Exterior wall coating suitable for various substrates and preparation method thereof

Through the combination of two-group distribution formula and specific raw material ratio, the construction process of exterior wall coating is simplified, the problems of complex construction and poor adhesion in the existing technology are solved, and good adhesion and alkali resistance to various substrates are achieved. reduces construction costs and construction periods.

CN116836604BActive Publication Date: 2024-12-03CHINA PAINT MFG CO SHENZHEN
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310997319.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-09
Publication Date
2024-12-03
Estimated Expiration
2043-08-09

AI Technical Summary

Technical Problem

The construction process of existing exterior wall coatings is complex, time-consuming and costly, and it is difficult to meet the needs of different substrates, and it is not able to effectively achieve adhesion and alkali resistance requirements.

Method used

Using a two-combination distribution formula, including acrylic emulsion and silicate cement, a component A and B are formed by mixing specific raw material ratios and additives, and mixed at 600 rpm to prepare and use a variety of suitable products. Exterior wall coating for substrates simplifies construction process.

Benefits of technology

It achieves good adhesion and alkali resistance to various substrates, reduces construction processes, reduces costs, complies with the performance requirements of national standards, and does not require the use of interface agents or primers, which significantly shortens the construction period.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004385100960000051
    Figure BDA0004385100960000051
  • Figure BDA0004385100960000061
    Figure BDA0004385100960000061
  • Figure BDA0004385100960000062
    Figure BDA0004385100960000062
Patent Text Reader

Abstract

The invention relates to the field of building exterior wall coatings, and discloses an exterior wall coating suitable for various substrates and a preparation method thereof. The exterior wall coating prepared by the invention comprises an A component and a B component, wherein the A component comprises the following raw materials, by mass percentage: acrylic emulsion: 40-60%, titanium dioxide: 15-20%, kaolin: 1-3%, calcium carbonate: 8-12%, cellulose: 0.1-0.2%, film-forming aid: 2-4%, antifreeze agent: 1.5-2.5%, other aids: 1-4%, and the rest is water; the B component comprises 32.5 white silicate cement; the mass ratio of the A component to the B component is 7:3, and the exterior wall coating suitable for various substrates is obtained after the two are fully mixed; the exterior wall coating does not need to be used in conjunction with a primer or an interface agent, has good stability, adhesion, weather resistance, alkali resistance, and has a short construction period, simplifies the construction process of the exterior wall coating, and can effectively reduce the construction cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building exterior wall coatings and discloses an exterior wall coating suitable for various substrates and a preparation method thereof. Background Art

[0002] Exterior wall paint is a kind of paint used for exterior wall protection and decoration. It has functions such as waterproof, dustproof, weather-resistant, corrosion-resistant and wear-resistant. It can meet the needs of building exterior walls under different climatic and environmental conditions, improve the overall quality of the building, and effectively extend the service life of the building.

[0003] Exterior wall paint is directly exposed to the external environment, so the paint is required to be water-resistant, color-retaining, and aging-resistant, and at the same time, it needs to have good adhesion. Existing exterior wall paints are divided into the following categories: thin exterior wall paints, multi-layer pattern paints, colored sand paints, and thick paints.

[0004] Due to the different application scenarios of exterior wall coatings, the substrates used are also diverse, including putty substrates, concrete substrates, tile substrates, old paint substrates, etc. Different construction processes are required for different substrates. The general construction process in the prior art is: substrate leveling, puttying, primer construction, and topcoat construction. The process is complicated, time-consuming and labor-intensive, and the overall cost is high.

[0005] CN104073035A discloses an acrylic copolymer emulsion cement-based waterproof coating, specifically relates to an acrylic copolymer emulsion cement-based waterproof coating, and belongs to the technical field of coatings. The acrylic copolymer emulsion cement-based waterproof coating is prepared from the following raw materials in percentage by weight: 55-60% of silicate cement, 35-40% of acrylic emulsion, 2-3% of calcined kaolin, 2-3% of pentanediol, and 1-2% of nano calcium carbonate. It provides a waterproof function for the wall, does not meet the performance requirements of exterior wall paint, and needs to be coated with exterior wall decorative paint, which is more troublesome to construct.

