A titanium dioxide carrier-supported metal nanocatalyst and its application
Through the combination of amorphous titanium dioxide-supported metal nanocatalyst and polydivinylbenzene, the problem of low deoxysulfide activity of catalytic sulfoxide in hydrogen is solved, and high activity, selectivity and stability are achieved, which simplifies the Preparation steps and extend service life.
Patent Information
- Application Number
- CN202310758904.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-26
AI Technical Summary
The existing methods of deoxygenating catalytic sulfoxide in hydrogen to obtain sulfides have problems of low activity and complex catalytic cycle processes.
Using a hydroxyl-rich amorphous titanium dioxide support to support metal nanocatalysts, the titanium dioxide support is prepared at room temperature and heat treated under a hydrogen atmosphere, combined with the use of polydivinylbenzene, to improve the activity and stability of the catalyst.
The high activity, selectivity and stability of catalytic sulfoxide in hydrogen is achieved, which reduces the reaction temperature, extends the service life of the catalyst, and simplifies the preparation steps.
Smart Images

Figure BDA0004304477870000201 
Figure BDA0004304477870000211 
Figure BDA0004304477870000212
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a metal nanocatalyst supported by a titanium dioxide carrier and application thereof. Background Art
[0002] Sulfides are important chemical intermediates in organic synthesis, biological research, pharmaceutical industry and pesticide synthesis, and have a wide range of applications. The main method for producing sulfides is to use the corresponding alcohols and highly toxic sulfur-containing molecules (such as S 2 Cl 2 , thiols and thiophenols) for sulfidation. However, the disadvantages of the sulfidation method are low product yield, large amount of waste liquid, dangerous and complicated operation process, and it is difficult to apply to the case where the substrate contains multiple active functional groups (such as C=C, C≡C and OH). In contrast, the method of catalyzing the deoxidation of sulfoxides in hydrogen to obtain sulfides has the advantages of being environmentally friendly, good product quality and high yield, so it has begun to be widely used and has attracted much attention.
[0003] According to the patent descriptions of Jpn. Kokai Tokkyo Koho, 2015211932, 26 Nov 2015 and Jpn. Kokai Tokkyo Koho, 2018076261, 17 May 2018, 0.048 wt% of Ru / TiO 2 or 0.5wt% Pt / MoO 3 The sulfides are prepared by catalytic deoxidation methods, but these methods have the disadvantages of low activity and complex and dangerous catalytic cycle processes. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a titanium dioxide carrier and a metal nanocatalyst loaded thereon, which can overcome the problem of low activity in catalyzing the deoxidation of sulfoxide in hydrogen to obtain sulfide, has high activity, selectivity and stability, simple preparation steps, wide application and good commercial value.
[0005] A first aspect of the present invention provides a titanium dioxide carrier.
[0006] A titanium dioxide carrier, wherein the X-ray diffraction pattern of the titanium dioxide carrier does not have a characteristic peak of titanium dioxide between 20° and 80°; and / or
[0007] The Raman spectrum of the titanium dioxide carrier does not have a peak at 250-750 cm -1 The characteristic peaks of titanium dioxide between
[0008] The thermogravimetric analysis curve of the titanium dioxide carrier in air shows that the titanium dioxide carrier has a weight loss of more than 10% between 120 and 500° C.
[0009] In one embodiment, the titanium dioxide support is prepared by the following method:
[0010] At room temperature, after dissolving titanate or titanium tetrachloride in an alcohol solvent, deionized water or an aqueous solution of alkali is added under stirring to generate a precipitate, and stirring is continued until the reaction is completed to obtain a suspension; or, at room temperature, after dissolving titanium trichloride or titanyl sulfate in deionized water, an aqueous solution of alkali is added under stirring, and stirring is continued until the reaction is completed to obtain a suspension;
[0011] Centrifuging the suspension to obtain the precipitate;
[0012] The precipitate is washed, vacuum dried, and calcined to obtain the titanium dioxide carrier.
[0013] In one embodiment, the titanate includes at least one of tetraisopropyl titanate, tetramethyl titanate, tetraethyl titanate, tetrapropyl titanate, tetrabutyl titanate, tetraisobutyl titanate, tetrapentyl titanate, tetrahexyl titanate, 2-ethylhexyl titanate, tetraphenyl titanate, octyl titanate, isooctyl titanate, and hexadecyl titanate.
[0014] In one embodiment, the titanium trichloride is a titanium trichloride solution containing hydrochloric acid.
[0015] In one embodiment, the titanyl sulfate is a titanyl sulfate solution containing sulfuric acid.
[0016] In one embodiment, the generated precipitate is washed three times with deionized water and ethanol respectively, and then placed in a vacuum drying oven at 60° C. for 24 hours. Finally, the dried white powder is calcined at 150° C. for 2 hours to fully remove physically adsorbed water.
