A directed coupled immunosorbent and its preparation method and application

The carrier with epoxy groups is prepared by the emulsification method of polyvinyl alcohol polysaccharide composite microspheres, and the directional coupling of sulfhydryl groups with recombinant proteins is used to solve the problem of reduced adsorption performance caused by amino coupling in the existing technology and achieve high efficiency and stability. protein adsorption effect.

CN116850977BActive Publication Date: 2024-10-01GUANGZHOU KONCEN BIOSCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310936877.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-28
Publication Date
2024-10-01
Estimated Expiration
2043-07-28

AI Technical Summary

Technical Problem

In existing protein coupling technology, amino coupling leads to multi-point coupling, and steric hindrance causes a decrease in adsorption performance. Moreover, common methods such as iodoacetyl or SMCC have high process stability and cost, making it difficult to obtain better directional coupling. connection effect.

Method used

Polyvinyl alcohol polysaccharide composite microspheres are used as carriers to prepare microspheres with epoxy groups through the emulsification method, and the thiol groups of the recombinant protein are used to react with the epoxy groups on the microspheres for directional coupling to form ether bonds to improve the adsorption performance. .

Benefits of technology

It effectively couples recombinant proteins under mild conditions, reduces activity loss, improves adsorption performance, and does not require secondary cross-linking, simplifying the process and reducing costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a directional coupling immunosorbent and its preparation method and application. The carrier of the directional coupling immunosorbent material is a polyvinyl alcohol polysaccharide composite microsphere with an epoxy group, and the adsorbent ligand is a recombinant protein. The recombinant protein reacts with the epoxy group on the polyvinyl alcohol polysaccharide composite microsphere through a thiol group and is directionally coupled to the surface of the microsphere. The reaction conditions for preparing the directional coupling immunosorbent material are mild, and the recombinant protein can be effectively coupled at a lower temperature (such as room temperature). After coupling, the activity loss of the recombinant protein is smaller, and the target substance can be better adsorbed. On the one hand, the modified epoxy group on the polyvinyl alcohol can be cross-linked with the hydroxyl group of the polysaccharide to form an ether bond, thereby increasing the strength of the microsphere without the need for secondary cross-linking. On the other hand, the epoxy group exposed on the surface can be used as an active group to play a pre-activation role. After the composite microsphere is prepared, it can be directly coupled with the protein to prepare the adsorbent, and the activation and secondary coupling can be completed during the ball making process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedical materials, and specifically to a directional coupling immunoadsorption material and a preparation method and application thereof. Background Art

[0002] In recent years, the global monoclonal antibody drugs have developed rapidly. Among the top 10 best-selling products in the world in 2020, 5 are monoclonal antibody drugs. In the downstream purification of antibody drugs, Protein A chromatography media plays a vital role in the capture stage. With the rapid development of large-scale and efficient culture technology for animal cell-expressed antibody products, downstream purification processes have increasingly become the main technical bottleneck in the production of antibody drugs. With the development of technology, the alkali resistance of Protein A chromatography fillers has been further enhanced, and the adsorption performance has been continuously improved, from the initial 20 mg / mL to more than 60 mg / mL.

[0003] The adsorption performance of the chromatographic filler is related to the solid phase microspheres. The smaller the particle size of the microspheres, the larger the surface area, the higher the density of the connected ligands, and the higher the adsorption performance. Another factor affecting the adsorption performance is the coupling method of the ligand. Commonly used protein coupling technology is mainly coupled through amino groups. Proteins contain a large number of amino groups, which will form multi-point couplings. Due to the effect of steric hindrance, the adsorption performance is reduced. In recent years, single-point coupling methods have emerged to improve the adsorption performance of the medium. CN110624274A synthesizes protein A filler by reacting iodoacetyl or bromoacetyl with the thiol on the rProtein A-cys ligand. CN113406320A, CN109781978A, and CN112305222A are coupled by the addition reaction of bifunctional crosslinkers such as SMCC (4-(N-maleimidomethyl) cyclohexane-1-carboxylic acid succinimidyl ester) with thiol groups. The iodoacetyl method is difficult to control the stability of the process because the intermediate iodine or bromine group is more active and the reaction speed is fast; SMCC has poor solubility, and its sulfonated derivative sulfo-SMCC has better stability and solubility, but the preparation process is complicated and expensive.

