A method for preparing ultrathin high-entropy metal hydroxide nanosheet catalysts by low-temperature quenching
The preparation of ultrathin high-entropy metal hydroxide nanosheet catalysts by rapid cooling of molten salts solves the problems of high cost and complex preparation of traditional precious metal catalysts, and realizes a highly efficient and stable OER catalyst, which promotes the conversion and storage of new energy sources.
Patent Information
- Application Number
- CN202310183831.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-02-28
AI Technical Summary
Traditional precious metal catalysts suffer from high cost and low reserves in the oxygen evolution reaction (OER), and existing preparation methods are complex and yield unstable, making it difficult to prepare efficient and stable electrocatalysts.
An ultrathin high-entropy metal hydroxide nanosheet catalyst was prepared by using a molten salt rapid cooling method, which involves mixing five metal acetylacetonate powders with sodium hydroxide solution. The molten salt was rapidly cooled at low temperature to form a defect-rich surface, thereby improving catalytic activity.
The preparation of ultrathin high-entropy metal hydroxide nanosheet catalysts with low cost, simple operation and stable yield has been achieved, which improves the electrocatalytic activity and stability of OER reaction and promotes the application of new energy conversion and storage.
Smart Images

Figure CN116876006B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing ultrathin high-entropy metal hydroxide nanosheet catalysts by low-temperature quenching, belonging to the fields of materials science and engineering technology and chemistry. Background Technology
[0002] Green hydrogen is an ideal form of hydrogen energy that aligns with energy conservation, emission reduction, and dual-carbon goals. Specifically, it refers to the production of hydrogen using renewable energy sources, often involving water electrolysis. In the water electrolysis process, the oxygen evolution reaction (OER) at the anode is slower than the hydrogen evolution reaction (HER) at the cathode. The OER reaction involves a four-electron concerted proton-electron transfer (CPET) reaction, whose sluggish kinetics and slow diffusion severely limit electrocatalytic efficiency, thus reducing the overall energy efficiency of the "electro-hydrogen" conversion. Therefore, developing and utilizing high-performance electrocatalysts is crucial for the smooth progress of the OER reaction and the further development of green hydrogen energy production via electrocatalytic water splitting.
[0003] Traditional precious metal catalysts suffer from high cost and low reserves. To reduce the loading of precious metals and develop materials with both good electrocatalytic activity and stability for OER reactions, high-entropy materials with five or more components have become a key research focus due to their highly tunable charge, spin, and combinatorial freedom. Furthermore, high-entropy materials exhibit thermodynamic high-entropy effects (easily forming stable single-phase solid solutions between elements), structural lattice distortion effects (greater lattice distortion and defects than traditional alloys), kinetic slow diffusion effects (slow diffusion and phase transformation within the material, less prone to grain coarsening and recrystallization at high temperatures), and a cocktail effect in performance (the basic properties of different components and their interactions give high-entropy materials more complex properties; their performance can be adjusted by regulating the relative content of each component). These characteristics ensure that high-entropy materials, when used in OER reactions, not only possess excellent electrocatalytic activity but also maintain good stability. Meanwhile, two-dimensional sheet materials also have significant advantages in the field of catalysis, mainly reflected in their huge specific surface area, excellent mechanical properties, and high electrical conductivity. These characteristics enable them to possess higher density, greater activity, and more stable electrochemical reaction surface active sites. Therefore, the preparation of ultrathin high-entropy metal hydroxide nanosheet catalysts holds promise for developing OER catalyst systems with superior performance and durability.
[0004] To further optimize the surface properties of catalysts, traditional methods generally include chemical methods, phase transitions, surface etching, and electrodeposition. However, these methods are relatively complex to operate and have unstable yields. The method of rapid cooling with molten salts, on the other hand, allows for the formation of defect-rich hydroxyl oxides on the surface of the metal oxide or hydroxide catalyst during the reaction, thus serving as a true "working" surface to enhance catalytic activity (molten salts possess many properties different from aqueous solutions, such as high-temperature stability, low vapor pressure over a wide range, low viscosity, good electrical conductivity, high ion migration and diffusion rates, high heat capacity, and the ability to dissolve various materials). Furthermore, this method is characterized by low cost, simple operation, controllable yield, and wide applicability, offering significant advantages over traditional methods for preparing high-entropy catalysts. Therefore, this invention proposes for the first time a method of rapid cooling with molten salts to prepare ultrathin high-entropy metal hydroxide nanosheet catalysts. Summary of the Invention
[0005] 1. Objective of this invention
[0006] The purpose of this invention is to propose a method for preparing ultrathin high-entropy metal hydroxide nanosheet catalysts by low-temperature cold quenching. This method utilizes rapid cooling of molten salt to prepare high-entropy metal hydroxides and adjust their surface properties. It is simple, safe, and allows for large-scale preparation of ultrathin high-entropy metal hydroxide nanosheet catalysts for the OER reaction of water electrolysis, thereby enriching the application of electrocatalysts in energy conservation, emission reduction, and achieving the "dual carbon target".