[0017] In one embodiment, the alcohol solvent includes at least one of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, hexanol, and octanol.
[0018] A second aspect of the present invention provides a metal nanocatalyst.
[0019] A metal nanocatalyst supported by a titanium dioxide carrier according to the first aspect, wherein the metal nanocatalyst is prepared by the following method:
[0020] At room temperature, the titanium dioxide carrier is dispersed in deionized water, and an aqueous solution of a metal salt is added dropwise under stirring, and the mixture is stirred until the reaction is complete to obtain a suspension;
[0021] Centrifuging the suspension to obtain a precipitate;
[0022] The precipitate was washed, vacuum dried, and 2 ) and an inert gas mixed atmosphere to obtain the metal nanocatalyst.
[0023] In one embodiment, the concentration of the aqueous solution of the metal salt is 1 mol / L.
[0024] In one embodiment, stirring is continued for 12 hours.
[0025] In one embodiment, the generated precipitate is washed three times with deionized water and ethanol respectively. Then, it is placed in a vacuum drying oven at 60° C. for 24 hours. Finally, the dried white powder is transferred to a tube furnace and heated in a mixed atmosphere of hydrogen and argon with a hydrogen volume fraction of 5% (5% H 2 The catalyst was heat treated at 120° C. for 2 hours in a mixed atmosphere of Ar / Ar. After the heat treatment was completed, the catalyst was cooled to room temperature to obtain the metal nanocatalyst.
[0026] In one embodiment, 5% H 2 The flow rate of the Ar / Ar mixed atmosphere was 40 mL / min.
[0027] In one embodiment, the mass ratio of the metal in the aqueous solution of the metal salt to the titanium dioxide support is 0.000975 to 0.0488:1.
[0028] In one embodiment, the mass ratio of the metal in the aqueous solution of the metal salt to the titanium dioxide carrier is 0.000975:1.
[0029] In one embodiment, the mass ratio of the metal in the aqueous solution of the metal salt to the titanium dioxide support is 0.00975:1.
[0030] In one embodiment, the mass ratio of the metal in the aqueous solution of the metal salt to the titanium dioxide support is 0.0488:1.
[0031] In one embodiment, the metal includes at least one of platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), iridium (Ir), iron (Fe), cobalt (Co), and nickel (Ni), preferably Pt.
[0032] A third aspect of the present invention provides a use.
[0033] A use of the metal nanocatalyst described in the second aspect in catalyzing the deoxidation of sulfoxide in hydrogen to prepare sulfide.
[0034] In one embodiment, the sulfoxide is at least one of diphenyl sulfoxide, 4,4'-dichlorodiphenyl sulfoxide, 4,4'-dimethyldiphenyl sulfoxide, 4,4'-dimethoxydiphenyl sulfoxide, phenylmethyl sulfoxide, 4-methylphenylmethyl sulfoxide, 4-methoxyphenylmethyl sulfoxide, butyl sulfoxide, benzyl sulfoxide, cyclobutyl sulfoxide, phenylchloromethyl sulfoxide, sulindac, omeprazole, fenbendazole, sulfinpyrazone, and ethiprole.
[0035] In one embodiment, the metal nanocatalyst is first added to polydivinylbenzene and mixed and ground evenly before use.
[0036] In one embodiment, the mass ratio of polydivinylbenzene to the metal nanocatalyst is 0.5 to 4:1.
[0037] In one embodiment, the mass ratio of polydivinylbenzene to the metal nanocatalyst is 0.5:1.
[0038] In one embodiment, the mass ratio of polydivinylbenzene to the metal nanocatalyst is 1:1.
[0039] In one embodiment, the mass ratio of polydivinylbenzene to the metal nanocatalyst is 2:1.
[0040] In one embodiment, the mass ratio of polydivinylbenzene to the metal nanocatalyst is 4:1.
[0041] In one embodiment, the mass ratio of the sulfoxide to the metal nanocatalyst is 2 to 8:1.
[0042] In one embodiment, the mass ratio of the metal nanocatalyst to the sulfoxide is 2:1.
[0043] In one embodiment, the mass ratio of the metal nanocatalyst to the sulfoxide is 4:1.
[0044] In one embodiment, the mass ratio of the metal nanocatalyst to the sulfoxide is 6:1.
[0045] In one embodiment, the mass ratio of the metal nanocatalyst to the sulfoxide is 8:1.
[0046] In one embodiment, the reaction temperature for catalyzing the deoxidation of sulfoxide in hydrogen to prepare sulfide is 30-120°C.
[0047] In one embodiment, the reaction temperature for catalyzing the deoxidation of sulfoxide in hydrogen to produce sulfide is 30°C.