[0006] CN107903740A discloses an environmentally friendly coating, comprising the following components in parts by weight: 2-4 parts of lemon oil, 2-4 parts of orange oil, 2-3 parts of titanium dioxide, 1-3 parts of carbon black, 6-12 parts of glyoxal, 1-4 parts of polyethylene glycol 200, 5-8 parts of n-butanol, 3-6 parts of methyl cellulose, 10-25 parts of filler, 15-30 parts of water, 25-50 parts of acrylic elastic emulsion, 5-8 parts of polycarboxylic acid-based high-performance water reducing agent, 6-13 parts of seaweed mud, 3-7 parts of titanium dioxide, and 40-70 parts of silicate cement. A variety of solvents are used in the coating, and the added amount is also relatively large. No more detailed information is disclosed, so it is difficult to determine whether the GB / T9755 standard for exterior wall paint is implemented.

[0007] Therefore, it is of great significance to study an exterior wall coating with simple process, good performance and applicable to a variety of substrates and its preparation method. Summary of the invention

[0008] The object of the present invention is to provide an exterior wall coating applicable to a variety of substrates and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0010] A method for preparing an exterior wall coating suitable for a variety of substrates comprises the following steps: S1: (1) taking acrylic emulsion, titanium dioxide, kaolin, calcium carbonate, cellulose, film-forming aid, antifreeze agent, other additives, and water, and mixing them uniformly to obtain component A; (2) taking silicate cement, which is named component B;

[0011] S2: Take component A and component B, mix them at a speed of 600 rpm for 5 to 10 minutes to obtain an exterior wall paint.

[0012] More optimally, a method for preparing an exterior wall coating suitable for a variety of substrates comprises the following steps: S1: (1) taking acrylic emulsion, titanium dioxide, kaolin, calcium carbonate, cellulose, film-forming aid, antifreeze agent, other additives, and water, and mixing them uniformly to obtain component A; (2) taking silicate cement, named component B;

[0013] S2: Take component A and component B, mix them at a speed of 600 rpm for 8 minutes to obtain an exterior wall paint.

[0014] More optimally, the mass ratio of component A to component B is 7:3.

[0015] More optimally, the component A includes the following raw materials, in percentage by mass: acrylic emulsion: 40-60%, titanium dioxide: 15-20%, kaolin: 1-3%, calcium carbonate: 8-12%, cellulose: 0.1-0.2%, film-forming aid: 2-4%, antifreeze agent: 1.5-2.5%, and other additives: 1-4%.

[0016] More optimally, the component A includes the following raw materials, in percentage by mass: acrylic emulsion: 50%, titanium dioxide: 18%, kaolin: 2%, calcium carbonate: 10%, cellulose: 0.15%, film-forming aid: 3.5%, antifreeze agent: 1.7%, and other additives: 1-4%.

[0017] More optimally, the other auxiliary agents include at least one of a dispersant, a wetting agent, a defoaming agent, a pH regulator, a polyurethane thickener, and a mildew preventer.

[0018] More optimally, the component A includes the following raw materials, in percentage by mass: acrylic emulsion: 40-60%, titanium dioxide: 15-20%, kaolin: 1-3%, calcium carbonate: 8-12%, cellulose: 0.1-0.2%, film-forming aid: 2-4%, antifreeze agent: 1.5-2.5%, dispersant 0.5-2%, wetting agent 0.1-0.5%, defoaming agent 0.1-0.5%, pH adjuster 0.2-0.5%, polyurethane thickener 0.05-0.2%, and mildewproofing agent 0.1-0.5%.

