A heat conduction composite material component and a connection method thereof
By combining high-thermal conductivity carbon fiber cloth and adhesive at the connection of the thermal conductivity composite material, and using high-thermal conductivity pins or screws and ceramic precursor solutions, the problem of low mechanical properties and thermal conductivity at the connection of the thermal conductivity composite material is solved. Significantly improves the stability and service life of the product.
Patent Information
- Application Number
- CN202310882167.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-07-18
AI Technical Summary
The mechanical properties and thermal conductivity of the existing thermally conductive composite materials are low, resulting in the impact of safety and service life when used in high temperature environments.
Use high thermal conductivity carbon fiber cloth filling and high thermal conductivity adhesive to combine, use high thermal conductivity pins or screws through mechanical connection, and processed through the PIP process of ceramic precursor solution to form dense ceramic caulks with high thermal conductivity to enhance connection strength and thermal conductivity. performance.
It significantly improves the mechanical properties and thermal conductivity of the connections of thermally-conductive composites, extends the service life of the product, and improves the stability and safety in high temperature environments.
Smart Images

Figure BDA0004345142720000201 
Figure BDA0004345142720000202
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat conduction composite materials, and in particular relates to a heat conduction composite material component and a connection method thereof. Background Art
[0002] In the thermal control systems of products in the aerospace and other fields, high thermal conductivity materials can play the role of heat dissipation, equipment temperature equalization, and reduced contact thermal resistance. They can be widely used in instruments and equipment that need to enhance heat conduction. Among them, high-speed aircraft have high flight speeds and long flight times, which lead to high temperatures and prominent thermal stresses on the outer surface of the aircraft. If the heat continues to accumulate, it is likely to cause material failure. Therefore, high thermal conductivity materials are needed to transfer heat in a timely manner, simplify heat protection design, and increase aircraft stability. Aircraft products are large in size and quite complex in structure. It is necessary to prepare parts separately before assembling and installing them. The joints are generally the weak parts of the components, and the mechanical strength performance is relatively low. At the same time, there are often gaps in the joints, which may loosen during high and low temperature cycles, affecting product safety and stability. Especially for heat-conducting composite materials, the interface gaps at the joints will cause the interface thermal resistance to increase significantly, the thermal conductivity of the joints is low, and the heat conduction path is blocked, which greatly affects the overall heat dissipation effect and the safety and service life of the components when used in harsh environments. Chinese patent application CN201811363591.3 discloses a heat-conducting ceramic-based composite material and a preparation method thereof. The thermal conductivity of the material can reach about 120 W / (m·K) and the bending strength can reach 132 to 235 MPa. However, it does not involve how to solve the problems of low strength of existing heat-conducting composite material connectors and low interface thermal conductivity.
[0003] Therefore, there is an urgent need to provide a method for connecting and reinforcing heat-conducting composite materials and components to provide technical support for later applications. Summary of the invention
[0004] In order to solve one or more technical problems existing in the prior art, the present invention provides a heat conduction composite material component and a preparation method and application thereof. The method of the present invention can significantly enhance the mechanical properties and thermal conductivity of the connection of the heat conduction composite material, and improve the performance and stability of the product.
[0005] In a first aspect, the present invention provides a method for connecting heat-conducting composite material components, the method comprising the following steps:
[0006] (1) After coating a high thermal conductivity adhesive on the high thermal conductivity carbon fiber cloth and / or the position to be connected of the first thermal conductive composite material to be connected, the high thermal conductivity carbon fiber cloth is filled in the position to be connected of the first thermal conductive composite material to be connected to obtain a pretreated connecting part;
[0007] (2) applying a high thermal conductivity adhesive to the connection position of the pre-treated connection piece and / or the second thermal conductive composite material to be connected, and then connecting the second thermal conductive composite material to be connected to the connection position of the pre-treated connection piece to obtain an assembly;
[0008] (3) Mechanically connecting the assembly using high thermal conductivity pins and / or high thermal conductivity screws to obtain a connection piece;
[0009] (4) The connecting piece is treated by a PIP process of impregnation / curing / cracking using a ceramic precursor solution as an impregnation liquid to obtain a heat-conducting composite material component.
[0010] Preferably, the single filament diameter of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is 8 to 12 μm; the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 800 W / (m·K); the density of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 2.15 g / cm 3 ; The high thermal conductivity carbon fiber cloth is a unidirectional high thermal conductivity carbon fiber cloth or a bidirectional high thermal conductivity carbon fiber cloth, the high thermal conductivity carbon fibers in the bidirectional high thermal conductivity carbon fiber cloth are arranged in two directions, the ratio of the high thermal conductivity carbon fibers in the two directions is in the range of (1 to 5): 1, and the angle between the high thermal conductivity carbon fibers in the two directions is in the range of 30° to 90°; and / or the thickness of the high thermal conductivity carbon fiber cloth is in the range of 0.1 to 0.3 mm.