[0048] In one embodiment, the reaction temperature for catalyzing the deoxidation of sulfoxide in hydrogen to produce sulfide is 50°C.
[0049] In one embodiment, the reaction temperature for catalyzing the deoxidation of sulfoxide in hydrogen to produce sulfide is 80°C.
[0050] In one embodiment, the reaction temperature for catalyzing the deoxidation of sulfoxide in hydrogen to produce sulfide is 120°C.
[0051] Beneficial Effects
[0052] Compared with the prior art, the advantages of the present invention are:
[0053] (1) The titanium dioxide carrier provided by the present invention is a hydroxyl-rich amorphous titanium dioxide, which provides a specific surface area exceeding that of general titanium dioxide carriers, is conducive to loading metals, and the hydroxyl groups therein are easy to leave to form oxygen vacancies, thereby obtaining high catalytic activity.
[0054] (2) The titanium dioxide carrier provided by the present invention can directly replace the titanium dioxide carrier used in commercial titanium dioxide-loaded metal catalysts, and the preparation steps are simple.
[0055] (3) The hydroxyl-rich amorphous titanium dioxide-supported metal catalyst provided by the present invention catalyzes the deoxidation of sulfoxide in hydrogen to prepare sulfide at a low reaction temperature, a sulfoxide conversion rate of up to 100%, high activity, and a selectivity of more than 99%, thereby obtaining a high-purity sulfide.
[0056] (4) The present invention introduces polydivinylbenzene into the metal catalyst to stabilize the activity of the catalyst, prolong its service life, and increase the number of recycling times. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 (a) is TiO in Example 1 2 (a) and TiO 2 (c) is the XRD pattern of TiO 2 (a) and TiO 2 (c) is the Raman spectrum of TiO 2 (a) Thermogravimetric analysis curve in air.
[0058] Figure 2 (a) is Pt in Example 4 1 / TiO 2 (a) Transmission electron microscopy image; (b) Pt / TiO 2 (a) Transmission electron microscope image; (c) Pt NPs / TiO 2 (a) Transmission electron microscopy image.
[0059] Figure 3 is Pt in Example 4 1 / TiO 2(a), Pt / TiO 2 (a) and Pt NPs / TiO 2 (a) In situ diffuse reflectance infrared spectrum of CO adsorption.
[0060] Figure 4 (a) is the Pt / TiO in Example 4 2 (c) Transmission electron microscopy image; (b) Pt / TiO 2 (a) and Pt / TiO 2 (c) In situ diffuse reflectance infrared spectrum of CO adsorption.
[0061] Figure 5 The Pt / TiO2 in Example 9 without the introduction of polydivinylbenzene 2 (a) Cyclic stability test results of catalytic deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide.
[0062] Figure 6 (a) is the molecular structure diagram of polydivinylbenzene in Example 10; (b) is the Pt / TiO 2 (a) Cyclic stability test results of catalytic deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide. DETAILED DESCRIPTION
[0063] In order to enable those skilled in the art to better understand the technical solution of the present invention, some non-limiting embodiments are further disclosed below to further illustrate the present invention in detail.
[0064] Definition of terms
[0065] The term "room temperature" in the present invention refers to ambient temperature, which is from about 10°C to about 40°C. In some embodiments, "room temperature" refers to a temperature from about 20°C to about 30°C; in other embodiments, "room temperature" refers to a temperature from about 25°C to about 30°C; in still other embodiments, "room temperature" refers to 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0066] Regardless of whether the words "about" or "approximately" are used, all numbers disclosed in the present invention are approximate values. Based on the disclosed numbers, the value of each number may vary by less than ±10% or reasonable differences considered by those skilled in the art, such as ±1%, ±2%, ±3%, ±4% or ±5%.
[0067] The term "and / or" in the present invention refers to any or all possible combinations of one or more of the listed items. In addition, the character " / " in the present invention generally indicates that the preceding and following related objects are in an "or" relationship, but it may also indicate an "and / or" relationship, which can be understood by referring to the preceding and following contexts.
[0068] In the present invention, the term "about" generally refers to a variation within the range of 0.5%-10% above or below the specified value, for example, a variation within the range of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, or 10% above or below the specified value.
[0069] In the present invention, it should be noted that, unless otherwise specified, “above” or “below” means the number is inclusive.
