of the carbonization treatment is 3-8 °C / min.