[0019] More optimally, the component A includes the following raw materials, in percentage by mass: acrylic emulsion: 50%, titanium dioxide: 18%, kaolin: 2%, calcium carbonate: 10%, cellulose: 0.15%, film-forming aid: 3.5%, antifreeze agent: 1.7%, dispersant 0.8%, wetting agent 0.2%, defoaming agent 0.2%, pH adjuster 0.25%, polyurethane thickener 0.1%, and mildew inhibitor 0.3%.

[0020] More optimally, in step S1, the specific preparation process of component A includes the following steps: take antifreeze agent, dispersant, wetting agent, and defoaming agent, add water in sequence, disperse at a speed of 1100-1300 rpm for 5-10 minutes, add titanium dioxide, kaolin, calcium carbonate, cellulose, and pH adjuster in sequence, maintain the speed of 1100-1300 rpm for 25-30 minutes, until the fineness is dispersed to ≤60 microns, add mildew inhibitor, preservative, acrylic emulsion, film-forming aid, and polyurethane thickener in sequence, maintain the speed of 900-1100 rpm for 10-15 minutes, and obtain component A.

[0021] More optimally, in step S1, the specific preparation process of component A includes the following steps: take antifreeze agent, dispersant, wetting agent, and defoaming agent, add water in sequence, disperse at a speed of 1200 rpm for 8 minutes, add titanium dioxide, kaolin, calcium carbonate, cellulose, and pH adjuster in sequence, maintain the speed of 1200 rpm for 28 minutes, until the fineness is dispersed to ≤60 microns, add mildew inhibitor, preservative, acrylic emulsion, film-forming aid, and polyurethane thickener in sequence, maintain stirring at a speed of 1000 rpm for 13 minutes, and obtain component A.

[0022] More optimally, the acrylic emulsion is a high-performance pure acrylic emulsion; the titanium dioxide is rutile titanium dioxide; and the kaolin is calcined kaolin.

[0023] More optimally, the calcium carbonate is heavy calcium carbonate; and the cellulose is hydroxyethyl cellulose ether.

[0024] More optimally, the film-forming aid is alcohol ester dodecasol; and the antifreeze agent is propylene glycol.

[0025] Preferably, the acrylic emulsion is a high-performance pure acrylic emulsion, specifically Dow TX-100; the titanium dioxide is rutile titanium dioxide, specifically Melilian Chemical Tiona 595; and the kaolin is calcined kaolin, specifically China Minerals Baixue 80.

[0026] Preferably, the calcium carbonate is heavy calcium carbonate, specifically CC-600 from Guangyuan Chemical; the cellulose is hydroxyethyl cellulose ether, specifically 250HBR from Ashland.

[0027] More optimally, the film-forming aid is alcohol ester dodecahydrate, the specific model is Eastman Texanol; the antifreeze agent is propylene glycol.

[0028] More optimally, the dispersant is Akzo Nobel 747; the wetting agent is Clariant X080; the defoaming agent is Blackburn CF1494; the pH adjuster is Dow AMP-95; the polyurethane thickener is Dow RM-2020NPR; the mildew inhibitor is Thor EPW; and the preservative is Thor RSC CONC.

[0029] More optimally, the silicate cement is 32.5 white silicate cement.

[0030] Optimally, the prepared exterior wall paint needs to be used within 5 hours to avoid curing.

[0031] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: (1) the exterior wall coating prepared by the present invention comprises component A and component B, wherein component A comprises the following raw materials, by mass percentage: acrylic emulsion: 40-60%, titanium dioxide: 15-20%, kaolin: 1-3%, calcium carbonate: 8-12%, cellulose: 0.1-0.2%, film-forming aid: 2-4%, antifreeze agent: 1.5-2.5%, other aids: 1-4%, and the rest is water; component B comprises 32.5 white silicate cement; the present invention designs the formula into a two-component formula, and adds silicate cement into the formula. The mass ratio of silicate cement (component B) to the other component (component A) is controlled to be 3:7, thereby improving the performance of the coating and its adhesion to various substrates; the other component (component A) uses pure acrylic emulsion with excellent compatibility with cement, which makes the entire coating have good stability. It has very good adhesion on substrates such as tiles, concrete, old paint, putty, etc., and is not easy to fall off. It also has excellent alkali resistance and prevents alkaline seepage from the wall. Therefore, compared with ordinary exterior wall coatings, there is no need to use interface agents, primers, and putty. It has better adhesion, weather resistance, and alkali resistance, which greatly shortens the construction period and reduces construction costs.

