Amorphous neodymium-doped manganese-based oxide catalyst material and preparation method and application thereof
Through hydrothermal synthesis, the rare earth elements neodymium and potassium are introduced into the crypto-potassium manganese ore-type manganese oxide to form an amorphous neodymium doped manganese-based oxide catalyst, which solves the problem of removing soot particles in diesel engine exhaust gas, and achieves efficient catalytic activity and stability and has the advantages of low cost and environmental protection.
Patent Information
- Application Number
- CN202310846171.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-07-11
AI Technical Summary
The prior art lacks high-performance catalysts to effectively remove soot particles in diesel engine exhaust gas, resulting in environmental pollution and health hazards. There is no record of the introduction of rare earth element Nd to form amorphous NdMnO materials for soot oxidation catalysts.
Neodymium and potassium are introduced through hydrothermal synthesis to transform the manganese oxide into an amorphous neodymium doped manganese oxide catalyst. The doping of rare earth elements Nd and potassium makes the crystalline cryptopotassium manganese ore into amorphous state by using the doping of rare earth elements Nd and potassium to transform the crystalline cryptopotassium manganese ore into an amorphous state Manganese-based oxides are used as catalysts for combustion reactions of soot particles.
Complete removal of soot particles below 395°C was achieved, which showed high catalytic activity and stability, and was simple in process, low in cost, green and pollution-free.
Smart Images

Figure CN116870901B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst material preparation, and in particular to an amorphous neodymium-doped manganese-based oxide catalyst material and a preparation method and application thereof. Background Art
[0002] As the importance and necessity of environmental protection and sustainable development in my country become increasingly prominent, the purification and elimination of motor vehicle exhaust pollutants has become one of the important research directions in the development of motor vehicles in the world today. Among them, diesel engine exhaust contains carbon monoxide (CO), nitrogen oxides (NO x ), hydrocarbons (C x H y ) and soot particles and other pollutants. Studies have shown that soot particles in diesel exhaust are the main component of exhaust pollutants and one of the main sources of urban air pollution. They also cause certain harm to human health. Therefore, reducing diesel exhaust pollutants, especially eliminating soot particles, is an important topic in the field of environmental protection. At present, a variety of technologies, including clean oil technology, engine fuel optimization combustion and exhaust after-treatment technology, have been widely studied and used to eliminate soot particles. Among them, catalytic purification of diesel exhaust pollutants before they are discharged into the atmosphere is one of the most effective means to solve the major environmental pollution problem of diesel exhaust soot particles. The key to restricting the development of this catalytic purification technology is the research and development of high-performance catalysts.
[0003] In recent years, manganese-based oxide catalysts have been widely used in various catalytic research fields due to their advantages such as low cost, high redox properties, thermal stability and high mechanical strength. Manganese-based oxide materials have various crystalline phase structures such as β-MnO2, λ-MnO2, γ-MnO2, α-MnO2 and δ-MnO2. Compared with manganese oxide materials with fixed crystalline phase structures, amorphous manganese oxides show more abundant structural defects and uniform active sites. Such unique properties make the design, preparation and application of amorphous manganese-based oxide materials gradually become one of the research hotspots. Chen et al. prepared a new type of amorphous MnO2 / C modified iron-based polymer sphere (a-MnO2 / C-FeGS) by solidification pyrolysis method and used it as a highly active photocatalyst for the photothermal Fenton reaction induced by sunlight. Studies have shown that in situ grown amorphous MnO2 can greatly improve catalytic performance and provide a feasible solution for constructing MnO2-based functional materials with unique structure and excellent catalytic activity [Chem. Eng. J., 2022, 449, 137857]. Han et al. used potassium permanganate and manganese acetate as raw materials to synthesize amorphous manganese oxide (MnO x ), studies have shown that synthesis parameters such as hydrothermal time, temperature and precursor molar ratio significantly affect the performance of MnOx The structural properties and ozone removal performance of KMnO4 and Mn-containing precursors were studied [J.Environ.Sci., 2022, In press]. Similarly, Huang et al. successfully prepared amorphous MnO for ozone catalytic decomposition by regulating the redox microenvironment of the mixed solution between KMnO4 and Mn-containing precursors. x -Cl catalyst [Appl. Catal. B, 2022, 315, 121552]. Yu et al. - prepared a series of amorphous cerium manganese oxide catalysts by a simple hydrothermal method and studied the effects of cerium doping amount and calcination temperature on the physical and chemical properties of the catalyst. The results showed that amorphous Ce n MnO x The catalyst exhibits high oxygen mobility and strong adsorption capacity for oxygen species, which enables it to exhibit excellent catalytic performance in the catalytic reaction of soot combustion [Fuel, 2022, 307, 121803]. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide an amorphous neodymium-doped manganese-based oxide catalyst material and a preparation method thereof, and to prepare a neodymium-doped manganese-based oxide catalyst material with an amorphous structure by a hydrothermal synthesis method.