[0011] Preferably, the high thermal conductivity adhesive comprises an inorganic filler and a phenolic resin; the inorganic filler contains at least two of carbon, silicon, oxygen, zirconium, hafnium, boron and nitrogen, and must contain carbon. Preferably, the carbon in the inorganic filler is graphitized at 3000-3200°C, and the degree of graphitization is not less than 90%; the phenolic resin is a phenolic resin modified by one or more elements of Si, Ti, Zr and B. Preferably, the phenolic resin is a Si-Ti modified phenolic resin, and the viscosity of the Si-Ti modified phenolic resin is 500-800 mPa·s; preferably, the mass ratio of the inorganic filler to the phenolic resin is (1.2-1.5):1, and the room temperature thermal conductivity of the high thermal conductivity adhesive is not less than 25 W / (m·K).
[0012] Preferably, the high thermal conductivity adhesive is a high thermal conductivity, high toughness and high temperature resistant adhesive, and the high thermal conductivity, high toughness and high temperature resistant adhesive comprises a high thermal conductivity filler, a modified phenolic resin, a curing agent and a diluent; the mass ratio of the high thermal conductivity filler to the modified phenolic resin is (1.2-1.5):1; the high thermal conductivity filler comprises 50-60% of chopped high thermal conductivity carbon fiber and 40-50% of boride inorganic powder in terms of mass percentage; preferably, the length of the chopped high thermal conductivity carbon fiber is 100-500 μm, the room temperature axial thermal conductivity of the chopped high thermal conductivity carbon fiber is not less than 800 W / (m·K), and the density of the chopped high thermal conductivity carbon fiber is not less than 2.15 g / cm 3 ; and / or the single filament diameter of the short-cut high thermal conductivity carbon fiber is 8 to 12 μm; preferably, the boride inorganic powder comprises ZrB2 powder and / or HfB2 powder, and the particle size of the boride inorganic powder is 10 to 50 μm; preferably, the modified phenolic resin is a phenolic resin modified by one or more elements of Si, Ti, Zr, and B, and more preferably, the modified phenolic resin is a Si-Ti modified phenolic resin, and / or the viscosity of the modified phenolic resin is 500 to 800 mPa·s.
[0013] Preferably, the high thermal conductivity pin and / or high thermal conductivity screw is made of carbon fiber toughened ceramic matrix composite material; the carbon fiber toughened ceramic matrix composite material comprises a carbon fiber preform and a ceramic matrix; the carbon fiber preform is woven with high thermal conductivity carbon fiber or mixed with high thermal conductivity carbon fiber and non-high thermal conductivity carbon fiber, and the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber is not less than 800W / (m·K); the ceramic matrix is one or more of SiC, ZrC, HfC, TaC, SiBCN, and SiCN; the density of the high thermal conductivity pin and / or high thermal conductivity screw is 2.2-3.5g / cm 3 The room temperature thermal conductivity of the high thermal conductivity pin and / or high thermal conductivity screw in the axial direction of the high thermal conductivity fiber is 200 to 300 W / (m·K).
[0014] Preferably, the ceramic precursor solution is one or more of a SiC ceramic precursor solution, a ZrC ceramic precursor solution, a HfC ceramic precursor solution, a TaC ceramic precursor solution, a SiBCN ceramic precursor solution, a SiCN ceramic precursor solution, and a silicon-zirconium integrated precursor; the ceramic yield of the ceramic precursor is not less than 60%; and / or the viscosity of the ceramic precursor solution is 50 to 100 mPa·s.
[0015] Preferably, step (3) is: after coating the inner surface of the hole of the assembly and the surface of the high thermal conductivity pin and / or high thermal conductivity screw with a high thermal conductivity adhesive, the assembly is mechanically connected using the high thermal conductivity pin and / or high thermal conductivity screw, and then cured at 100-130° C. for 4-6 hours to obtain a connecting part.
[0016] Preferably, in step (4), the number of times of impregnation-curing-cracking is 3 to 5 times, and the cracking temperature is 1000 to 1500°C.
[0017] In a second aspect, the present invention provides a heat conducting composite material component obtained by the connection method described in the first aspect of the present invention.
[0018] Preferably, the flexural strength of the heat conducting composite material component is not less than 337 MPa, and the room temperature thermal conductivity of the heat conducting composite material component in the axial direction of the high thermal conductivity fiber is not less than 152 W / (m·K).
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] (1) The present invention adopts a four-in-one combination method of high thermal conductivity adhesive, high thermal conductivity carbon fiber cloth filling, high thermal conductivity screws and / or high thermal conductivity pins mechanical connection, and ceramic dense caulking, which significantly enhances the mechanical properties and thermal conductivity of the connection of the heat-conducting composite material and improves the performance and stability of the product.