[0032] (2) The acrylic emulsion used in the present invention is a high-performance pure acrylic emulsion, which has excellent weather resistance, good adhesion to substrates such as concrete, tiles, masonry, and good compatibility with cement; the titanium dioxide used in the present invention is rutile titanium dioxide, which has excellent weather resistance, good hiding power, and stable color; the kaolin used in the present invention is calcined kaolin, which has the characteristics of good hiding power, good durability, and chemical corrosion resistance, and can also effectively reduce the gloss of the coating; the calcium carbonate used in the present invention is heavy calcium carbonate, which can be used in combination with kaolin to effectively reduce the gloss of the coating; the cellulose used in the present invention is hydroxyethyl cellulose ether, which has good viscosity stability and good water retention; the other additives used in the present invention are used in combination with the above raw materials in a certain proportion to obtain an exterior wall coating that is suitable for a variety of substrates and has good adhesion, good alkali resistance, good weather resistance, good stability, and is easy to construct.

[0033] (3) The other additives described in the present invention include dispersants, wetting agents, defoamers, pH regulators, polyurethane thickeners, and mildew inhibitors. The dispersant used in the present invention is Akzo Nobel 747; the wetting agent is Clariant X080; the defoamer is Blackburn CF1494; the pH regulator is Dow AMP-95; the polyurethane thickener is Dow RM-2020NPR; the mildew inhibitor is Thor EPW; and the preservative is Thor RSC CONC. These additives have the characteristics of small dosage and large effect. When used in a certain proportion, an exterior wall coating suitable for a variety of substrates with good adhesion, good alkali resistance, good weather resistance, good stability, and easy construction can be obtained. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The following examples include the following raw materials: acrylic emulsion (pure acrylic emulsion, Dow TX-100); titanium dioxide (Meililian Chemical Tiona 595); kaolin (China Mineral Baixue 80); calcium carbonate (Guangyuan Chemical CC-600); cellulose (Ashland 250HBR); film-forming aid (Eastman Texanol); antifreeze agent (propylene glycol, CAS: 57-55-6); dispersant (Akzo Nobel 747); wetting agent (Clariant X080); defoaming agent (Blackburn CF1494); pH adjuster (Dow AMP-95); polyurethane thickener (Dow RM-2020NPR); mildew inhibitor (Thor EPW); preservative (Thor RSC CONC);

[0036] The following parts are percentages by mass;

[0037] Embodiment 1:

[0038] Specific preparation steps:

[0039] S1: Prepare component A. For specific raw materials and steps, refer to Table 1;

[0040] S2: Take component A and component B, mix them at a speed of 600 rpm for 8 minutes to obtain an exterior wall paint.

[0041] Table 1:

[0042]

[0043] Embodiment 2:

[0044] Specific preparation steps:

[0045] S1: Prepare component A. For specific raw materials and steps, refer to Table 2;

[0046] S2: Take component A and component B, mix them at a speed of 600 rpm for 8 minutes to obtain an exterior wall paint.

[0047] Table 2:

[0048]

[0049] Comparative Example 1 (the amount of pure acrylic emulsion added is lower than the range requirement):

[0050] Specific preparation steps:

[0051] S1: Prepare component A. For specific raw materials and steps, refer to Table 3;

[0052] S2: Take component A and component B, mix them at a speed of 600 rpm for 8 minutes to obtain an exterior wall paint.