[0005] To achieve the above object, the present invention first provides a method for preparing an amorphous neodymium-doped manganese-based oxide catalyst material, which innovatively transforms crystalline cryptomelane-type manganese oxide into an amorphous manganese-based oxide material by doping with rare earth elements neodymium and potassium, and uses the amorphous manganese-based oxide material as a catalyst for catalyzing the combustion of soot particles. The preparation method comprises the following steps:
[0006] Dissolving a precursor material of an amorphous neodymium-doped manganese-based oxide catalyst in water to prepare a precursor solution, wherein the precursor material comprises manganese nitrate, neodymium nitrate and potassium nitrate;
[0007] mixing hydrogen peroxide, tetramethylammonium hydroxide and water to obtain a mixed solution;
[0008] The precursor solution and the mixed solution are mixed, and then subjected to a hydrothermal treatment;
[0009] After the hydrothermal treatment is completed, the amorphous neodymium-doped manganese-based oxide catalyst is obtained by suction filtration, drying and calcination.
[0010] In the above preparation method, preferably, the mass ratio of manganese nitrate, neodymium nitrate and potassium nitrate is 0.5-10:0.1-10:0.1-5.
[0011] In the above preparation method, preferably, the volume ratio of hydrogen peroxide, tetramethylammonium hydroxide and water is 1-10:1-30:10-100.
[0012] In the above preparation method, preferably, the temperature of the hydrothermal treatment is 60-180° C., and the time is 4-48 hours.
[0013] In the above preparation method, preferably, the calcination temperature is 650-1000° C. and the calcination time is 2-10 hours.
[0014] In the above preparation method, preferably, the heating rate of the calcination is 2-10°C / min, preferably 5°C / min.
[0015] In the above preparation method, preferably, mixing the precursor solution and the mixed solution is to drop the mixed solution into the precursor solution.
[0016] According to a specific embodiment of the present invention, preferably, the method for preparing the amorphous neodymium-doped manganese-based oxide catalyst material can be carried out according to the following specific steps:
[0017] The precursor materials of the amorphous manganese-based oxide catalyst material, manganese nitrate, neodymium nitrate and potassium nitrate, are weighed according to a certain stoichiometric ratio and placed in a polytetrafluoroethylene liner, and then placed on a magnetic stirrer and stirred until fully dissolved to obtain a precursor solution, wherein the amount of manganese nitrate is 0.5-10g, the amount of neodymium nitrate is 0.1-10g, the amount of potassium nitrate is 0.1-5g, the stirring time is 0.5-2h, and the amount of water is 10-50mL; then, a certain amount of hydrogen peroxide, tetramethylammonium hydroxide and water are measured and placed in a beaker, and then placed on a magnetic stirrer and fully stirred to obtain a mixed solution. The amount of hydrogen peroxide used is 1-10 mL, the amount of tetramethylammonium hydroxide used is 1-30 mL, the stirring time is 0.5-2 h, and the amount of water used is 10-100 mL; after the above solutions are mixed, the mixed solution in the beaker is dripped into the polytetrafluoroethylene liner, and after stirring, the solution is placed in an oven for hydrothermal treatment for 4-48 h, the oven temperature is 60-180° C., and after cooling to room temperature, the solution is removed by suction filtration, and the obtained solid is placed in a constant temperature drying oven at 50-100° C. for drying, and the dried sample is placed in a muffle furnace for calcination at 650-1000° C. for 2-10 h to obtain an amorphous Nd-doped manganese-based oxide catalyst material.