[0004] In order to obtain better directional coupling effect, it is necessary to develop a new type of directional coupling immunoadsorbent. Summary of the invention

[0005] The purpose of the present invention is to overcome at least one deficiency of the prior art and to provide a directional coupling immunoadsorption material and a preparation method and application thereof.

[0006] The technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides:

[0008] A directional coupling immunoadsorption material, wherein the adsorbent carrier is a polyvinyl alcohol polysaccharide composite microsphere with an epoxy group, the adsorbent ligand is a recombinant protein, and the recombinant protein reacts with the epoxy group on the polyvinyl alcohol polysaccharide composite microsphere through a thiol group to be directionally coupled on the microsphere surface.

[0009] In some examples of directional coupling immunoadsorbent materials, the polyvinyl alcohol-polysaccharide composite microspheres are obtained by reacting polysaccharide with epoxy-modified polyvinyl alcohol through an emulsification method.

[0010] In some examples of directed coupling immunosorbent materials, the epoxy groups are located on the surface and inside of the microspheres.

[0011] In some examples of directional coupled immunosorbent materials, the molar content of epoxy groups in the polyvinyl alcohol polysaccharide composite microspheres is 20-40 μmol / g.

[0012] In some examples of directional coupled immunosorbent materials, the particle size of the polyvinyl alcohol polysaccharide composite microspheres is 40-70 μm.

[0013] In some examples of directed coupled immunoadsorbent materials, the polysaccharide is selected from at least one of cellulose, agarose, dextran and chitosan.

[0014] In some examples of directional coupled immunosorbent materials, the molar content of epoxy groups in the polyvinyl alcohol polysaccharide composite microspheres is 20-40 μmol / g, and the particle size of the polyvinyl alcohol polysaccharide composite microspheres is 40-70 μm.

[0015] The second aspect of the present invention provides:

[0016] The method for preparing the directional coupled immunosorbent material according to the first aspect of the present invention comprises the following steps:

[0017] S1) dissolving polysaccharide and epoxy-modified polyvinyl alcohol, and then obtaining polyvinyl alcohol-polysaccharide composite microspheres by an emulsification method;

[0018] S2) dissolving the recombinant protein in a buffer, adding a disulfide bond reducing agent if necessary, and mixing to obtain a recombinant protein solution;

[0019] S3) mixing the polyvinyl alcohol polysaccharide composite microspheres and the recombinant protein solution for cross-linking reaction, adding a blocking reagent for end-blocking after the cross-linking reaction is completed, and washing to obtain a directional coupled immunosorbent.

[0020] In some examples of the preparation method, the dosage of the recombinant protein is 5 to 30 mg / mL microspheres.

[0021] In some examples of the preparation method, the disulfide bond reducing agent is selected from at least one of tris(2-carboxyethyl)phosphine, β-mercaptoethanol, dithiothreitol and 3-(2-formylethyl)phosphine hydrochloride.

[0022] In some examples of the preparation method, the concentration of the disulfide bond reducing agent in the reaction system is 2-15 mM.

[0023] In some examples of preparation methods, the preparation method of polyvinyl alcohol polysaccharide composite microspheres specifically includes:

[0024] 1) mixing a polysaccharide aqueous solution and an epoxy-modified polyvinyl alcohol aqueous solution, and stirring to obtain an aqueous phase solution, wherein the molar content of epoxy groups in the aqueous phase solution is 30 to 55 μmol / g;

[0025] 2) dissolving the surfactant in the oil phase to obtain an oil phase solution;

[0026] 3) The aqueous phase solution and the oil phase solution are mixed to obtain an emulsion, which is fully emulsified and solidified to obtain composite microspheres.

[0027] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the mass fraction of the polysaccharide in the polysaccharide aqueous solution is 1% to 10%.

