Preparation method and application of carbon-based hollow sphere material

The resorcinol-formaldehyde resin hollow sphere formed by reacting in ethanol, water and ammonia water is heated in an inert atmosphere to obtain carbon-based hollow sphere material, which solves the problems of cumbersome steps and irregular structure in the prior art, and realizes the problem of numbness in the process of the prior art. It has efficient catalytic and environmentally friendly industrial applications.

CN116902958BActive Publication Date: 2024-11-26LIAONING YUANTONG ELECTRIC POWER TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310907675.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-24
Publication Date
2024-11-26
Estimated Expiration
2043-07-24

AI Technical Summary

Technical Problem

The preparation methods of existing carbon-based hollow sphere materials are cumbersome, the conditions are harsh, and the product structure is poor, making them not suitable for large-scale applications.

Method used

The reaction of linear alkyl amine, n-alkanes, resorcinol and formaldehyde in a mixed solution of ethanol, water and ammonia is used to form a hollow sphere of resorcinol-formaldehyde resin, and the carbon-based is obtained by heating in an inert atmosphere. Hollow ball material.

Benefits of technology

It has achieved carbon-based hollow sphere materials with high catalytic efficiency, regular morphology, ideal nitrobenzene conversion and ortho-chloroaniline selectivity. It is simple in process, low cost, environmentally friendly, and suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116902958B_ABST
    Figure CN116902958B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of catalytic material synthesis, and in particular to a preparation method and application of a carbon-based hollow sphere material. The carbon-based material comprises resorcinol-formaldehyde resin and charcoal. The outer diameter of the hollow sphere is 0.8-1.8 μm, and the hollow diameter is 0.3-1.0 μm. The synthesis method of the carbon-based hollow sphere material comprises the following steps: (1) dispersing a straight-chain alkylamine and a normal alkane in a mixed solution of ethanol, water and ammonia water, and adding resorcinol and formaldehyde to obtain an initial mixture; (2) placing the obtained initial mixture in a reaction temperature range of 25-35°C for reaction for not less than 16 hours, and the obtained solid product is a hollow sphere of resorcinol-formaldehyde resin, and further carbonization can obtain a carbon hollow sphere. The preparation method of the present invention has a simple process, low cost, strong practicality and good industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic material synthesis, and in particular relates to a preparation method of a carbon-based hollow sphere material and application thereof. Background Art

[0002] Carbon-based hollow sphere materials have the characteristics of low mass density, high porosity, large specific surface area and acid and alkali resistance. They are widely used in catalysis, energy storage and conversion, adsorption and separation, and are a hot spot in the field of nanomaterial synthesis and application research. However, the preparation method of carbon-based hollow sphere materials is relatively simple. The hard template method is currently commonly used, that is, using decomposable and removable micro-nanospheres such as silicon dioxide, metal oxides, etc. as templates, and coating the carbon-based material on the template surface by physical or chemical means. Finally, the template is removed by acid or alkali etching to form a carbon-based hollow sphere material. Fuertes et al. (Chem. Commun., 2012, 48, 6124) synthesized SiO2@RF core-shell structure by one-pot method. After carbonization, SiO2 was removed by sodium hydroxide solution to obtain carbon hollow spheres. Liu et al. used silica as template, polymerized dopamine on its surface to form a carbon layer, and then removed silica by hydrofluoric acid to form carbon hollow spheres (Angew. Chem. Int. Ed., 2011, 50, 6799). Although the product obtained by the template method has regular morphology and strong controllability, the synthesis steps are cumbersome and the process is relatively complicated. Removing the template requires a large amount of acid or alkaline solution, which is unfavorable to the environment and is not suitable for large-scale application. Therefore, developing a simple synthesis method for carbon-based hollow sphere materials is a common goal of researchers in this field. Summary of the invention

[0003] The present invention aims to overcome the shortcomings of the prior art such as complicated synthesis steps, harsh conditions, poor product structural regularity, etc., and provide a preparation method and application of a carbon-based hollow sphere material with high catalytic efficiency, regular morphology, and ideal nitrobenzene conversion rate and o-chloroaniline selectivity.

[0004] To solve the above technical problems, the present invention is achieved as follows:

[0005] A method for preparing a carbon-based hollow sphere material comprises the following steps:

[0006] (1) First, a linear alkylamine and a normal alkane are dispersed in a mixed solution of ethanol, water and ammonia, and then resorcinol and formaldehyde are added to obtain an initial mixture;

[0007] (2) placing the initial mixture obtained in step (1) in a temperature environment of 25 to 35° C. for a reaction time of not less than 16 hours to obtain a solid product of resorcinol-formaldehyde resin hollow spheres;

[0008] (3) The resorcinol-formaldehyde resin hollow spheres obtained in step (2) are heated at 500-900° C. for not less than 4 hours in an inert atmosphere to obtain the target carbon-based hollow sphere material.