[0018] The present invention introduces neodymium and potassium through a hydrothermal synthesis method, and transforms cryptomelane-type manganese oxide into an amorphous manganese-based oxide material by the combined action of the two.
[0019] The present invention also provides an amorphous neodymium-doped manganese-based oxide catalyst material, which is prepared by the above method.
[0020] The present invention also provides the use of the above-mentioned amorphous neodymium-doped manganese-based oxide catalyst material in the catalytic combustion reaction of carbon smoke particles.
[0021] In the above application, preferably, the catalytic combustion reaction process is to heat up to 50-650° C. at a heating rate of 2° C. / min.
[0022] The amorphous Nd-doped manganese-based oxide catalyst material of the present invention can exhibit high catalytic activity and stability when applied to the catalytic combustion reaction of soot particles, wherein the soot particles can be completely removed at a temperature below 395°C.
[0023] Most of the existing technologies have studied crystalline NdMnO3 as a catalytic material. Currently, there is no record of obtaining a soot oxidation catalyst by introducing the rare earth element Nd to form an amorphous NdMnO material. The present invention prepares a series of amorphous Nd-doped manganese-based oxide catalyst materials by hydrothermal synthesis, and combines them with amorphous Ce n MnO x Compared with the catalysts of the present invention, there are significant differences in the selection of precursor materials and the preparation process, and the present invention exhibits excellent catalytic activity and stability in the catalytic reaction of carbon soot particles.
[0024] The present invention prepares an amorphous Nd-doped manganese-based oxide catalyst material by a hydrothermal method. The catalyst material is composed of neodymium (Nd), potassium (K), manganese (Mn), and oxygen (O) elements. The material is a manganese-based oxide material doped with rare earth element Nd according to a certain stoichiometric ratio. An amorphous Nd-doped manganese-based oxide catalyst material is prepared by a hydrothermal synthesis method, and the amorphous catalyst is applied to the catalytic combustion reaction of diesel engine carbon smoke particles. The present invention introduces rare earth elements neodymium and potassium in the hydrothermal synthesis process to transform crystalline cryptomelane-type manganese oxide into an amorphous manganese-based oxide material, wherein the amorphous manganese-based oxide catalyst material is prepared by a low-cost precursor material and a simple hydrothermal synthesis method. The preparation method involved in the present invention has the advantages of not requiring special equipment and harsh conditions, and the prepared amorphous manganese-based oxide catalyst material exhibits good activity and stability in the catalytic carbon smoke combustion reaction, and has the advantages of simple preparation process, low cost, and green and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 XRD diffraction pattern of K-OMS-2 catalyst provided in Comparative Example 1;
[0026] Figure 2 The SEM photo of the K-OMS-2 catalyst provided in Comparative Example 1;
[0027] Figure 3The XRD diffraction patterns of n% Nd-KMnO catalysts obtained under different Nd doping conditions in Example 1;
[0028] Figure 4 The SEM photos of the n% Nd-KMnO catalysts obtained under different Nd doping conditions provided in Example 1;
[0029] Figure 5 XRD diffraction pattern of the 20% Nd-KMnO catalyst before and after the reaction provided in Example 2;
[0030] Figure 6 This is the XRD diffraction pattern of the 20% Nd—MnO catalyst provided for Comparative Example 2. DETAILED DESCRIPTION
[0031] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for preparing an amorphous Nd-doped manganese-based oxide catalyst, which comprises the following steps:
[0034] At room temperature, 3.58g of manganese nitrate, 0.505g of potassium nitrate and 0.165-3.30g of neodymium nitrate were weighed according to a certain stoichiometric ratio, and 20mL of deionized water was measured. The above precursor materials were placed in a polytetrafluoroethylene liner, and then placed on a magnetic stirrer and stirred until fully dissolved; then, 5mL of hydrogen peroxide, 15mL of tetramethylammonium hydroxide and water were measured and placed in a beaker, and then placed on a magnetic stirrer and stirred fully. After the above solutions were mixed, the solution in the beaker was added dropwise to the polytetrafluoroethylene liner, and after stirring, the solution was placed in an oven for hydrothermal treatment for 12h, and the oven temperature was 120°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in an 80°C constant temperature drying oven for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain an amorphous Nd-doped manganese-based oxide catalyst.