[0007] 2. Key Invention Points of this Technology
[0008] The key points of this invention are as follows:
[0009] (1) Weigh a certain amount of five metal acetylacetone salt powders according to the proportion of various metal elements in the finished product, mix them to obtain powder A, wherein the acetylacetone salt powder is ruthenium acetylacetone (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 ZnO4), manganese acetylacetonate (C 10 H 14 MnO4), copper acetylacetone (C 10 H 14 CuO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 Any five of the following: NiO4;
[0010] (2) Weigh 4g of sodium hydroxide powder, dissolve it in a solution of 50ml of ultrapure water and 50ml of anhydrous ethanol, stir well to obtain 1M NaOH, i.e., solution B;
[0011] (3) Place the powder A prepared in step (1) into a preheated muffle furnace and keep it warm for 30 minutes. The reaction atmosphere during preheating is air, the heating rate of the muffle furnace is 5℃ / min, and the holding temperature range is 250℃-300℃. The temperature after preheating and during holding is determined according to the melting point of the selected acetylacetone salt.
[0012] (4) After sealing the solution B prepared in step (2) above with a quartz beaker and sealing film, place it in a cooling bath at -20℃ and keep it for 30 minutes.
[0013] (5) Quickly pour the molten A obtained in step (3) into the cooled B obtained in step (4). After reacting for 30 minutes, filter the resulting mixture and wash it with anhydrous ethanol. Collect and dry for 24 hours to obtain the ultrathin high-entropy metal hydroxide nanosheet catalyst.
[0014] The method for preparing ultrathin high-entropy metal hydroxide nanosheet catalysts by rapid cooling of molten salt proposed in this invention has the advantages of utilizing the properties of molten salt, high-entropy materials, and ultrathin two-dimensional materials, and features simple operation, stable yield, and low cost. It can reduce the loading of precious metals in OER catalysts, thereby promoting the further application of new energy conversion and storage. Attached Figure Description
[0015] Figure 1 This invention relates to the method for preparing ultrathin, high-entropy metal hydroxide nanosheet catalyst materials CuMnFeCoNi(OH). 10 and RuMnFeCoNi(OH) 10 A comparison of the catalytic activity of oxygen evolution in 1M KOH electrolyte with the electrocatalytic performance of the commercial catalyst RuO2. Figure 2 This is an ultrathin RuMnFeCoNi(OH) prepared by the method of this invention. 10 Scanning electron microscope image of two-dimensional nanomaterials. Detailed Implementation
[0016] The following describes embodiments of the method of the present invention:
[0017] Example 1
[0018] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeCoNi(OH) 10 Preparation of .
[0019] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeCoNi(OH) was obtained. 10 .
[0020] Example 2
[0021] Ultrathin, high-entropy metal hydroxide nanosheets CuZnFeCoNi(OH) 10 Preparation of .
[0022] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Zn:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), zinc acetylacetonate (C 10 H 14 ZnO4), iron acetylacetonate (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuZnFeCoNi(OH) was obtained. 10 .
[0023] Example 3
[0024] Ultrathin, high-entropy metal hydroxide nanosheets CuMnZnCoNi(OH) 10 Preparation of .
[0025] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Zn:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), zinc acetylacetonate (C 10 H 14 ZnO4), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnZnCoNi(OH) was obtained. 10 .
[0026] Example 4
[0027] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeZnNi(OH) 10 Preparation of .
[0028] Weigh out 1 mmol of copper acetylacetone (C) according to the molar ratio of Cu:Mn:Fe:Zn:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), zinc acetylacetonate (C 10 H 14 ZnO4), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeZnNi(OH) was obtained. 10 .
[0029] Example 5
[0030] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeCoZn(OH) 10 Preparation of .
[0031] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Fe:Co:Zn = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), zinc acetylacetonate (C 10 H 14After mixing with ZnO4, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a mixture of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH, i.e., solution B, was obtained. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B, and after reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeCoZn(OH)2 was obtained. 10 .
[0032] Example 6
[0033] Ultrathin, high-entropy metal hydroxide nanosheets ZnMnFeCoNi(OH) 10 Preparation of .