[0028] In some examples of the preparation method, when preparing polyvinyl alcohol-polysaccharide composite microspheres, the mass fraction of the epoxy-modified polyvinyl alcohol in the epoxy-modified polyvinyl alcohol aqueous solution is 5 to 20 wt.%.

[0029] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the temperature of the aqueous phase solution is 60-75°C.

[0030] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the stirring time is 30 to 150 minutes.

[0031] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the surfactant is selected from at least one of Span 40, Span 60, Span 80, Span 85 and Tween 20.

[0032] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the oil phase is selected from at least one of liquid paraffin, cyclohexane and toluene.

[0033] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the content of the surfactant in the oil phase is 0.1% to 5%.

[0034] In some examples of the preparation method, the preparation method of the epoxy-modified polyvinyl alcohol includes:

[0035] a) mixing polyvinyl alcohol and water, and heating to obtain a polyvinyl alcohol aqueous solution;

[0036] b) After cooling, an epoxidation reagent is added and reacted in an alkaline environment to obtain epoxy-modified polyvinyl alcohol.

[0037] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the molar ratio of the hydroxyl group of the polyvinyl alcohol to the epoxidation reagent is (1-10):1.

[0038] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the epoxidation agent is selected from at least one of bisglycidyl ether, pentaerythritol glycidyl ether and epichlorohydrin.

[0039] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, bisglycidyl ether is added after the temperature is lowered to 37-70°C.

[0040] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the molar content of the epoxy group of the epoxy-modified polyvinyl alcohol is 90-150 μmol / g.

[0041] The third aspect of the present invention provides:

[0042] The use of a directional coupled immunosorbent material in the preparation of a protein separation and purification agent or a blood purifier, wherein the directional coupled immunosorbent material is as described in the first aspect of the present invention, or is prepared by the preparation method described in the second aspect of the present invention.

[0043] The beneficial effects of the present invention are:

[0044] The directed coupled immunosorbent materials of some examples of the present invention are prepared under mild reaction conditions and can effectively couple recombinant proteins at lower temperatures (such as room temperature). The activity loss of the recombinant proteins after coupling is smaller, and the target substances can be better adsorbed.

[0045] In the process of preparing polysaccharide composite microspheres of the directional coupled immunosorbent material of some examples of the present invention, the epoxy groups modified on the polyvinyl alcohol can cross-link with the hydroxyl groups of the polysaccharide to form ether bonds, thereby increasing the strength of the microspheres without the need for secondary cross-linking. On the other hand, the epoxy groups exposed on the surface can serve as active groups to play a pre-activation role. After the composite microspheres are prepared, they can be directly coupled with proteins to prepare adsorbents, and activation and secondary coupling can be completed during the process of making the microspheres.

[0046] In some examples of the directional coupling immunoadsorption material of the present invention, the epoxy groups on the surface of the composite microspheres are provided by polyvinyl alcohol, which prolongs the distance between the microspheres and the coupled proteins, reduces steric hindrance, and has little effect on the protein performance.

[0047] The directed coupling immunosorbent materials of some examples of the present invention can utilize the thiol and epoxy groups on the recombinant protein for site-specific coupling, have little steric hindrance, can fully expose the active sites of the protein, and thus significantly improve the adsorption performance.

[0048] In some examples of the directional coupling immunoadsorption material of the present invention, the polysaccharide and the polyvinyl alcohol are partially cross-linked before being sphericalized, and active epoxy groups are present inside and on the surface of the composite microspheres, the active sites are increased, and the protein coupling density is improved. DETAILED DESCRIPTION

[0049] The first aspect of the present invention provides:

[0050] A directional coupling immunoadsorption material, wherein the adsorbent carrier is a polyvinyl alcohol polysaccharide composite microsphere with an epoxy group, the adsorbent ligand is a recombinant protein, and the recombinant protein reacts with the epoxy group on the polyvinyl alcohol polysaccharide composite microsphere through a thiol group to be directionally coupled on the microsphere surface.