[0070] Example 1
[0071] Hydroxyl-rich amorphous titanium dioxide TiO 2 Preparation of (a)
[0072] 1. Synthesis of TiO from isopropyl titanate 2 (a)
[0073] At room temperature, isopropyl titanate (10 mL) was dissolved in isopropanol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. After that, it was placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0074] 2. Synthesis of TiO from Methyl Titanate 2 (a)
[0075] At room temperature, methyl titanate (10 mL) was dissolved in methanol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was separated by centrifugation and washed with deionized water and ethanol respectively, and the washing was repeated three times respectively, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0076] 3. Synthesis of TiO from Ethyl Titanate 2 (a)
[0077] At room temperature, ethyl titanate (10 mL) was dissolved in ethanol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. After that, it was placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0078] 4. Synthesis of TiO from Propyl Titanate 2 (a)
[0079] At room temperature, titanate propoxide (10 mL) was dissolved in propanol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was separated by centrifugation and washed with deionized water and ethanol respectively, and the washing was repeated three times respectively, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0080] 5. Synthesis of TiO from Butyl Titanate 2 (a)
[0081] At room temperature, butyl titanate (10 mL) was dissolved in butanol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. After that, it was placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0082] 6. Synthesis of TiO from isobutyl titanate 2 (a)
[0083] At room temperature, isobutyl titanate (10 mL) was dissolved in isobutyl alcohol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was separated by centrifugation and washed with deionized water and ethanol respectively, and the washing was repeated three times respectively, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0084] 7. Synthesis of TiO from Pentyl Titanate 2 (a)
[0085] At room temperature, pentyl titanate (10 mL) was dissolved in amyl alcohol (40 mL) to form a clear and transparent solution. Deionized water (40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. After that, it was placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0086] 8. Synthesis of TiO from hexyl titanate 2 (a)
[0087] At room temperature, hexyl titanate (10 mL) was dissolved in hexanol (40 mL) to form a clear and transparent solution. An aqueous solution of sodium hydroxide (1 g / L, 40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0088] 9. Synthesis of TiO from Octyl Titanate 2 (a)
[0089] At room temperature, octyl titanate (10 mL) was dissolved in ethanol (40 mL) to form a clear and transparent solution. An aqueous solution of sodium hydroxide (1 g / L, 40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After continuous stirring for two minutes, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0090] 10. Synthesis of TiO from Tetraphenyl Titanate 2 (a)
[0091] At room temperature, tetraphenyl titanate (10 mL) was dissolved in ethanol (40 mL) to form a clear and transparent solution. An aqueous solution of sodium hydroxide (1 g / L, 40 mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times, and then placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0092] 11. Synthesis of TiO from titanium trichloride 2 (a)
[0093] At room temperature, take titanium (III) chloride solution (AR, 15.0-20.0% TiCl 3 basis in30% HCl, 10mL) was dispersed in deionized water (40mL) to form a clear and transparent solution. An aqueous solution of sodium hydroxide (1g / L, 40mL) was added to the solution under stirring, and a purple precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was separated by centrifugation and washed with deionized water and ethanol respectively, and the washing was repeated three times respectively, and then placed in a vacuum drying oven at 60°C for 24 hours. Finally, the dried white powder was calcined at 150°C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0094] 12. Synthesis of TiO from Titanyl Sulfate 2 (a)
[0095] At room temperature, titanium (IV) sulfate solution (~15wt% in dilute sulfuric acid, 99.99% trace metals basis, 10mL) was dispersed in deionized water (40mL) to form a clear and transparent solution. An aqueous solution of sodium hydroxide (1g / L, 40mL) was added to the solution under stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times, and then placed in a vacuum drying oven at 60°C for 24 hours. Finally, the dried white powder was calcined at 150°C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0096] 13. Synthesis of TiO from Titanium Tetrachloride 2 (a)
[0097] At room temperature, titanium tetrachloride (1 mL) was dissolved in isopropanol (40 mL) to form a clear and transparent solution. During the dissolution process, hydrochloric acid mist was generated, so please pay attention to the treatment and protection. Deionized water (40 mL) was added to the solution while stirring, and a white precipitate was observed to form rapidly. After two minutes of continuous stirring, the precipitate was separated by centrifugation, and washed with deionized water and ethanol respectively, and the washing was repeated three times. After that, it was placed in a vacuum drying oven at 60 ° C for 24 hours. Finally, the dried white powder was calcined at 150 ° C for 2 hours to fully remove the physically adsorbed water, and TiO 2 (a).
[0098] The TiO prepared in this example 2 (a) and TiO 2 (c) X-ray diffraction (XRD) analysis was performed. TiO 2 (c) is the purchased crystalline titanium dioxide P25. Figure 1 (a) shown. Figure 1 (a) Display TiO 2 The XRD peaks of (c) are clear and obvious, while TiO 2 (a) has no obvious signal. This indicates that TiO 2 (c) is the classic crystalline phase of TiO 2 , while TiO 2 (a) Amorphous TiO 2 .