[0035] Among them, the catalysts obtained under different Nd doping conditions are recorded as n% Nd-KMnO, where n is the molar ratio of the raw material Nd(NO3)3·6H2O to 50% Mn(NO3)2, and n% is 5%, 10%, 20%, 50%, 70% and 100% respectively.
[0036] Figure 3 Figure 2 is the XRD pattern of n%Nd-KMnO catalysts obtained under different Nd doping conditions. Figure 3It can be seen that when the Nd doping amount is 5%, the prepared catalyst has a weak diffraction peak at 2θ angle, which belongs to the characteristic diffraction peak of cryptomelane-type manganese oxide crystal phase (K-OMS-2). As the Nd doping amount increases to 100%, the characteristic diffraction peak of the crystal phase disappears, indicating that Nd ions are doped into the lattice of K-OMS-2 and simultaneously destroy its ordered crystal structure to obtain an amorphous manganese-based oxide catalyst. Figure 1 It can be observed that the doping of rare earth element Nd can transform the crystalline cryptomelane-type manganese oxide into an amorphous manganese-based oxide catalyst material. Figure 4 The SEM images of n% Nd-KMnO catalysts obtained under different Nd doping conditions are shown in Figure 1. The n% Nd-KMnO catalyst is a micron-scale cluster structure formed by the aggregation of nanoparticles. Combined with Comparative Example 1, it can be observed that the doping of Nd greatly reduces the particle size of the nanoparticles, and as the Nd doping amount increases, the particle size of the nanoparticles gradually decreases and the number of agglomerates increases.
[0037] Table 1 shows the activity of n% Nd-KMnO catalysts tested in Example 1 for catalytic combustion of soot particles. This series of catalysts have good activity for the combustion of soot particles, and their catalytic activity shows a trend of first increasing and then decreasing with the increase of Nd doping amount. Among them, 20% Nd-KMnO and 50% Nd-KMnO catalysts show relatively high catalytic activity.
[0038] Table 1 Catalytic combustion activity of soot particles over n% Nd-KMnO catalyst
[0039] catalyst <![CDATA[T 10 / ℃]]> <![CDATA[T 50 / ℃]]> <![CDATA[T 90 / ℃]]> <![CDATA[Sco2 m / %]]> 100%Nd-KMnO 285 352 392 99.6 70%Nd-KMnO 272 320 346 99.6 50%Nd-KMnO 269 312 341 99.4 20%Nd-KMnO 272 315 342 99.3 10%Nd-KMnO 275 314 343 98.6 5%Nd-KMnO 278 317 346 98.2
[0040] Example 2
[0041] This example tests the stability of the 20% Nd-KMnO catalyst, as follows:
[0042] To further explore the catalytic performance of the 20% Nd-KMnO catalyst, the catalyst was tested for stability five times under the same conditions. The test results are shown in Table 2. As can be seen from Table 2, in the five cycle tests, the T 10 、T 50 and T 90 The values of 276±4℃, 318±4℃ and 345±3℃ were respectively maintained constant. In addition, the CO2 selectivity of this series of catalysts was higher than 99.0%.
[0043] In order to further verify whether the amorphous structure of the catalyst changed before and after the reaction, the catalyst after the reaction was characterized by XRD, such as Figure 5 As shown. Figure 5It can be seen that compared with the fresh catalyst, the catalyst used for 5 cycles has no obvious diffraction peaks, indicating that the structure of the catalyst has not changed during the reaction and has always maintained an amorphous structure. The above results all show that the prepared 20% Nd-KMnO catalyst has high stability in the reaction of catalyst carbon soot particle combustion.