[0034] Weigh out 1 mmol of zinc acetylacetonate (C) according to the molar ratio of Zn:Mn:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 ZnO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 250℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 250℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst ZnMnFeCoNi(OH) was obtained. 10 .
[0035] Example 7
[0036] Ultrathin, high-entropy metal hydroxide nanosheets RuMnFeCoNi(OH) 10 Preparation of .
[0037] Weigh out 1 mmol of ruthenium acetylacetone (C) according to the molar ratio of Ru:Mn:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 15 H 21 O6Ru), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst RuMnFeCoNi(OH) was obtained. 10 .
[0038] Example 8
[0039] Ultrathin, high-entropy metal hydroxide nanosheets CuRuFeCoNi(OH) 10 Preparation of .
[0040] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Ru:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), ruthenium acetylacetone (C 15 H 21 O6Ru), acetylacetone iron (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuRuFeCoNi(OH) was obtained. 10 .
[0041] Example 9
[0042] Ultrathin, high-entropy metal hydroxide nanosheets CuMnRuCoNi(OH) 10 Preparation of .
[0043] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Ru:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), ruthenium acetylacetonate (C 15 H 21 O6Ru), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnRuCoNi(OH) was obtained. 10 .
[0044] Example 10
[0045] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeRuNi(OH) 10 Preparation of .
[0046] Weigh out 1 mmol of copper acetylacetone (C) according to the molar ratio of Cu:Mn:Fe:Ru:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), ruthenium acetylacetone (C 15 H 21 O6Ru), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeRuNi(OH) was obtained. 10 .
[0047] Example 11
[0048] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeCoRu(OH) 10 Preparation of .
[0049] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Fe:Co:Ru = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), ruthenium acetylacetone (C 15 H 21After mixing with O6Ru, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH, i.e., solution B, was obtained. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeCoRu(OH) was obtained. 10 .
[0050] Example 12
[0051] Ultrathin, high-entropy metal hydroxide nanosheets RuZnFeCoNi(OH) 10 Preparation of .
[0052] Weigh out 1 mmol of ruthenium acetylacetone (C) according to the molar ratio of Ru:Zn:Fe:Co:Ni = 1:1:1:1:1 in the finished product. 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 ZnO4), iron acetylacetonate (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst RuZnFeCoNi(OH) was obtained. 10 .
[0053] Example 13
[0054] Ultrathin, high-entropy metal hydroxide nanosheets RuMnZnCoNi(OH) 10 Preparation of .
[0055] Weigh out 1 mmol of ruthenium acetylacetone (C) according to the molar ratio of Ru:Mn:Zn:Co:Ni = 1:1:1:1:1 in the finished product. 15 H 21 O6Ru), manganese acetylacetonate (C 10 H 14 MnO4), zinc acetylacetonate (C 10 H 14 ZnO4), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst RuMnZnCoNi(OH) was obtained. 10 .
[0056] Example 14
[0057] Ultrathin, high-entropy metal hydroxide nanosheets (Ru, Mn, Fe, Zn, Ni(OH)) 10 Preparation of .
[0058] Weigh out 1 mmol of ruthenium acetylacetone (C) according to the molar ratio of Ru:Mn:Fe:Zn:Ni = 1:1:1:1:1 in the finished product. 15 H 21 O6Ru), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), zinc acetylacetonate (C 10 H 14 ZnO4), nickel acetylacetonate (C 10 H 14NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst RuMnFeZnNi(OH) was obtained. 10 .
[0059] Example 15
[0060] Ultrathin, high-entropy metal hydroxide nanosheets (RuMnFeCoZn(OH)) 10 Preparation of .
[0061] Weigh out 1 mmol of ruthenium acetylacetone (C) according to the molar ratio of Ru:Mn:Fe:Co:Zn = 1:1:1:1:1 in the finished product. 15 H 21 O6Ru), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), zinc acetylacetonate (C 10 H 14 After mixing with ZnO4, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH, i.e., solution B, was obtained. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B, and after reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst RuMnFeCoZn(OH)2 was obtained. 10 .
[0062] Example 16
[0063] Ultrathin, high-entropy metal hydroxide nanosheets CuRuZnCoNi(OH) 10 Preparation of .
[0064] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Ru:Zn:Co:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), ruthenium acetylacetone (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 ZnO4), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuRuZnCoNi(OH) was obtained. 10 .
[0065] Example 17
[0066] Ultrathin, high-entropy metal hydroxide nanosheets CuRuFeZnNi(OH) 10 Preparation of .