[0051] The epoxy groups on the polyvinyl alcohol polysaccharide composite microspheres can react and couple with the sulfhydryl groups of the recombinant protein or the sulfhydryl groups formed by opening the disulfide bonds, and the reaction conditions are mild.

[0052] In some examples of directional coupling immunoadsorbent materials, the polyvinyl alcohol-polysaccharide composite microspheres are obtained by reacting polysaccharide with epoxy-modified polyvinyl alcohol through an emulsification method.

[0053] In some examples of directed coupling immunosorbent materials, the epoxy groups are located on the surface and inside of the microspheres.

[0054] The specific content of epoxy groups can be adjusted according to the amount of coupled protein so as to effectively couple the recombinant protein. In some examples of directional coupled immunosorbent materials, the molar content of epoxy groups in the polyvinyl alcohol polysaccharide composite microspheres is 20-40 μmol / g.

[0055] In some examples of directional coupled immunosorbent materials, the particle size of the polyvinyl alcohol polysaccharide composite microspheres is 40-70 μm.

[0056] In some examples of directional coupled immunosorbent materials, the polysaccharide is selected from at least one of cellulose, agarose, dextran and chitosan. These polysaccharides are commonly used materials with relatively stable properties and high safety.

[0057] In some examples of directional coupled immunosorbent materials, the molar content of epoxy groups in the polyvinyl alcohol polysaccharide composite microspheres is 20-40 μmol / g, and the particle size of the polyvinyl alcohol polysaccharide composite microspheres is 40-70 μm.

[0058] The second aspect of the present invention provides:

[0059] The method for preparing the directional coupled immunosorbent material according to the first aspect of the present invention comprises the following steps:

[0060] S1) dissolving polysaccharide and epoxy-modified polyvinyl alcohol, and then obtaining polyvinyl alcohol-polysaccharide composite microspheres by an emulsification method;

[0061] S2) dissolving the recombinant protein in a buffer, adding a disulfide bond reducing agent if necessary, and mixing to obtain a recombinant protein solution;

[0062] S3) mixing the polyvinyl alcohol polysaccharide composite microspheres and the recombinant protein solution for cross-linking reaction, adding a blocking reagent for end-blocking after the cross-linking reaction is completed, and washing to obtain a directional coupled immunosorbent.

[0063] Specifically, when the recombinant protein has thiol groups, it is not necessary to add a disulfide bond reducing agent to form thiol groups. The thiol groups can react and couple with epoxy groups under mild conditions that will not denature the recombinant protein, thereby coupling the recombinant protein and the polyvinyl alcohol polysaccharide composite microspheres together.

[0064] The amount of recombinant protein added can be adjusted according to specific needs and the amount of epoxy groups on the microspheres. Generally speaking, the larger the amount of added, the more epoxy groups there are, the more recombinant protein will be coupled, and vice versa. In some examples of the preparation method, the amount of recombinant protein added is 5 to 30 mg / mL microspheres.

[0065] The disulfide bond reducing agent opens the disulfide bonds in the recombinant protein to form sulfhydryl groups. There is no particular requirement for the type of the reducing agent, as long as the effect on the activity of the recombinant protein is small and the reduction efficiency is high. In some examples of the preparation method, the disulfide bond reducing agent is selected from at least one of tris(2-carboxyethyl)phosphine (TCEP), β-mercaptoethanol (BME), dithiothreitol (DTT) and 3-(2-formylethyl)phosphine hydrochloride (TCEP-HCl).

[0066] The amount of the disulfide bond reducing agent can be adjusted according to the amount of the recombinant protein and the amount of thiol groups required. In some examples of the preparation method, the concentration of the disulfide bond reducing agent in the reaction system is 2-15 mM.

[0067] In some examples of preparation methods, the preparation method of polyvinyl alcohol polysaccharide composite microspheres specifically includes:

[0068] 1) mixing a polysaccharide aqueous solution and an epoxy-modified polyvinyl alcohol aqueous solution, and stirring to obtain an aqueous phase solution, wherein the molar content of epoxy groups in the aqueous phase solution is 30 to 55 μmol / g;

[0069] 2) dissolving the surfactant in the oil phase to obtain an oil phase solution;

[0070] 3) The aqueous phase solution and the oil phase solution are mixed to obtain an emulsion, which is fully emulsified and solidified to obtain composite microspheres.