[0099] The TiO prepared in this example 2 (a) and TiO 2 (c) Raman spectroscopy analysis was performed. The results are shown in Figure 1 (b) as shown. Figure 1 (b) shows TiO2 (c) TiO with obvious rutile and anatase phases 2 Raman signal, while TiO 2 (a) has no obvious signal. This indicates that TiO 2 (c) The classic rutile and anatase mixed phase of TiO 2 , while TiO 2 (a) Amorphous TiO 2 .
[0100] The TiO prepared in this example 2 (a) Thermogravimetric analysis was performed in air. Figure 1 (c) as shown. Figure 1 (c) Display TiO 2 (a) Continuously lose weight after heating. After the physically adsorbed water is completely removed at 120℃, TiO 2 (a) When heated to 500°C, the dehydration rate will continue to exceed 10% due to the condensation of hydroxyl groups. 2 (a) The surface is rich in hydroxyl groups.
[0101] Example 2
[0102] Hydroxyl-rich amorphous titanium dioxide supported metal nanocatalyst M / TiO 2 (a)
[0103] 1.Pt / TiO 2 (a) Synthesis
[0104] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and a chloroplatinic acid aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Pt / TiO 2 (a). Pt loading is Pt / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0105] 2. Pd / TiO 2 (a) Synthesis
[0106] At room temperature, weigh TiO 2(a) (500 mg) was dispersed in deionized water (10 mL), and a tetrachloropalladic acid aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirred for 12 hours. The suspension was centrifuged to separate the precipitate, and then centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Pd / TiO 2 (a) Pd loading is Pd / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0107] 3. Rh / TiO 2 (a) Synthesis
[0108] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and an aqueous solution of rhodium acetate (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Rh / TiO 2 (a) Rh loading is Rh / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0109] 4.Ru / TiO 2 (a) Synthesis
[0110] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and an aqueous solution of ruthenium trichloride (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Ru / TiO 2 (a) Ru loading is Ru / TiO 2(a) 1 wt% of the total mass of the catalyst.
[0111] 5.Ir / TiO 2 (a) Synthesis
[0112] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and an aqueous solution of chloroiridic acid (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Ir / TiO 2 (a) The loading amount of Ir is Ir / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0113] 6.Fe / TiO 2 (a) Synthesis
[0114] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and an aqueous solution of ferric chloride (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Fe / TiO 2 (a). Fe loading is Fe / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0115] 7. Co / TiO 2 (a) Synthesis
[0116] At room temperature, weigh TiO 2(a) (500 mg) was dispersed in deionized water (10 mL), and a cobalt dichloride aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and then centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Co / TiO 2 (a) Co loading is Co / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0117] 8.Ni / TiO 2 (a) Synthesis
[0118] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and a nickel dichloride aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and then centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Ni / TiO 2 (a) Ni loading is Ni / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0119] Example 3
[0120] 9.Pt / TiO 2 (a) Synthesis
[0121] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and a chloroplatinic acid aqueous solution (0.1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Pt / TiO 2(a). Pt loading is Pt / TiO 2 (a) 0.1 wt% of the total mass of the catalyst.
[0122] 10.Pt / TiO 2 (a) Synthesis
[0123] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and a chloroplatinic acid aqueous solution (1 mol / L, 0.125 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and then centrifuged and washed with deionized water and ethanol, respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed and cooled to room temperature, Pt / TiO 2 (a). Pt loading is Pt / TiO 2 (a) 4 wt% of the total mass of the catalyst.
[0124] Example 4
[0125] 1.TiO 2 (a) Synthesis of supported Pt single atom catalysts
[0126] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and an aqueous solution of chloroplatinic acid (1 mol / L, 0.025 mL) was added dropwise during stirring. The mixed solution was irradiated under a xenon lamp equipped with a 420 nm bandpass filter and stirred for 3 hours. After the photodeposition process was completed, the suspension was centrifuged to separate the precipitate, and the precipitate was washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven and vacuum dried at 60 ° C for 24 hours. The synthesized sample was labeled Pt 1 / TiO 2 (a). The loading amount of Pt is Pt 1 / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0127] 2.TiO 2 (a) Synthesis of supported large-sized Pt catalysts
[0128] At room temperature, weigh TiO 2 (a) (500 mg) was dispersed in deionized water (10 mL), and chloroplatinic acid aqueous solution (1 mol / L, 0.025 mL) was added dropwise under stirring. NaBH 4Solution (0.1mmo / L, 10mL) was added and stirred for 4 hours. The suspension was centrifuged to separate the precipitate, and then centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours. The synthesized sample was labeled Pt NPs / TiO 2 (a). The loading amount of Pt is Pt NPs / TiO 2 (a) 1 wt% of the total mass of the catalyst.