[0021] (2) After coating the high thermal conductivity adhesive on the high thermal conductivity carbon fiber cloth and / or the position to be connected of the first thermal conductive composite material to be connected, the high thermal conductivity carbon fiber cloth is then filled in the position to be connected of the first thermal conductive composite material to be connected. By filling the high thermal conductivity carbon fiber cloth, the high thermal conductivity adhesive partially penetrates into the high thermal conductivity carbon fiber cloth, which can make the originally randomly distributed fillers present a similar orientation distribution in the high thermal conductivity carbon fiber cloth as a whole, which can make the high thermal conductivity carbon fiber cloth and the high thermal conductivity adhesive jointly form a thermal conductive path or a thermal conductive network, which can reduce the thermal resistance caused by the interface mismatch between the matrix and the filler, and greatly improve the thermal conductivity performance; the coordinated use of the high thermal conductivity carbon fiber cloth and the high thermal conductivity adhesive helps to enhance the thermal conductivity of the thermal conductive composite material component; in addition, the high thermal conductivity carbon fiber cloth and the thermal conductive composite material parts have similar physical properties such as thermal expansion coefficient and density, and have strong adaptability during connection, which can improve product performance and stability.
[0022] (3) In some preferred embodiments of the present invention, the high thermal conductivity adhesive used is a high thermal conductivity, high toughness, and high temperature resistant adhesive. The high thermal conductivity, high toughness, and high temperature resistant adhesive uses a suitable proportion of short-cut high thermal conductivity carbon fibers and boride micron-sized inorganic powder particles to fill and modify the adhesive. The synergistic effect of the two can optimize the heat transfer channel, which is conducive to the formation of a thermal conductive network and significantly improves the thermal conductivity of the adhesive. In addition, the phenolic resin modified by the active element is used to improve the mass retention rate of the phenolic resin after treatment at high temperature, improve the density of the adhesive, reduce the interface thermal resistance, and improve the thermal conductivity. The high thermal conductivity, high toughness, and high temperature resistant adhesive in the present invention uses short-cut high thermal conductivity carbon fibers. The micron-sized inorganic powder particles of fibers and boride synergistically enhance the fracture toughness of the adhesive. The use temperature range of the high thermal conductivity, high toughness and high temperature resistant adhesive is room temperature-1500°C. It can be configured and bonded to samples at room temperature. It has high bonding strength and thermal conductivity in the range from room temperature to high temperature, and has excellent bonding effect. At the same time, the adhesive has high fracture toughness after curing, which is beneficial to improving the repeatable service life of the bonded parts. The adhesive has high fracture toughness after curing and can be repeatedly used under hot and cold alternating conditions. The use of the high thermal conductivity, high toughness and high temperature resistant adhesive can further improve the mechanical properties and thermal conductivity of the joints of heat-conducting composite materials, and is more conducive to improving the performance and stability of the product. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] In a first aspect, the present invention provides a method for connecting heat-conducting composite material components, the method comprising the following steps:
[0025] (1) After coating the high thermal conductivity adhesive on the high thermal conductivity carbon fiber cloth and / or the position to be connected of the first thermal conductive composite material to be connected, the high thermal conductivity carbon fiber cloth is filled (pasted) at the position to be connected of the first thermal conductive composite material to be connected. Specifically, the high thermal conductivity carbon fiber cloth is pasted on the inner wall of the position to be connected of the first thermal conductive composite material to be connected to obtain a pre-treated connection part; during the filling, the side of the high thermal conductivity carbon fiber cloth coated with the high thermal conductivity adhesive is bonded and connected to the surface to be connected of the first thermal conductive composite material to be connected to obtain a pre-treated connection part; in the present invention, the first thermal conductive composite material to be connected has a groove (position to be connected), and the high thermal conductivity carbon fiber cloth is pasted on the inner wall of the groove;
[0026] (2) applying a high thermal conductivity adhesive to the pre-treated connector and / or the position to be connected of the second thermal conductive composite material to be connected, and then connecting the second thermal conductive composite material to be connected to the position to be connected of the pre-treated connector to obtain a composite member; in the present invention, the second thermal conductive composite material to be connected is connected to the groove pasted with the high thermal conductive carbon fiber cloth. Specifically, in step (2), a high thermal conductivity adhesive is applied to the side of the high thermal conductive carbon fiber cloth included in the pre-treated connector obtained in step (1) that is away from the first thermal conductive composite material to be connected and / or the position to be connected of the second thermal conductive composite material to be connected;
[0027] (3) Mechanically connecting the assembly using high thermal conductivity pins and / or high thermal conductivity screws to obtain a connection piece; in the present invention, holes matching the high thermal conductivity pins and / or high thermal conductivity screws are provided on the assembly to install the high thermal conductivity pins and / or high thermal conductivity screws so as to mechanically connect the assembly;
[0028] (4) Using a ceramic precursor solution as an impregnation liquid to treat the connector through a PIP process of impregnation / curing / cracking to obtain a heat-conducting composite material component; the present invention does not specifically limit the ceramic precursor solution, and those skilled in the art can conventionally select it. In the present invention, for example, a high-yield, low-viscosity ceramic precursor solution can be used as an impregnation liquid to carry out the PIP process; the present invention does not specifically limit the first heat-conducting composite material to be connected and the second heat-conducting composite material to be connected, for example, it is a heat-conducting ceramic-based composite material, prepared by a method in the prior art, for example, it can be prepared by referring to the method disclosed in CN109320278B. It is particularly noted that in the present invention, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance; for ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.