[0071] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the mass fraction of the polysaccharide in the polysaccharide aqueous solution is 1% to 10%.

[0072] In some examples of the preparation method, when preparing polyvinyl alcohol-polysaccharide composite microspheres, the mass fraction of the epoxy-modified polyvinyl alcohol in the epoxy-modified polyvinyl alcohol aqueous solution is 5 to 20 wt.%.

[0073] In some examples of the preparation method, when preparing polyvinyl alcohol-polysaccharide composite microspheres, the temperature of the aqueous solution is 60-75° C. This can ensure that the polyvinyl alcohol remains dissolved and has a better reaction effect.

[0074] The stirring time can be adjusted according to the reaction conditions (progress), so that the polyvinyl alcohol can be fully epoxidized. In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the stirring time is 30 to 150 minutes.

[0075] There is no special requirement for the surfactant, as long as it is conducive to good emulsification after the water phase and the oil phase are mixed. In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the surfactant is selected from at least one of Span 40, Span 60, Span 80, Span 85, and Tween 20. These surfactants are highly safe and have good emulsification effects.

[0076] In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the oil phase is selected from at least one of liquid paraffin, cyclohexane and toluene. These oil phases are highly safe and low in cost.

[0077] The amount of the surfactant is preferably sufficient for effective emulsification. In some examples of the preparation method, when preparing polyvinyl alcohol polysaccharide composite microspheres, the content of the surfactant in the oil phase is 0.1% to 5%.

[0078] In some examples of the preparation method, the preparation method of the epoxy-modified polyvinyl alcohol includes:

[0079] a) mixing polyvinyl alcohol and water, and heating to obtain a polyvinyl alcohol aqueous solution;

[0080] b) After cooling, an epoxidation reagent is added and reacted in an alkaline environment to obtain epoxy-modified polyvinyl alcohol.

[0081] The epoxy modification reaction is a reversible reaction. The alkaline environment is conducive to the ring-opening coupling of the epoxy group, which can better modify the epoxy group on the polyvinyl alcohol. Generally speaking, the pH of the reaction system is controlled at 7.5-11, preferably 8-10, which can well promote epoxy modification and retain more epoxy groups.

[0082] By adjusting the mixing ratio of the hydroxyl group of polyvinyl alcohol to the epoxidation reagent, the degree of epoxy modification can be adjusted to meet the needs of different applications. In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the molar ratio of the hydroxyl group of the polyvinyl alcohol to the epoxidation reagent is (1-10):1.

[0083] The epoxidation reagent only needs to be safe, stable and easy to react. In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the epoxidation reagent is selected from at least one of bisglycidyl ether, pentaerythritol glycidyl ether and epichlorohydrin. These epoxidation reagents are widely available, safe and easy to use.

[0084] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, diglycidyl ether is added after the temperature is lowered to 37-70° C. This can achieve a better reaction speed.

[0085] In some examples of the preparation method, when preparing the epoxy-modified polyvinyl alcohol, the molar content of the epoxy group of the epoxy-modified polyvinyl alcohol is 90-150 μmol / g.

[0086] The third aspect of the present invention provides:

[0087] The use of a directional coupled immunosorbent material in the preparation of a protein separation and purification agent or a blood purifier, wherein the directional coupled immunosorbent material is as described in the first aspect of the present invention, or is prepared by the preparation method described in the second aspect of the present invention.

[0088] The technical solution of the present invention is further explained below in conjunction with examples.