[0129] 3.TiO 2 (c) Synthesis of supported Pt catalyst
[0130] At room temperature, weigh TiO 2 (c) (500 mg) was dispersed in deionized water (10 mL), and a chloroplatinic acid aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed, cool to room temperature. The synthesized sample is marked as Pt / TiO 2 (c) Pt loading is Pt / TiO 2 (c) 1 wt% of the total mass of the catalyst.
[0131] 4. Synthesis of Pt Catalysts Supported by Commercial Supports
[0132] The commercial vector Ti 2 O 3 , Fe 2 O 3 、V 2 O 5 、MoO 3 、Al 2 O 3 、Co 2 O 3 、Co 3 O 4 、SiO 2 、In 2 O 3 、ZrO 2 、CeO 2 The corresponding commercial carrier-supported Pt catalysts were synthesized.
[0133] At room temperature, the corresponding commercial carrier (500 mg) was weighed and dispersed in deionized water (10 mL), and a chloroplatinic acid aqueous solution (1 mol / L, 0.025 mL) was added dropwise during stirring, and stirring was continued for 12 hours. The suspension was centrifuged to separate the precipitate, and the precipitate was centrifuged and washed with deionized water and ethanol respectively, and the washing was repeated three times. The precipitate was then placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours. Afterwards, the dried powder was transferred to a tube furnace and heated at 5% H 2 / Ar (40mL / min) at 120℃ for 2 hours. After the heat treatment is completed, cool to room temperature. The synthesized samples are marked as Pt / Ti 2 O 3 、Pt / Fe 2 O 3 、Pt / V 2 O 5 、Pt / MoO 3 、Pt / Al 2 O 3 、Pt / Co 2 O 3 、Pt / Co 3 O 4 、Pt / SiO 2 、Pt / In 2 O 3 、Pt / ZrO 2 、Pt / CeO 2 The loading amount of Pt was 1 wt% of the total mass of the corresponding Pt catalyst.
[0134] Pt 1 / TiO 2 (a), Pt / TiO 2 (a) and Pt NPs / TiO 2 (a) Scanning electron microscope was used to take pictures. The results are as follows: Figure 2 As shown in (a)-(c). Figure 2 (a) Display Pt 1 / TiO 2 (a) Single Pt atom dispersed in TiO 2 (a) On the carrier. Figure 2 (b) shows Pt / TiO 2 (a) Pt small clusters of about 1 nm are dispersed in TiO 2 (a) On the support, TiO 2 (a) The carrier is a 20-100 nm flocculent aggregate of a large number of 1-5 nm ultra-small nanoparticles. Figure 2 (c) Display Pt NPs / TiO 2(a) Pt particles of about 3 nm are dispersed in TiO 2 (a) On the carrier.
[0135] Pt 1 / TiO 2 (a), Pt / TiO 2 (a) and Pt NPs / TiO 2 (a) In situ diffuse reflectance infrared spectroscopy analysis of CO adsorption was performed. The results are shown in Figure 3 shown. Figure 3 The three different catalysts show different characteristic CO adsorption in situ diffuse reflectance infrared spectroscopy signals. 2 (a) CO adsorption infrared spectrum at 2050 cm -1 There is a characteristic absorption peak.
[0136] For Pt / TiO 2 (c) Scanning electron microscopy was performed to obtain the following results: Figure 4 (a) shown. Figure 4 (a) shows Pt / TiO 2 (c) Pt particles of about 3 nm are dispersed in TiO 2 (c) On a carrier.
[0137] For Pt / TiO 2 (a) and Pt / TiO 2 (c) In situ diffuse reflectance infrared spectroscopy analysis of CO adsorption was performed. The results are shown in Figure 4 (b) as shown. Figure 4 (b) shows Pt / TiO 2 (a) and Pt / TiO 2 (c) In situ diffuse reflectance infrared spectroscopy signals with different characteristic CO adsorption.
[0138] Example 5
[0139] Weigh 0.05g Pt 1 / TiO 2 (a), Pt / TiO 2 (a), Pt NPs / TiO 2 (a), Pt / TiO 2 (c), Pd / TiO 2 (a), Ru / TiO 2 (a), Rh / TiO 2 (a), Ir / TiO 2 (a), Pt / Ti 2 O 3 、Pt / Fe 2 O3 、Pt / V 2 O 5 、Pt / MoO 3 、Pt / Al 2 O 3 、Pt / Co 2 O 3 、Pt / Co 3 O 4 、Pt / SiO 2 、Pt / In 2 O 3 、Pt / ZrO 2 、Pt / CeO 2 , named test groups 1 to 19, added to a 20 mL reaction bottle, and then added 0.1 g of diphenyl sulfoxide and 5 mL of toluene as solvent, and heated at 1 bar H 2 , 80°C for 20 minutes / 1 hour (the slow reaction takes 1 hour), then samples are taken and analyzed by gas chromatography using the internal standard method to determine the performance of different catalysts in catalyzing the deoxidation of diphenyl sulfoxide to prepare diphenyl sulfide. The specific situation is shown in Table 1.