[0029] In the prior art, the first heat conducting composite material to be connected has a groove, and the second heat conducting composite material to be connected matches the shape of the groove. When connecting, the second heat conducting composite material to be connected is filled in the groove of the first heat conducting composite material to be connected. However, due to the microscopic flatness of the surface of the parts to be connected, if the second heat conducting composite material to be connected is directly connected to the first heat conducting composite material to be connected by an adhesive, a gap will still appear at the connection. In the present invention, by filling with high thermal conductivity carbon fiber cloth, the gap at the connection can be effectively reduced, which is conducive to improving the mechanical properties and thermal conductivity of the connection of the heat conducting composite material; by filling with high thermal conductivity carbon fiber cloth, the gap at the connection is filled, a tighter contact area is provided, and the mechanical strength of the connection point is enhanced. At the same time, the thermal conductivity of the high thermal conductivity carbon fiber cloth helps to effectively transfer heat, reduce the thermal resistance of the connection, and improve the thermal conductivity efficiency of the entire heat conducting composite material component; by filling with high thermal conductivity carbon fiber cloth, the present invention can significantly reduce the gap at the connection, ensuring that the mechanical properties and thermal conductivity of the connection of the heat conducting composite material component are significantly enhanced. Furthermore, after coating the high thermal conductivity adhesive on the high thermal conductivity carbon fiber cloth and / or the position to be connected of the first thermal conductive composite material to be connected, the high thermal conductivity carbon fiber cloth is filled in the position to be connected of the first thermal conductive composite material to be connected. By filling the high thermal conductivity carbon fiber cloth, the high thermal conductivity adhesive partially penetrates into the high thermal conductivity carbon fiber cloth, which can make the originally randomly distributed fillers present a similar orientation distribution in the high thermal conductivity carbon fiber cloth as a whole, which can make the high thermal conductivity carbon fiber cloth and the high thermal conductivity adhesive jointly form a thermal conductive path or a thermal conductive network, which can reduce the thermal resistance caused by the interface mismatch between the matrix and the filler, and greatly improve the thermal conductivity performance; the coordinated use of the high thermal conductivity carbon fiber cloth and the high thermal conductivity adhesive is even more helpful to enhance the thermal conductivity of the thermal conductive composite material component; in addition, the high thermal conductivity carbon fiber cloth and the thermal conductive composite material parts have similar physical properties such as thermal expansion coefficient and density, and have strong adaptability during connection, which can improve product performance and stability.
[0030] In addition, the present invention adopts high thermal conductivity pins and / or high thermal conductivity screws for the first time to mechanically connect the assembly. Compared with pins and / or screws made of metal materials (such as stainless steel), it can effectively solve the problems of thermal resistance and thermal expansion mismatch caused by traditional metal pins and screws, thereby ensuring that the mechanical properties and thermal conductivity of the connection are significantly enhanced. This connection method helps to improve the overall performance and reliability of the thermal conductive composite material assembly; the present invention adopts high thermal conductivity pins and / or high thermal conductivity screws to mechanically connect the assembly. The high thermal conductivity pins and / or high thermal conductivity screws can provide a good thermal conduction path, which is conducive to the transfer and dispersion of heat, thereby reducing the thermal resistance of the connection and improving The thermal conductivity efficiency of the entire thermally conductive composite material component is improved, and there are often different thermal expansion coefficients between the thermally conductive composite material and the metal material when the temperature changes. Compared with the use of metal pins and / or screws, the present invention uses high thermal conductivity pins and / or high thermal conductivity screws, whose thermal conductivity and thermal expansion coefficient are closer to those of the thermally conductive composite material, which can reduce stress concentration and structural damage caused by thermal expansion mismatch, and is beneficial to improving the mechanical properties and durability of the connection. Compared with metal pins and screws, high thermal conductivity pins and / or high thermal conductivity screws can not only reduce the overall weight of the assembly, but also provide better corrosion resistance, which can effectively extend the service life of the thermally conductive composite material component.
[0031] The present invention adopts a four-dimensional integrated method of high thermal conductivity adhesive, high thermal conductivity carbon fiber cloth filling, high thermal conductivity screws and / or high thermal conductivity pin mechanical connection, and ceramic dense caulking. Specifically, the present invention adopts high thermal conductivity carbon fiber cloth to fill the to-be-connected position of the thermal conductive composite material to be connected; adopts high thermal conductivity adhesive to fix and connect the connection parts of the thermal conductive composite material to be connected; adopts high thermal conductivity pins and / or high thermal conductivity screws to mechanically connect the thermal conductive composite material to be connected, and preferably adopts a high-yield low-viscosity ceramic precursor solution to impregnate-curing-cracking the assembly to form high thermal conductivity dense ceramics at the gap, which significantly enhances the mechanical properties and thermal conductivity of the connection of the thermal conductive composite material, and improves the performance and stability of the product.