[0089] Example 1: Preparation of polyvinyl alcohol-agarose composite microspheres

[0090] S1) dissolving polyvinyl alcohol in hot water at a temperature of 90-98°C to prepare a 10% polyvinyl alcohol solution;

[0091] S2) After the polyvinyl alcohol solution is cooled to 50-60°C, diglycidyl ether is added, and the molar ratio of polyvinyl alcohol hydroxyl group to diglycidyl ether is 5:1. The reaction is carried out in an alkaline environment (pH=10) for 3 h to obtain an epoxy-modified polyvinyl alcohol aqueous solution. After testing, the epoxy group density is 105 μmol / g epoxy-modified polyvinyl alcohol;

[0092] S3) dissolving agarose in hot water at a temperature of 90-98°C to prepare a 5% agarose solution;

[0093] S4) mixing the epoxy-modified polyvinyl alcohol aqueous solution and the agarose solution at a volume ratio of 1:1 at 60-75° C. and stirring for 60 min to obtain an aqueous phase solution;

[0094] S5) A toluene oil phase solution containing 2% of a mixed surfactant of Span 80 and Tween 60 (mass ratio 5:1) was prepared, and the aqueous phase solution and the oil phase solution were evenly mixed at a volume ratio of 1.2:1, and mechanically stirred at 70°C for 2 h to form small water-in-oil droplets. Finally, the solution was cooled to 35°C for solidification and washed to obtain pre-activated polyvinyl alcohol-agarose composite microspheres. The epoxy group density of the polyvinyl alcohol-agarose composite microspheres was tested to be 32 μmol / g.

[0095] Example 2: Preparation of polyvinyl alcohol-agarose composite microspheres

[0096] S1) dissolving polyvinyl alcohol in hot water at a temperature of 90-98°C to prepare a 20% polyvinyl alcohol solution;

[0097] S2) After the polyvinyl alcohol solution is cooled to 70°C, epichlorohydrin is added, and the molar ratio of polyvinyl alcohol hydroxyl group to epichlorohydrin is 1:1. The reaction is carried out in an alkaline environment (pH=9) for 2 hours to obtain an epoxy-modified polyvinyl alcohol aqueous solution. After testing, the epoxy group density is 150 μmol / g epoxy-modified polyvinyl alcohol;

[0098] S3) Dissolve agarose in hot water at a temperature of 90-98°C to prepare a 1% agarose solution;

[0099] S4) mixing the epoxy-modified polyvinyl alcohol aqueous solution and the agarose solution at a volume ratio of 1:1 at 60-75° C., stirring for 150 min, to obtain an aqueous phase solution;

[0100] S5) A toluene oil phase solution containing 2% of a mixed surfactant of Span 80 and Tween 60 (mass ratio 5:1) was prepared, and the aqueous phase solution and the oil phase solution were uniformly mixed at a volume ratio of 1.2:1, and mechanically stirred at 70°C for 2 h to form small water-in-oil droplets. Finally, the solution was cooled to 35°C for solidification and washed to obtain pre-activated polyvinyl alcohol-agarose composite microspheres. The epoxy group density of the polyvinyl alcohol-agarose composite microspheres was tested to be 40 μmol / g.

[0101] Example 3: Preparation of polyvinyl alcohol-agarose composite microspheres

[0102] S1) dissolving polyvinyl alcohol in hot water at a temperature of 90-98°C to prepare a 5% polyvinyl alcohol solution;

[0103] S2) After the polyvinyl alcohol solution is cooled to 37° C., diglycidyl ether is added, and the molar ratio of polyvinyl alcohol hydroxyl group to pentaerythritol glycidyl ether is 10:1, and the mixture is reacted in an alkaline environment (pH=9) for 2-4 hours to obtain an epoxy-modified polyvinyl alcohol aqueous solution. After testing, the epoxy group density is 90 μmol / g epoxy-modified polyvinyl alcohol;

[0104] S3) dissolving agarose in hot water at a temperature of 90-98°C to prepare a 10% agarose solution;

[0105] S4) mixing the epoxy-modified polyvinyl alcohol aqueous solution and the agarose solution at a volume ratio of 10:1 at 60-75° C. and stirring for 30 minutes to obtain an aqueous phase solution;

[0106] S5) A toluene oil phase solution containing 2% of a mixed surfactant of Span 80 and Tween 60 (mass ratio 5:1) was prepared, and the aqueous phase solution and the oil phase solution were evenly mixed at a volume ratio of 1.2:1, and mechanically stirred at 70°C for 2 h to form small water-in-oil droplets. Finally, the solution was cooled to 35°C for solidification and washed to obtain pre-activated polyvinyl alcohol-agarose composite microspheres. The epoxy group density of the polyvinyl alcohol-agarose composite microspheres was tested to be 20 μmol / g.