[0044] Table 2 Stability of soot particles during catalytic combustion over 20% Nd-KMnO catalyst
[0045] catalyst <![CDATA[T 10 / ℃]]> <![CDATA[T 50 / ℃]]> <![CDATA[T 90 / ℃]]> <![CDATA[Sco2 m / %]]> 20%Nd-KMnO-Cycle1 272 315 342 99.3 20%Nd-KMnO-Cycle2 273 317 342 99.1 20%Nd-KMnO-Cycle3 273 318 345 99.0 20%Nd-KMnO-Cycle4 274 317 343 99.0 20%Nd-KMnO-Cycle5 279 322 348 99.1
[0046] Comparative Example 1
[0047] This comparative example provides a method for preparing a cryptomelane-type manganese oxide K-OMS-2 catalyst, comprising the following steps:
[0048] At room temperature, 3.58g of manganese nitrate and 0.505g of potassium nitrate were weighed according to a certain stoichiometric ratio, and 20mL of deionized water was measured. The above precursor materials were placed in a polytetrafluoroethylene liner, and then placed on a magnetic stirrer and stirred until fully dissolved; then, 5mL of hydrogen peroxide, 15mL of tetramethylammonium hydroxide and water were measured and placed in a beaker, and then placed on a magnetic stirrer and stirred fully. After the above solutions were mixed, the solution in the beaker was added dropwise to the polytetrafluoroethylene liner, and after stirring, the solution was placed in an oven for hydrothermal heating for 12h, and the oven temperature was 120°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain a cryptomelane-type manganese oxide K-OMS-2 catalyst.
[0049] Figure 1 is the XRD diffraction pattern of K-OMS-2 agent, Figure 1 It can be seen that the diffraction peaks of the catalyst are all attributed to cryptomelane-type manganese oxide K 2-x Mn8O 16 (K-OMS-2) crystal form. Figure 2 is a SEM photo of the K-OMS-2 catalyst, and the sample is a micron-scale cluster structure formed by the agglomeration of nanoparticles. Table 3 is the activity test results of the K-OMS-2 catalyst prepared in Comparative Example 1 for catalytic combustion of soot particles. Combined with Table 1 in Example 1, it can be observed that the catalytic activity of the catalyst is significantly lower than that of 20% Nd-KMnO and 50% Nd-KMnO catalysts, which further indicates that an appropriate amount of Nd element doping can significantly improve the catalytic activity of amorphous catalysts.
[0050] Table 3 Catalytic combustion activity of soot particles over K-OMS-2 catalyst
[0051] catalyst <![CDATA[T 10 / ℃]]> <![CDATA[T 50 / ℃]]> <![CDATA[T 90 / ℃]]> <![CDATA[Sco2 m / %]]> K-OMS-2 288 330 360 98.4
[0052] The method for evaluating the activity of the catalyst in the present invention is as follows: using a gas chromatography detection system, the catalyst adopts a fixed bed method, and the specific steps are as follows:
[0053] Weighed 0.1g catalyst and 0.01g soot particles are placed on weighing paper, stirred evenly with a spatula to make the catalyst and soot particles loosely contact, and loaded into a 6mm quartz reaction tube, wherein the gas flow rate is controlled to be 50mL / min, the volume content of NO in the gas is 2000ppm, the volume content of O2 is 10%, and the balance is Ar; the heating rate is controlled to be about 2℃ / min.
[0054] Evaluation method: The oxidation ability of the catalyst is expressed by the combustion temperature of the soot particles, where the ignition temperature of the soot particles (T 10 ), the temperature corresponding to the maximum burning rate (T 50 ) and burnout temperature (T 90 ), respectively representing the temperature points corresponding to 10%, 50% and 90% of the soot combustion completion. The calculation method is to integrate the curves of CO2 and CO produced by the soot combustion in the programmed temperature oxidation reaction. The temperature points corresponding to 10%, 50% and 90% of the sum of the integral areas of CO2 and CO are T 10 、T 50 and T 90 . Where S CO2 m It indicates the CO2 selectivity of the catalyst when the soot has the maximum combustion rate. The catalytic combustion results of pure soot particles are shown in Table 4. It can be seen from Table 4 that in the absence of a catalyst, the combustion temperature of pure soot is relatively high, indicating that the amorphous Nd-doped manganese-based oxide catalyst prepared by the present invention has a high catalytic activity for the catalytic combustion of soot particles.