[0140] Table 1 Specific conditions of preparing diphenyl sulfide by deoxygenation of diphenyl sulfoxide catalyzed by different catalysts
[0141]
[0142]
[0143] Table 1 shows that the titanium oxide support performs better than other supports in this catalytic reaction, and the Pt / TiO 2 (a) The catalyst has the best catalytic activity.
[0144] Example 6
[0145] Weigh 0.05g Pt / TiO 2 (a) and 0.5 mmol of sulfoxide substrates such as diphenyl sulfoxide, 4,4'-dichlorodiphenyl sulfoxide, 4,4'-dimethyldiphenyl sulfoxide, 4,4'-dimethoxydiphenyl sulfoxide, phenylmethyl sulfoxide, 4-methylphenylmethyl sulfoxide, 4-methoxyphenylmethyl sulfoxide, phenylchloromethyl sulfoxide, benzyl sulfoxide, cyclobutyl sulfoxide, butyl sulfoxide, sulindac, omeprazole, sulfinpyrazone, ethiprole, named test groups 20 to 34, were added to a 20 mL reaction bottle, and 5 mL of deuterated chloroform was added as solvent. The mixture was heated at 1 bar H 2 , 80℃ reaction for several hours, sample was taken, and NMR analysis was used to determine the Pt / TiO 2 (a) Catalytic performance of the catalyst in catalyzing the deoxidation of different types of sulfoxide substrates to produce sulfides. The details are shown in Table 2.
[0146] Table 2 Pt / TiO 2 (a) Catalytic deoxygenation of different types of sulfoxide substrates to produce sulfides
[0147]
[0148]
[0149] Table 2 shows the Pt / TiO 2 (a) It can be applied to catalyze the deoxygenation of various types of sulfoxide substrates to prepare sulfides.
[0150] Example 7
[0151] Weigh 0.05g Pt / TiO 2 (a) and 0.2, 0.3 and 0.4 g of the sulfoxide substrate diphenyl sulfoxide, named test groups 35-37, were added to a 20 mL reaction bottle, and 10 mL of toluene was added as solvent. The mixture was heated at 1 bar H 2 , 80℃ for several hours, then sample and analyze by gas chromatography using internal standard method to determine Pt / TiO 2 (a) Catalytic performance of the catalyst in the deoxidation of different masses of diphenyl sulfoxide to prepare diphenyl sulfide. The details are shown in Table 3.
[0152] Table 3 Pt / TiO 2 (a) Catalytic deoxygenation of diphenyl sulfoxide of different masses to prepare diphenyl sulfide
[0153] Test group number Diphenyl sulfoxide mass (g) Conversion rate (%) Reaction time (h) Test group 35 0.2 100 2 Test group 36 0.3 100 5 Test group 37 0.4 100 12
[0154] Example 8
[0155] Weigh 0.05g Pt / TiO 2 (a) and 0.101 g of the sulfoxide substrate diphenyl sulfoxide, named test groups 38 to 40, were added to a 20 mL reaction bottle, and 10 mL of toluene was added as solvent. 2 After reacting for several hours at 30, 50, and 120 °C, samples were taken and analyzed by gas chromatography using the internal standard method to determine the Pt / TiO 2 (a) The performance of the catalyst in catalyzing the deoxidation of diphenyl sulfoxide to prepare diphenyl sulfide at different temperatures. The specific situation is shown in Table 4.
[0156] Table 4 Pt / TiO 2 (a) Catalytic deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide at different temperatures
[0157] Test group number Temperature(℃) Conversion rate (%) Reaction time (h) Test group 38 30 100 12 Test group 39 50 100 1 Test group 40 120 100 0.08
[0158] Example 9
[0159] Pt / TiO 2 (a) Reuse
[0160] However, the method of catalyzing the deoxidation of sulfoxide in hydrogen to obtain sulfide has a most concerned problem, that is, the metal catalyst is easily poisoned by the product sulfide, thereby reducing the catalyst activity. In addition, to solve these problems, there are usually two ways: (1) high-temperature hydrogen reduction before the catalyst is recycled; (2) improving the structural properties of the catalyst to achieve the purpose of not being easily poisoned by the product sulfide.
[0161] Weigh 0.05g Pt / TiO 2 (a) and 0.101 g of the sulfoxide substrate diphenyl sulfoxide were added to a 20 mL reaction bottle, and 10 mL of toluene was added as solvent. 2 , 80℃ for 15 minutes, then sampled, washed with ethanol three times, and reused under the same conditions, and sampled separately. The performance of the catalyst in catalyzing the deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide was determined by gas chromatography using the internal standard method. Figure 5 As shown in the figure, the conversion rate of diphenyl sulfoxide in the fourth cycle reaction dropped significantly to less than 60%. 2 (a) The catalyst stability is average.