[0032] According to some preferred embodiments, the high thermal conductivity carbon fiber cloth is made of high thermal conductivity carbon fiber, and the single fiber diameter of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is 8 to 12 μm; the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 800 W / (m·K); the density of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 2.15 g / cm 3; The high thermal conductivity carbon fiber cloth is a unidirectional high thermal conductivity carbon fiber cloth or a bidirectional high thermal conductivity carbon fiber cloth, the high thermal conductivity carbon fibers in the bidirectional high thermal conductivity carbon fiber cloth are arranged in two directions, the ratio of the high thermal conductivity carbon fiber content in the two directions is in the range of (1-5): 1, the angle between the high thermal conductivity carbon fibers in the two directions is 30°-90°; and / or the thickness of the high thermal conductivity carbon fiber cloth is in the range of 0.1-0.3 mm; In the present invention, the ratio of the high thermal conductivity carbon fiber content in the two directions refers to the ratio of the volume fraction of the high thermal conductivity carbon fibers in the two directions.
[0033] The present invention preferably uses high thermal conductivity carbon fiber cloth of appropriate thickness. The high thermal conductivity carbon fiber cloth can be a unidirectional or bidirectional structure. The fiber content in each direction in the bidirectional high thermal conductivity carbon fiber cloth can be designed and proportioned according to product performance requirements, which is beneficial to enhancing the mechanical properties of the material connection.
[0034] According to some preferred embodiments, the high thermal conductivity adhesive comprises an inorganic filler and a phenolic resin; the inorganic filler contains at least two of carbon, silicon, oxygen, zirconium, hafnium, boron and nitrogen, and must contain carbon. Preferably, the carbon in the inorganic filler is graphitized at 3000-3200°C, and the degree of graphitization is not less than 90%; the phenolic resin is a phenolic resin modified by one or more elements of Si, Ti, Zr and B. Preferably, the phenolic resin is a Si-Ti modified phenolic resin, and the viscosity of the Si-Ti modified phenolic resin is 500-800 mPa·s; preferably, the mass ratio of the inorganic filler to the phenolic resin is (1.2-1.5):1 (for example, 1.2:1, 1.3:1, 1.4:1 or 1.5:1), and the room temperature thermal conductivity of the high thermal conductivity adhesive is not less than 25 W / (m·K).
[0035] According to some preferred embodiments, the high thermal conductivity adhesive is a high thermal conductivity, high toughness, and high temperature resistant adhesive, and the high thermal conductivity, high toughness, and high temperature resistant adhesive comprises a high thermal conductivity filler, a modified phenolic resin, a curing agent, and a diluent; the mass ratio of the high thermal conductivity filler to the modified phenolic resin is (1.2 to 1.5): 1 (for example, 1.2: 1, 1.3: 1, 1.4: 1 or 1.5: 1); the high thermal conductivity filler comprises 50 to 60% (for example, 5 0%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or 60%) of chopped high thermal conductive carbon fiber and 40-50% (for example 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%) of boride inorganic powder; in the present invention, the chopped high thermal conductive carbon fiber is also referred to as high thermal conductive chopped carbon fiber; the boride inorganic powder is also referred to as boride ceramic powder.
[0036] The present invention preferably uses the high thermal conductivity adhesive as a high thermal conductivity, high toughness, and high temperature resistant adhesive. The high thermal conductivity, high toughness, and high temperature resistant adhesive uses high thermal conductivity chopped carbon fibers of different sizes, i.e., a length of 100 to 500 μm and a boride inorganic powder with a high thermal conductivity of 10 to 50 μm as high thermal conductivity fillers in synergistic combination, and reasonably controls the ratio of the two, and optimizes the formula of the high thermal conductivity filler. The synergistic effect of the two can optimize the heat transfer channel, form a thermal conductive network, and significantly improve the adhesive. Thermal conductivity; In the present invention, preferably, the high thermal conductivity filler comprises 50-60% of short-cut high thermal conductivity carbon fiber and 40-50% of boride inorganic powder in terms of mass percentage. By selecting a suitable ratio, the two fillers are combined together to form a more effective thermal conductivity network, thereby improving the overall thermal conductivity of the adhesive. In addition, by selecting a suitable ratio, a balance between toughness and hardness and high temperature stability between the short-cut high thermal conductivity carbon fiber and zirconium boride can be achieved, so that the adhesive has The invention has high toughness, can resist external impact and stress, and has high bonding strength at high temperature; at the same time, the high thermal conductivity, high toughness and high temperature resistant adhesive adopts phenolic resin modified by active elements to improve the mass retention rate of phenolic resin after treatment at high temperature, improve the density of adhesive, reduce interface thermal resistance, and improve thermal conductivity; the thermal conductive composite material component of the invention has a wide operating temperature range of room temperature to 1500°C, the thermal conductive composite material component of the invention has low cost, short preparation cycle, simple process, high bonding strength in the range of room temperature to high temperature, and excellent bonding effect; the invention adopts short-cut high thermal conductivity carbon fiber and boride micron-sized inorganic powder particles to synergistically enhance the fracture toughness of the adhesive and improve the repeatable service life of the adhesive. After the adhesive is cured, the fracture toughness is high and it can be reused under hot and cold alternating conditions. The use of the high thermal conductivity, high toughness and high temperature resistant adhesive can further improve the mechanical properties and thermal conductivity of the connection of the thermal conductive composite material component, which is more conducive to improving the performance and stability of the product.