[0107] Example 4: Preparation of Directed Coupling Immunosorbent

[0108] S1) preparing a recombinant protein A solution with a mass concentration of 20 mg / ml, adding 3 mM TCEP and reacting overnight to obtain an activated protein solution;

[0109] S2) taking 20 mL of the polyvinyl alcohol-agarose composite microspheres prepared in Example 1, Example 2, and Example 3, adding 40 mL of PB buffer to obtain a microsphere solution;

[0110] S3) The microsphere solution and the protein solution were mixed in a volume ratio of 3:2, and the mixture was shaken at 35°C for 1 h. After the reaction, the mixture was washed with pure water to obtain the coupled agarose.

[0111] S4) End-capping: Add 1M ethanolamine (2 times the volume of filler) to the coupled agarose and react at 35°C, 180 rpm overnight. After the reaction, rinse with a large amount of purified water and finally store it in 20% ethanol for later use.

[0112] Comparative Example 1:

[0113] Prepared according to Example 2 of CN110026166A. Specifically:

[0114] S1) After rinsing 100 g of agarose gel (Sepharose 6FF) with about 10 times the volume of injection water, add 100 mL of 1 M NaOH solution, 30 mL of epibromopropane and 70 mL of 1,4-butanediol diglycidyl ether and 0.2 g of sodium borohydride, stir, react at 30°C for 1.5 h, and after the reaction is completed, rinse with a large amount of injection water to obtain epoxy-activated agarose gel;

[0115] S2) Add 100 mL of the above-synthesized epoxy-activated agarose gel and 150 mL of 0.1 mol / L borate buffer to a 500 mL reaction vessel, control the system pH to 7.5 to 8.5, add 14 g of genetic engineering recombinant protein A, react for 20 h in a 37°C constant temperature system, stop the reaction, rinse the filler with about 10 times the volume of injection water, and after rinsing, add 200 mL of 0.2 M ethanolamine solution to block the unreacted epoxy group, and react at 20°C for 10 h. After the reaction is completed, rinse with a large amount of injection water, and finally store it in a solution containing a preservative.

[0116] Adsorption performance test

[0117] Take 1 mL of the three synthetic fillers prepared in Example 4 and the filler synthesized in Comparative Example 1 respectively in a 10 mL EP tube, add 8 mL of human plasma, place in a shaker, and slowly shake at room temperature for 1 hour. After adsorption, pour the suspension into a disposable affinity chromatography column, first rinse with about 100 mL PBS, then elute with 80 mL pH 3.0 0.1 M acetate buffer solution, collect the elution peak, and detect the OD280 value by ultraviolet. The adsorption performance (mg / mL) = [(OD280 / 1.38)×80] / 1.

[0118] The adsorption performance of the three immunoadsorption column fillers synthesized in Example 4 for IgG is 75 mg / ml, 68 mg / mL, and 55 mg / mL, respectively. The adsorption performance of the immunoadsorption column filler synthesized in Comparative Example 1 for IgG is 28 mg / mL, which has a good ability to remove IgG antibodies, but is significantly weaker than the three fillers in Example 4.

[0119] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A directed coupled immunosorbent material, characterized in that: The carrier of the adsorption material is polyvinyl alcohol polysaccharide composite microspheres with epoxy groups, the adsorbent ligand is a recombinant protein, the recombinant protein reacts with the epoxy groups on the polyvinyl alcohol polysaccharide composite microspheres through thiol groups and is directionally coupled to the surface of the microspheres, the polyvinyl alcohol polysaccharide composite microspheres are obtained by reacting polysaccharides with epoxy-modified polyvinyl alcohol through an emulsification method, the epoxy groups are located on the surface and inside of the microspheres, and the molar content of the epoxy groups in the polyvinyl alcohol polysaccharide composite microspheres is 20 to 40 μmol / g.