[0009] Furthermore, in step (1), in the initial mixture, the ratio of ethanol to water is: 25-40 ml: 45-60 ml; the ratios of ammonia water, linear alkylamine, normal alkane, resorcinol and formaldehyde are: 0.2 g: 0.05-0.4 g: 0.06-0.48 g: 0.1-0.6 g: 0.15-0.9 g, respectively.

[0010] Furthermore, the concentration of the aqueous ammonia is in the range of 25-28 wt %, and the concentration of the formaldehyde solution is in the range of 35-40 wt %.

[0011] Furthermore, the carbon-based material in the carbon-based hollow sphere material includes resorcinol-formaldehyde resin or carbon, the outer diameter of the carbon-based hollow sphere is 0.8-1.8 μm, and the hollow diameter of the carbon-based hollow sphere is 0.3-1.0 μm.

[0012] Furthermore, the chemical formula of the linear alkylamine is C n H 2n+1 NH2, where n=12~16.

[0013] Furthermore, the chemical formula of the normal alkane is C n H 2n+2 , where n=6~12.

[0014] Furthermore, in step (3), the inert atmosphere is selected from at least one of nitrogen, helium and argon.

[0015] The product obtained by the above-mentioned method for preparing the carbon-based hollow sphere material is used as a catalyst carrier for preparing aniline by hydrogenating nitrobenzene.

[0016] The present invention has high catalytic efficiency, regular morphology, and ideal nitrobenzene conversion rate and o-chloroaniline selectivity. Compared with the prior art, the present invention can produce the following beneficial effects:

[0017] 1) The carbon-based hollow sphere material provided in this application has regular morphology and significant structural characteristics, and can be used as a catalyst carrier to catalyze the hydrogenation of nitrobenzene to produce aniline, with good results, and is expected to be applied in large-scale industry.

[0018] 2) The preparation method of the carbon-based hollow sphere material provided in this application has a simple process and low cost, overcomes the limitations of the cumbersome steps of the prior art, is environmentally friendly, has strong practicality, environmental protection and good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1This is a transmission electron microscope photograph of the resorcinol-formaldehyde resin hollow spheres obtained in Example 2 of the present invention.

[0020] Figure 2 This is a transmission electron microscope photograph of the carbon-based hollow spheres obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0021] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the protection scope of the present invention. After reading the contents recorded in the present invention, all other embodiments obtained after various changes or modifications made to the present invention based on the technical solution and embodiments of the present invention also fall within the scope of protection of the claims of the present invention.

[0022] Unless otherwise specified, the basic raw materials used in this application were purchased from commercial sources and used directly without special treatment.

[0023] In the examples, the calculation methods for the conversion rate of nitrobenzene and the selectivity of o-chloroaniline are (1)-(2) respectively:

[0024] (1)

[0025] (2)

[0026] M1 is the mass of raw material nitrobenzene, M2 and M3 are the mass of nitrobenzene and o-chloroaniline after the reaction, respectively.

[0027] Example 1 Preparation of materials

[0028] Take 0.05g dodecylamine and 0.06g n-hexane and dissolve them in 25ml ethanol, add 60ml deionized water and 0.2g ammonia water (25-28wt%) and mix well, add 0.1g resorcinol and 0.15g formaldehyde solution (37wt%), stir continuously at 25°C for 24h, separate the solid product by centrifugation, and obtain resorcinol-formaldehyde resin hollow spheres after drying, which are recorded as sample 1 # . Sample 1 # Heating at 500 °C for 4 h in a nitrogen atmosphere gave carbon-based hollow spheres, which were designated as sample 2. # .

[0029] Example 2 Preparation of materials

[0030] Take 0.1g dodecylamine and 0.12g n-hexane and dissolve them in 25ml ethanol, add 60ml deionized water and 0.2g ammonia water (25-28wt%) and mix evenly, add 0.2g resorcinol and 0.3g formaldehyde solution (37wt%), stir continuously at 30°C for 24h, separate the solid product by centrifugation, and obtain resorcinol-formaldehyde resin hollow spheres after drying, which are recorded as sample 3 # . Sample 3 # The carbon-based hollow spheres were obtained by heating at 500°C for 4 hours in a nitrogen atmosphere and recorded as sample 4. # .

[0031] Example 3 Preparation of materials

[0032] Take 0.4 g dodecylamine and 0.48 g n-hexane and dissolve them in 40 ml ethanol, add 45 ml deionized water and 0.2 g ammonia water (25-28 wt%) and mix well, add 0.6 g resorcinol and 0.9 g formaldehyde solution (37 wt%), stir at 30 ° C for 24 h, separate the solid product by centrifugation, and dry to obtain resorcinol-formaldehyde resin hollow spheres, which are recorded as sample 5 # . Sample 5 # The carbon-based hollow spheres were obtained by heating at 900 °C for 4 h in an argon atmosphere and recorded as sample 6. # .