[0067] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Ru:Fe:Zn:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), ruthenium acetylacetone (C 15 H 21 O6Ru), acetylacetone iron (C 15 H 21 FeO6), zinc acetylacetonate (C 10 H 14 ZnO4), nickel acetylacetonate (C 10 H 14NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuRuFeZnNi(OH) was obtained. 10 .
[0068] Example 18
[0069] Ultrathin, high-entropy metal hydroxide nanosheets CuRuFeCoZn(OH) 10 Preparation of .
[0070] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Ru:Fe:Co:Zn = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), ruthenium acetylacetone (C 15 H 21 O6Ru), acetylacetone iron (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), zinc acetylacetonate (C 10 H 14 After mixing with ZnO4, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH, i.e., solution B, was obtained. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuRuFeCoZn(OH) was obtained. 10 .
[0071] Example 19
[0072] Ultrathin, high-entropy metal hydroxide nanosheets CuMnRuZnNi(OH) 10 Preparation of .
[0073] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Ru:Zn:Ni = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), ruthenium acetylacetonate (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 ZnO4), nickel acetylacetonate (C 10 H 14 NiO4 was mixed to obtain powder A. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnRuZnNi(OH) was obtained. 10 .
[0074] Example 20
[0075] Ultrathin, high-entropy metal hydroxide nanosheets CuMnRuCoZn(OH) 10 Preparation of .
[0076] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Ru:Co:Zn = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), ruthenium acetylacetone (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14After mixing with ZnO4, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH was obtained, i.e., solution B. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B. After reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnRuCoZn(OH)2 was obtained. 10 .
[0077] Example 21
[0078] Ultrathin, high-entropy metal hydroxide nanosheets CuMnFeRuZn(OH) 10 Preparation of .
[0079] Weigh out 1 mmol of copper acetylacetonate (C) according to the molar ratio of Cu:Mn:Fe:Ru:Zn = 1:1:1:1:1 in the finished product. 10 H 14 CuO4), manganese acetylacetonate (C 10 H 14 MnO4), iron acetylacetone (C 15 H 21 FeO6), ruthenium acetylacetone (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 After mixing with ZnO4, powder A was obtained. 4g of sodium hydroxide powder was weighed and dissolved in a solution of 50ml ultrapure water and 50ml anhydrous ethanol. After stirring evenly, 1M NaOH, or solution B, was obtained. Powder A was placed in a muffle furnace preheated to 300℃ and held for 30min. The reaction atmosphere was air, the muffle furnace heating rate was 5℃ / min, and the holding temperature was 300℃. Solution B was then sealed in a quartz beaker and sealing film and placed in a cooling bath at -20℃ for 30min. Finally, molten A was quickly poured into the cooled B, and after reacting for 30min, the resulting mixture was filtered and washed with anhydrous ethanol. After collection and drying for 24h, the ultrathin high-entropy metal hydroxide nanosheet catalyst CuMnFeRuZn(OH)2 was obtained. 10 .
Claims
1. A method for preparing ultrathin high-entropy metal hydroxide nanosheet catalysts by low-temperature quenching, characterized in that... The method includes the following steps: (1) Weigh a certain amount of five metal acetylacetone salt powders according to the proportion of various metal elements in the finished product, mix them to obtain powder A, wherein the acetylacetone salt powder is ruthenium acetylacetone (C 15 H 21 O6Ru), zinc acetylacetonate (C 10 H 14 ZnO4), manganese acetylacetonate (C 10 H 14 MnO4), copper acetylacetone (C 10 H 14 CuO4), iron acetylacetone (C 15 H 21 FeO6), cobalt acetylacetonate (C 15 H 21 CoO6), nickel acetylacetonate (C 10 H 14 Any five of the following: NiO4; (2) Weigh 4g of sodium hydroxide powder, dissolve it in a solution of 50ml of ultrapure water and 50ml of anhydrous ethanol, stir well to obtain 1M NaOH, i.e., solution B; (3) Place the powder A prepared in step (1) into a preheated muffle furnace and keep it warm for 30 minutes. The reaction atmosphere during preheating is air, the heating rate of the muffle furnace is 5℃ / min, and the holding temperature range is 250℃-300℃. The temperature after preheating and during holding is determined according to the melting point of the selected acetylacetone salt. (4) After sealing the solution B prepared in step (2) above with a quartz beaker and sealing film, place it in a cooling bath at -20℃ and keep it for 30 minutes. (5) Quickly pour the molten A obtained in step (3) into the cooled B obtained in step (4). After reacting for 30 minutes, filter the resulting mixture and wash it with anhydrous ethanol. Collect the mixture and air dry it for 24 hours to obtain the ultrathin high-entropy metal hydroxide nanosheet catalyst.