[0055] Table 4 Catalytic combustion activity of pure soot particles
[0056] catalyst <![CDATA[T 10 / ℃]]> <![CDATA[T 50 / ℃]]> <![CDATA[T 90 / ℃]]> <![CDATA[Sco2 m / %]]> Pure carbon smoke particles 461 552 594 38.5
[0057] Comparative Example 2
[0058] This comparative example provides a method for preparing a 20% Nd-MnO catalyst, which comprises the following steps:
[0059] At room temperature, 3.58g of manganese nitrate and 0.660g of neodymium nitrate were weighed according to a certain stoichiometric ratio, and 20mL of deionized water were measured. The above precursor materials were placed in a polytetrafluoroethylene liner, and then placed on a magnetic stirrer and stirred until fully dissolved; then, 5mL of hydrogen peroxide, 15mL of tetramethylammonium hydroxide and water were measured and placed in a beaker, and then placed on a magnetic stirrer and stirred fully. After the above solutions were mixed, the solution in the beaker was added dropwise to the polytetrafluoroethylene liner, and after stirring, the solution was placed in an oven for hydrothermal treatment for 12h at an oven temperature of 120°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in an 80°C constant temperature drying oven for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain a 20% Nd-MnO catalyst.
[0060] Figure 6 The XRD diffraction pattern of 20% Nd-MnO catalyst is shown in Figure 2. Figure 6 It can be seen that the diffraction peaks of the catalyst all belong to the Mn3O4 crystal form. Combining Example 1 and Comparative Example 1, it can be seen that amorphous manganese oxide cannot be obtained by adding Nd alone. Only when Nd and K are simultaneously introduced into the hydrothermal process can the transformation of crystalline manganese oxide to amorphous manganese oxide be achieved.
[0061] Table 5 shows the activity test results of the 20% Nd-MnO catalyst prepared in Comparative Example 2 for catalytic combustion of soot particles.
[0062] Table 5 Catalytic activity of 20% Nd-MnO catalyst in the combustion of soot particles
[0063] catalyst <![CDATA[T 10 / ℃]]> <![CDATA[T 50 / ℃]]> <![CDATA[T 90 / ℃]]> <![CDATA[Sco2 m / %]]> 20%Nd-MnO 280 341 375 99.6
[0064] It can be seen from Table 1 of Example 1 that the catalytic activity of the catalyst is significantly lower than that of the 20% Nd-KMnO catalyst, which further indicates that the catalytic activity of the amorphous manganese oxide obtained under the combined action of Nd and K is much higher than that of the crystalline manganese oxide catalyst.
Claims
1. A method for preparing an amorphous neodymium-doped manganese-based oxide catalyst material, comprising the following steps: Dissolving a precursor material of an amorphous neodymium-doped manganese-based oxide catalyst in water to prepare a precursor solution, wherein the precursor material comprises manganese nitrate, neodymium nitrate and potassium nitrate, and the mass ratio of manganese nitrate, neodymium nitrate and potassium nitrate is 0.5-10:0.1-10:0.1-5; Mixing hydrogen peroxide, tetramethylammonium hydroxide and water to obtain a mixed solution, wherein the volume ratio of hydrogen peroxide, tetramethylammonium hydroxide and water is 1-10:1-30:10-100; The precursor solution and the mixed solution are mixed, and then subjected to a hydrothermal treatment; After the hydrothermal treatment is completed, the amorphous neodymium-doped manganese-based oxide catalyst is obtained by suction filtration, drying and calcination.
2. The preparation method according to claim 1, wherein The temperature of the hydrothermal treatment is 60-180° C., and the time is 4-48 hours.
3. The preparation method according to claim 1, wherein The calcination temperature is 650-1000°C and the calcination time is 2-10 hours.
4. The preparation method according to claim 3, wherein: The heating rate of the calcination is 2-10°C / min.
5. The preparation method according to claim 1, wherein The precursor solution and the mixed solution are mixed by dropping the mixed solution into the precursor solution.
6. An amorphous neodymium-doped manganese-based oxide catalyst material prepared by the method according to any one of claims 1 to 5.
7. Use of the amorphous neodymium-doped manganese-based oxide catalyst material according to claim 6 in the catalytic combustion reaction of soot particles.