[0162] Example 10
[0163] Weigh 0.05g Pt / TiO 2 (a) and 0.025, 0.05, 0.1 and 0.2 g of polydivinylbenzene (molecular structure: Figure 6 The mixture (as shown in (a)) was mixed and ground evenly, named test groups 41 to 44, added to a 20 mL reaction bottle, added 0.101 g of diphenyl sulfoxide, and then added 10 mL of toluene as solvent, and heated at 1 bar H 2 , 80℃ for 15 minutes, then sampled, washed with ethanol three times, and reused under the same conditions, and sampled separately. The performance of the catalyst in catalyzing the deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide was determined by gas chromatography using the internal standard method.
[0164] Pt / TiO with different mass of polydivinylbenzene 2 (a) The details of the 7th reaction cycle of the catalyst for the deoxygenation of diphenyl sulfoxide to prepare diphenyl sulfide are shown in Table 5.
[0165] Table 5 Pt / TiO with different mass of polydivinylbenzene 2 (a) Details of the seventh cycle of the catalyst catalyzing the deoxygenation of diphenyl sulfoxide to produce diphenyl sulfide
[0166] Test group number Polydivinylbenzene mass (g) Conversion rate (%) Test group 41 0.025 75 Test group 42 0.05 80 Test group 43 0.1 80 Test group 44 0.2 80
[0167] Pt / TiO with 0.05 g polydivinylbenzene 2 (a) The conversion rate of diphenyl sulfoxide in the deoxidation of diphenyl sulfoxide to prepare sulfide by catalytic reaction of 7 cycles of the catalyst is as follows: Figure 6 As shown in (b), after 7 cycles of reaction, the conversion rate of diphenyl sulfoxide remained basically stable. This indicates that the introduction of polydivinylbenzene makes Pt / TiO 2 (a) The catalyst has stable activity, high product quality, long service life, can be recycled many times, and can reduce process costs.
[0168] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A metal nanocatalyst supported by a titanium dioxide carrier, characterized in that: The transmission electron microscopy image of the metal nanocatalyst shows that small clusters of metal nanoparticles of 1 nm are dispersed on flocculent aggregates of 20-100 nm, and the flocculent aggregates are formed by the aggregation of titanium dioxide nanoparticles of 1-5 nm; The X-ray diffraction pattern of the titanium dioxide carrier does not have a characteristic peak of titanium dioxide between 20° and 80°; and / or The Raman spectrum of the titanium dioxide carrier does not have a peak in the range of 250-750 cm -1 The characteristic peaks of titanium dioxide between and The thermogravimetric analysis curve of the titanium dioxide carrier in air shows that the titanium dioxide carrier has a weight loss of more than 10% between 120 and 500° C.; The metal includes at least one of platinum, palladium, rhodium, ruthenium, iridium, iron, cobalt, and nickel; Prepared by the following method: At room temperature, the titanium dioxide carrier is dispersed in deionized water, and an aqueous solution of a metal salt is added dropwise under stirring, and the mixture is stirred until the reaction is complete to obtain a suspension; Centrifuging the suspension to obtain a precipitate; The precipitate is washed, vacuum dried, and heat treated in a mixed atmosphere of hydrogen and inert gas to obtain the metal nanocatalyst.
2. The metal nanocatalyst according to claim 1, characterized in that Prepared by the following method: At room temperature, after dissolving titanate or titanium tetrachloride in an alcohol solvent, deionized water or an aqueous solution of alkali is added under stirring to generate a precipitate, and stirring is continued until the reaction is completed to obtain a suspension; or, at room temperature, after dissolving titanium trichloride or titanyl sulfate in deionized water, an aqueous solution of alkali is added under stirring, and stirring is continued until the reaction is completed to obtain a suspension; Centrifuging the suspension to obtain the precipitate; The precipitate is washed, vacuum dried, and calcined to obtain the titanium dioxide carrier.
3. The metal nanocatalyst according to claim 1, characterized in that The mass ratio of the metal in the aqueous solution of the metal salt to the titanium dioxide carrier is 0.000975-0.0488:
1.
4. The metal nanocatalyst according to claim 1, characterized in that The metal is platinum.
5. Use of the metal nanocatalyst according to any one of claims 1 to 4 in catalyzing the deoxidation of sulfoxide in hydrogen to prepare sulfide.
6. The use according to claim 5, characterized in that The metal nanocatalyst is first added with polydivinylbenzene and mixed and ground evenly before use.
7. The use according to claim 6, characterized in that The mass ratio of polydivinylbenzene to the metal nanocatalyst is 0.5-4:
1.