[0037] According to some preferred embodiments, in the high thermal conductivity, high toughness and high temperature resistant adhesive, the length of the short chopped high thermal conductivity carbon fiber is 100-500 μm; the room temperature axial thermal conductivity of the short chopped high thermal conductivity carbon fiber is not less than 800 W / (m·K); in the present invention, the short chopped high thermal conductivity carbon fiber refers to the short chopped high thermal conductivity carbon fiber whose axial thermal conductivity is not less than 800 W / (m·K) at room temperature (for example, room temperature 15-35°C). The short chopped high thermal conductivity carbon fiber in the present invention is made of high thermal conductivity carbon fiber. The present invention does not specifically limit the source of the high thermal conductivity carbon fiber, and can use products that can be purchased on the market or products synthesized by existing methods; the density of the short chopped high thermal conductivity carbon fiber is not less than 2.15 g / cm 3 ; and / or the single fiber diameter of the short-cut high thermal conductivity carbon fiber is 8 to 12 μm.
[0038] According to some preferred embodiments, in the high thermal conductivity, high toughness and high temperature resistant adhesive, the boride inorganic powder contains ZrB2 powder and / or HfB2 powder. Preferably, the boride inorganic powder is ZrB2 powder; and / or the particle size of the boride inorganic powder is 10 to 50 μm.
[0039] According to some preferred embodiments, in the high thermal conductivity, high toughness and high temperature resistant adhesive, the modified phenolic resin is a phenolic resin modified by one or more elements of Si, Ti, Zr and B. Preferably, the modified phenolic resin is a Si-Ti modified phenolic resin (also referred to as silicon-titanium modified phenolic resin); the present invention does not specifically limit the source of the Si-Ti modified phenolic resin, which may be a product that can be directly purchased on the market or a product synthesized by an existing method; and / or the viscosity of the modified phenolic resin is 500 to 800 mPa·s (for example, 500, 600, 700 or 800 mPa·s).
[0040] According to some preferred embodiments, in the high thermal conductivity, high toughness and high temperature resistant adhesive, the mass ratio of the curing agent to the modified phenolic resin is (0.06-0.15):1 (for example, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.13:1, 0.14:1 or 0.15:1), preferably, the curing agent is triethylenetetramine; and / or the mass ratio of the diluent to the modified phenolic resin is (0.1-0.3):1 (for example, 0.1:1, 0.15:1, 0.2:1, 0.25:1 or 0.3:1), preferably, the diluent is butyl acetate.
[0041] According to some preferred embodiments, the room temperature thermal conductivity of the high thermal conductivity, high toughness and high temperature resistant adhesive is 25 to 30 W / (m·K); the room temperature fracture toughness of the high thermal conductivity, high toughness and high temperature resistant adhesive is 10 to 16 MPa·m 1 / 2 ; and / or the bonding strength of the high thermal conductivity, high toughness and high temperature resistant adhesive at 1500°C is 5 to 8 MPa; in the present invention, the high thermal conductivity, high toughness and high temperature resistant adhesive refers to an adhesive having a room temperature thermal conductivity of up to 25 to 30 W / (m·K) and a room temperature fracture toughness of up to 10 to 16 MPa·m 1 / 2 High temperature resistant adhesive.
[0042] According to some preferred embodiments, the high thermal conductivity, high toughness and high temperature resistant adhesive further comprises a filler auxiliary agent, the filler auxiliary agent is nano alumina powder (nano Al2O3 powder), the particle size of the nano alumina powder can be, for example, 20 to 50 nm, and the amount of the nano alumina powder is 5 to 20% (for example, 5%, 6%, 7%, 8%, 9%, 10%, 12%, 15%, 18% or 20%) of the mass of the high thermal conductivity filler; the present invention finds that the addition of an appropriate amount of nano alumina powder can further improve the high thermal conductivity, high toughness and high temperature resistant adhesive. The possible reason for the improvement in toughness and bonding strength at high temperatures is that the addition of nano-alumina powder can reduce the expansion and thermal deformation of high-temperature resistant adhesives, because nano-sized particles have a larger specific surface area and better dispersibility, which helps to reduce the thermal stress and thermal expansion of the adhesive in a high-temperature environment, thereby improving the interfacial adhesion and high-temperature resistant bonding strength; in addition, the small size of nano-alumina powder enables it to better fill the defects and pores between the filler and the resin matrix, increase the overall tightness and stability of the adhesive, and help improve the overall toughness and stability of the adhesive.
[0043] According to some specific embodiments, the high thermal conductivity, high toughness and high temperature resistant adhesive used in the present invention includes: a high thermal conductivity filler, a modified phenolic resin, a curing agent and a diluent; the high thermal conductivity, high toughness and high temperature resistant adhesive is composed of 52wt% of a high thermal conductivity filler, 40wt% of a modified phenolic resin, 4wt% of a curing agent and 4wt% of a diluent, and in the high thermal conductivity filler, the mass ratio of high thermal conductivity chopped carbon fiber to ZrB2 ceramic powder is 7:6; the length of the high thermal conductivity chopped carbon fiber is 100-500μm, the axial thermal conductivity at room temperature is not less than 800W / (m·K), and the density is not less than 2.15g / cm 3 The diameter of the single wire is 11 μm, the particle size of the ZrB2 ceramic powder is 10-50 μm, the modified phenolic resin is Si-Ti modified phenolic resin, the viscosity of the modified phenolic resin is 800 mPa·s, the curing agent is triethylenetetramine, and the diluent is butyl acetate.