2. The directional coupled immunoadsorbent material according to claim 1, characterized in that: It satisfies at least one of the following conditions: The particle size of the polyvinyl alcohol polysaccharide composite microspheres is 40 to 70 μm; The polysaccharide is selected from at least one of cellulose, agarose, dextran and chitosan.

3. The method for preparing the directional coupled immunoadsorbent material according to claim 1 or 2, comprising the following steps: S1) dissolving polysaccharide and epoxy-modified polyvinyl alcohol, and then obtaining polyvinyl alcohol-polysaccharide composite microspheres by an emulsification method; S2) dissolving the recombinant protein in a buffer, mixing to obtain a recombinant protein solution; or dissolving the recombinant protein in a buffer, adding a disulfide bond reducing agent, and mixing to obtain a recombinant protein solution; S3) mixing the polyvinyl alcohol polysaccharide composite microspheres and the recombinant protein solution for cross-linking reaction, adding a blocking reagent for end-blocking after the cross-linking reaction is completed, and washing to obtain a directional coupled immunosorbent.

4. The preparation method according to claim 3, characterized in that: The dosage of the recombinant protein is 5-30 mg / mL microspheres.

5. The preparation method according to claim 3, characterized in that: The disulfide bond reducing agent is selected from at least one of tris(2-carboxyethyl)phosphine, β-mercaptoethanol, dithiothreitol and 3-(2-formylethyl)phosphine hydrochloride.

6. The preparation method according to claim 3, characterized in that: The preparation method of polyvinyl alcohol polysaccharide composite microspheres specifically includes: 1) mixing a polysaccharide aqueous solution and an epoxy-modified polyvinyl alcohol aqueous solution, and stirring to obtain an aqueous phase solution, wherein the molar content of epoxy groups in the aqueous phase solution is 30 to 55 μmol / g; 2) dissolving the surfactant in the oil phase to obtain an oil phase solution; 3) The aqueous phase solution and the oil phase solution are mixed to obtain an emulsion, which is fully emulsified and solidified to obtain composite microspheres.

7. The preparation method according to claim 6, characterized in that: It satisfies at least one of the following conditions: The mass fraction of polysaccharide in the polysaccharide aqueous solution is 1% to 10%; In the epoxy-modified polyvinyl alcohol aqueous solution, the mass fraction of epoxy-modified polyvinyl alcohol is 5 to 20 wt.%; The temperature of the aqueous phase solution is 60-75°C; The stirring time is 30 to 150 minutes; The surfactant is selected from at least one of Span 40, Span 60, Span 80, Span 85 and Tween 20; The oil phase is selected from at least one of liquid paraffin, cyclohexane and toluene; The content of the surfactant in the oil phase is 0.1% to 5%.

8. The preparation method according to claim 3, characterized in that: The preparation method of the epoxy-modified polyvinyl alcohol comprises: a) mixing polyvinyl alcohol and water and heating to obtain a polyvinyl alcohol aqueous solution; b) After cooling, an epoxidation reagent is added and reacted in an alkaline environment to obtain epoxy-modified polyvinyl alcohol.

9. The preparation method according to claim 8, characterized in that: The preparation method of the epoxy-modified polyvinyl alcohol satisfies at least one of the following conditions: The molar ratio of the hydroxyl group of the polyvinyl alcohol to the epoxidation reagent is (1-10):1; After cooling to 37-70°C, add the epoxidation reagent; The epoxidation agent is selected from at least one of bisglycidyl ether, pentaerythritol glycidyl ether and epichlorohydrin; The molar content of epoxy groups in the epoxy-modified polyvinyl alcohol is 90 to 150 μmol / g.

10. Use of a directional coupled immunosorbent material in the preparation of a protein separation and purification agent or a blood purifier, wherein the directional coupled immunosorbent material is as described in claim 1 or 2, or is prepared by the preparation method according to any one of claims 3 to 9.