[0053] Table 3:

[0054]

[0055]

[0056] Test: Take the exterior wall paint obtained in Examples 1 to 2, the exterior wall paint prepared in Comparative Example 1, and the common exterior wall paint (Juhua brand advanced acrylic exterior wall paint), and test their key performance indicators. The specific conclusions are shown in Table 4;

[0057] Table 4:

[0058]

[0059]

[0060]

[0061] Conclusion: The amount of pure acrylic emulsion added to the exterior wall paint prepared in Comparative Example 1 is reduced, which does not meet the requirements defined in the present invention. Although it can also be directly constructed and is suitable for a variety of substrates, the amount of emulsion is too small, resulting in poor adhesion of the paint film and alkali efflorescence. When its resistance to salt and alkali efflorescence is tested with reference to the JG / T210-2018 exterior wall type I film-forming standard, it does not meet the standard; a common exterior wall paint commonly used on the market (Chrysanthemum brand advanced acrylic exterior wall paint) is selected for testing. When the exterior wall paint is used, an interface agent must be applied first, and then a primer and an exterior wall topcoat must be applied. If no interface agent and primer are applied, the adhesion is poor, alkali efflorescence is easy, and the construction is time-consuming. The washability, alkali resistance, water resistance, and artificial weathering resistance of the exterior wall paint are all below those of Examples 1 to 2. When its resistance to salt and alkali efflorescence is tested with reference to the JG / T210-2018 exterior wall type I film-forming standard, it does not meet the standard.

[0062] Therefore, the exterior wall coating prepared by the present invention meets national standards, and has good properties such as adhesion, alkali resistance, weather resistance, stability, etc. It can be directly constructed without interface agents, putties, primers, etc., and is suitable for a variety of substrates.

[0063] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0064] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An exterior wall coating suitable for a variety of substrates, characterized by: The exterior wall coating comprises component A and component B, wherein component A comprises the following raw materials, in percentage by mass: acrylic emulsion: 50%, titanium dioxide: 18%, kaolin: 2%, calcium carbonate: 10%, cellulose: 0.15%, film-forming aid: 3.5%, antifreeze agent: 1.7%, dispersant 0.8%, wetting agent 0.2%, defoamer 0.2%, pH regulator 0.25%, polyurethane thickener 0.1%, mildewproof agent 0.3%, preservative 0.15%; component B comprises silicate cement; the mass ratio of component A to component B is 7:3; The silicate cement is 32.5 white silicate cement; the dispersant is Akzo Nobel 747; the wetting agent is Clariant X080; the defoamer is Blackburn CF1494; the pH adjuster is Dow AMP-95; the polyurethane thickener is Dow RM-2020NPR; the mildew inhibitor is Thor EPW; the preservative is Thor RSC CONC; the acrylic emulsion is pure acrylic emulsion Dow TX-100; the titanium dioxide is rutile titanium dioxide; the kaolin is calcined kaolin; the calcium carbonate is heavy calcium carbonate; the cellulose is hydroxyethyl cellulose ether; The film-forming aid was Eastman Texanol; The antifreeze agent is propylene glycol; The method for preparing an exterior wall coating suitable for a variety of substrates comprises the following steps: S1: (1) taking an antifreeze agent, a dispersant, a wetting agent, and a defoaming agent, adding them to water in sequence, dispersing them at a speed of 1100 to 1300 rpm for 5 to 10 minutes, adding titanium dioxide, kaolin, calcium carbonate, cellulose, and a pH regulator in sequence, maintaining a speed of 1100 to 1300 rpm for 25 to 30 minutes until the fineness is dispersed to ≤60 microns, adding a mildew inhibitor, a preservative, an acrylic emulsion, a film-forming aid, and a polyurethane thickener in sequence, maintaining a speed of 900 to 1100 rpm for 10 to 15 minutes, and obtaining component A; (2) taking silicate cement, named component B; S2: Take component A and component B, mix them at a speed of 600-700 rpm for 5-10 minutes to obtain an exterior wall paint.

Citation Information

Cited By

  • Weather-resistant, crack-resistant and high-color-retention exterior wall coating

    CN122405094A