[0044] According to some preferred embodiments, the preparation of the high thermal conductivity, high toughness and high temperature resistant adhesive comprises the following steps:
[0045] (a) uniformly mixing short-cut high thermal conductivity carbon fibers, boride inorganic powder and solvent, and then drying to obtain a high thermal conductivity filler; specifically, for example, stirring and ultrasonicating a mixture of the high thermal conductivity short-cut carbon fibers, boride inorganic powder and solvent, and then drying to obtain the high thermal conductivity filler;
[0046] (b) the high thermal conductivity filler, modified phenolic resin, curing agent and diluent are mixed uniformly to obtain a high thermal conductivity, high toughness and high temperature resistant adhesive. For example, the high thermal conductivity filler, modified phenolic resin, curing agent and diluent can be mixed and then mixed uniformly by stirring and ultrasonication. The present invention does not specifically limit the stirring and ultrasonication conditions, and those skilled in the art can make conventional selections. Optionally, a filler auxiliary agent is also added in step (b), that is, step (b) is: the high thermal conductivity filler, filler auxiliary agent, modified phenolic resin, curing agent and diluent are mixed uniformly to obtain a high thermal conductivity, high toughness and high temperature resistant adhesive.
[0047] In the present invention, the high thermal conductivity, high toughness and high temperature resistant adhesive has a short preparation cycle, low cost and broad market prospects, and can be promoted for use.
[0048] According to some preferred embodiments, in step (a): the solvent is an alcohol and / or ketone organic solvent, preferably, the solvent is acetone; the amount of the solvent is 0.8 to 2 times (for example, 0.8, 0.9, 1, 1.2, 1.5, 1.8 or 2 times) the sum of the mass amounts of the chopped high thermal conductive carbon fiber and the boride inorganic powder; and / or the drying is carried out at 100 to 150°C (for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C).
[0049] According to some preferred embodiments, the high thermal conductivity pin and / or high thermal conductivity screw is made of carbon fiber toughened ceramic matrix composite material; the carbon fiber toughened ceramic matrix composite material comprises a carbon fiber preform and a ceramic matrix; the carbon fiber preform is woven from high thermal conductivity carbon fiber alone or mixed with high thermal conductivity carbon fiber and non-high thermal conductivity carbon fiber, and the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber is not less than 800W / (m·K); in the present invention, the non-high thermal conductivity carbon fiber can be, for example, polyacrylonitrile-based carbon fiber; the carbon fiber preform adopts a needle-punched structure, a sutured structure or a fine-woven puncture structure; the ceramic matrix is one or more of SiC, ZrC, HfC, TaC, SiBCN, and SiCN; the density of the high thermal conductivity pin and / or high thermal conductivity screw is 2.2-3.5g / cm 3 ; The room temperature thermal conductivity of the high thermal conductivity pin and / or high thermal conductivity screw in the axial direction of the high thermal conductivity fiber is 200-300 W / (m·K); In the present invention, the preparation of the carbon fiber toughened ceramic-based composite material is a conventional technology in the field, for example, it can be prepared by referring to the method disclosed in CN113563091B.
[0050] According to some preferred embodiments, in step (4), the ceramic precursor solution is one or more of a SiC ceramic precursor solution, a ZrC ceramic precursor solution, a HfC ceramic precursor solution, a TaC ceramic precursor solution, a SiBCN ceramic precursor solution, a SiCN ceramic precursor solution, and a silicon-zirconium integrated precursor (also referred to as a silicon-hafnium integrated ceramic precursor solution); the ceramic yield of the ceramic precursor is not less than 60%; and / or the viscosity of the ceramic precursor solution is 50 to 100 mPa·s.
[0051] According to some preferred embodiments, before performing step (1) and step (2), dust and stains on the surfaces of the first thermal conductive composite material to be connected and the second thermal conductive composite material to be connected are first wiped off with a solvent (preferably acetone).
[0052] According to some preferred embodiments, step (3) is: after coating the inner surface of the hole of the assembly and the surface of the high thermal conductivity pin and / or high thermal conductivity screw with a high thermal conductivity adhesive, the assembly is mechanically connected using the high thermal conductivity pin and / or high thermal conductivity screw, and then cured at 100-130°C (for example, 100°C, 110°C, 120°C or 130°C) for 4-6h (for example, 4, 4.5, 5, 5.5 or 6h) to obtain a connector.
[0053] According to some specific embodiments, the high thermal conductivity pins and / or high thermal conductivity screws and the matching pin holes and / or threaded holes in the assembly are first cleaned with a solvent (preferably acetone), and a high thermal conductivity adhesive is evenly coated in the holes and on the surfaces of the high thermal conductivity pins and / or high thermal conductivity screws, and the assembly is further mechanically fixed and connected. After the assembly is placed in an air environment and cured at 100-130° C. for 4-6 hours, the excess high thermal conductivity adhesive around the connection is polished off with sandpaper to obtain the connector.