[0033] Example 4 Preparation of materials

[0034] Take 0.13g hexadecylamine and 0.12g n-hexane and dissolve them in 25ml ethanol, add 60ml deionized water and 0.2g ammonia water (25-28wt%) and mix well, add 0.2g resorcinol and 0.3g formaldehyde solution (37wt%), stir at 30°C for 24h, separate the solid product by centrifugation, and obtain resorcinol-formaldehyde resin hollow spheres after drying, which are recorded as sample 7. # . Sample 7 # The carbon-based hollow spheres were obtained by heating at 600°C for 4 hours in a nitrogen atmosphere and recorded as sample 8. # .

[0035] Example 5 Preparation of materials

[0036] 0.1 g dodecylamine and 0.237 g n-dodecane were dissolved in 25 ml ethanol, 60 ml deionized water and 0.2 g ammonia water (25-28 wt%) were added and mixed evenly, 0.2 g resorcinol and 0.3 g formaldehyde solution (37 wt%) were added, and the mixture was stirred at 30 °C for 24 h. The solid product was separated by centrifugation and dried to obtain hollow resorcinol-formaldehyde resin spheres, which were recorded as sample 9. # . Sample 9 # The carbon-based hollow spheres were obtained by heating at 500 °C for 4 h in a nitrogen atmosphere and recorded as sample 10.# .

[0037] Example 6 Application of Materials

[0038] Weigh 0.2g of sample 3 # Dispersed in 5 ml of deionized water and 45 ml of ethanol, 0.5 g of chloroplatinic acid aqueous solution (77 mM) was added, and the resulting mixture was refluxed at 80 ° C for 2 h, and the solid product was separated by centrifugation to obtain a platinum catalyst supported on a hollow sphere of resorcinol-formaldehyde resin, which was marked as sample 11 # .

[0039] Take 0.04g of sample 11 # The catalyst and 5 ml of nitrobenzene toluene solution (0.1 M) were placed in a 40 ml stainless steel autoclave with a polytetrafluoroethylene liner. The air was purged with hydrogen and filled with hydrogen to a pressure of 0.3 MPa. The autoclave was placed in a 40°C water bath for 1 h and the products were analyzed.

[0040] The products were analyzed using an Agilent gas chromatograph 7890 with a FID detector and a FFAP capillary column.

[0041] The reaction results are as follows:

[0042] The nitrobenzene conversion was 100% and the aniline selectivity was 90.2%.

[0043] Example 7 Application of Materials

[0044] Weigh 0.2g of sample 4 # Dispersed in 5 ml of deionized water and 45 ml of ethanol, 0.5 g of chloroplatinic acid aqueous solution (77 mM) was added, and the resulting mixture was refluxed at 80 ° C for 2 h, and the solid product was separated by centrifugation to obtain a carbon-based hollow sphere-supported platinum catalyst, which was marked as sample 12 # .

[0045] Take 0.04g of sample 12 # The catalyst and 5 ml of nitrobenzene toluene solution (0.1 M) were placed in a 40 ml stainless steel autoclave with a polytetrafluoroethylene liner. The air was purged with hydrogen and filled with hydrogen to a pressure of 0.3 MPa. The autoclave was placed in a 40°C water bath for 1 h and the products were analyzed.

[0046] The products were analyzed using an Agilent gas chromatograph 7890 with a FID detector and a FFAP capillary column.

[0047] The reaction results are as follows:

[0048] The conversion rate of nitrobenzene was 90.1%, and the selectivity of o-chloroaniline was 89.2%.

[0049] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. Application of a product obtained by a method for preparing a carbon-based hollow sphere material in a catalyst carrier for preparing aniline by hydrogenation of nitrobenzene, characterized in that: Take 0.1g dodecylamine and 0.12g n-hexane and dissolve them in 25ml ethanol, add 60ml deionized water and 0.2g 25-28wt% ammonia water and mix well, add 0.2g resorcinol and 0.3g 37wt% formaldehyde solution, stir continuously at 30°C for 24h, separate the solid product by centrifugation, and obtain resorcinol-formaldehyde resin hollow spheres after drying, which are recorded as sample 3 # ; Sample 3 # Heating at 500 °C for 4 h in a nitrogen atmosphere gave carbon-based hollow spheres; Weigh 0.2g of sample 3 # The mixture was dispersed in 5 ml of deionized water and 45 ml of ethanol, and 0.5 g of 77 mM chloroplatinic acid aqueous solution was added. The resulting mixture was refluxed at 80 ° C for 2 h, and the solid product was separated by centrifugation to obtain a platinum catalyst supported by hollow spheres of resorcinol-formaldehyde resin, which was marked as sample 11. # ; Take 0.04g of sample 11 # The catalyst and 5 ml of a 0.1 M toluene solution of nitrobenzene were placed in a 40 ml stainless steel autoclave lined with polytetrafluoroethylene, the air was purged with hydrogen, and the autoclave was filled with hydrogen to a pressure of 0.3 MPa. The autoclave was placed in a 40°C water bath for reaction for 1 h, and the product analysis was performed; the product analysis was performed using an Agilent gas chromatograph 7890, an FID detector, and an FFAP capillary column; the reaction results were as follows: the nitrobenzene conversion rate was 100%, and the aniline selectivity was 90.2%.