[0054] According to some preferred embodiments, in step (4), the number of times of impregnation-curing-cracking is 3 to 5 times (for example, 3, 4 or 5 times), and the cracking temperature is 1000 to 1500°C (for example, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C or 1500°C).
[0055] In a second aspect, the present invention provides a heat conducting composite material component obtained by the connection method described in the first aspect of the present invention.
[0056] According to some preferred embodiments, the flexural strength of the heat conducting composite material component is not less than 337 MPa, and the room temperature thermal conductivity of the heat conducting composite material component in the axial direction of the high thermal conductivity fiber is not less than 152 W / (m·K).
[0057] The present invention is further described below in conjunction with the examples. These examples are only used to illustrate the preferred embodiments of the present invention, and the protection scope of the present invention should not be interpreted as being limited to these examples.
[0058] Example 1
[0059] This embodiment provides a method for connecting heat-conducting ceramic-based composite material components, which specifically includes the following steps:
[0060] (1) scrubbing the first thermal conductive ceramic matrix composite material to be connected with acetone, then coating the high thermal conductive adhesive on the high thermal conductive carbon fiber cloth and the connection position of the first thermal conductive ceramic matrix composite material to be connected, and then filling the high thermal conductive carbon fiber cloth at the connection position of the first thermal conductive ceramic matrix composite material to be connected to obtain a pretreated connection part; the single fiber diameter of the high thermal conductive carbon fiber in the high thermal conductive carbon fiber cloth is 11 μm; the room temperature axial thermal conductivity of the high thermal conductive carbon fiber in the high thermal conductive carbon fiber cloth is 800 W / (m·K); the density of the high thermal conductive carbon fiber in the high thermal conductive carbon fiber cloth is 2.20 g / cm 3 The high thermal conductivity carbon fiber cloth has a bidirectional structure, the ratio of the high thermal conductivity carbon fibers in the two directions is 1:1, the angle between the high thermal conductivity carbon fibers in the two directions is 90°, and the thickness of the high thermal conductivity carbon fiber cloth is 0.18 mm.
[0061] (2) scrubbing the second thermal conductive ceramic-based composite material to be connected with acetone, applying a high thermal conductive adhesive to the positions to be connected of the pretreated connecting member and the second thermal conductive ceramic-based composite material to be connected, and then connecting the second thermal conductive ceramic-based composite material to be connected to the position to be connected of the pretreated connecting member to obtain an assembly;
[0062] (3) Cleaning the holes of the assembly and the high thermal conductivity screws with acetone, applying a high thermal conductivity adhesive on the inner surface of the hole of the assembly and the surface of the high thermal conductivity screw, mechanically fixing and connecting the assembly with the high thermal conductivity screws, and then curing at 130° C. in an air atmosphere for 4 hours, sanding off the excess high thermal conductivity adhesive around the connection to obtain a connection piece; the assembly is provided with a hole matching the high thermal conductivity screw for installing the high thermal conductivity screw; the high thermal conductivity screw is made of a carbon fiber toughened ceramic matrix composite material; the carbon fiber toughened ceramic matrix composite material comprises a carbon fiber preform and a ceramic matrix; the carbon fiber preform is made of a mixed weaving of high thermal conductivity carbon fiber and non-high thermal conductivity carbon fiber (polyacrylonitrile-based carbon fiber), and the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber is 800 W / (m·K); the ceramic matrix is a SiC, TaC and HfC matrix; the room temperature thermal conductivity of the carbon fiber toughened ceramic matrix composite material used in the high thermal conductivity screw in the axial direction of the high thermal conductivity fiber is 253 W / (m·K).
[0063] (4) A ceramic precursor solution is used as an impregnation liquid to treat the connector through a PIP process of impregnation / curing / cracking to obtain a heat-conducting ceramic-based composite material component; the PIP process is specifically as follows: the connector is impregnated, cured and cracked in a silicon-zirconium integrated ceramic precursor solution for 4 rounds, in which the molar ratio of zirconium to silicon is 4:1, the viscosity of the silicon-zirconium integrated ceramic precursor solution is 80 mPa·s, and the ceramic yield is 65%; the impregnation is carried out in the following manner: the connector is immersed in the silicon-zirconium integrated ceramic precursor solution, vacuumed, immersed in a vacuum state for 1 hour, and then immersed at 2 MPa for 1 hour; the curing is carried out at 300°C and 1.5 MPa for 1 hour; the cracking is carried out at 1500°C for 2 hours.
[0064] In step (1), step (2) and step (3), the high thermal conductivity adhesive used is a high thermal conductivity, high toughness and high temperature resistant adhesive, and the high thermal conductivity, high toughness and high temperature resistant adhesive comprises the following components:
[0065] 5.2 parts by weight of high thermal conductivity filler, consisting of 2.8 parts by weight of short-cut high thermal conductivity carbon fiber and 2.4 parts by weight of ZrB2 powder;
[0066] 4.0 parts by weight of Si-Ti modified phenolic resin (silicon-titanium modified phenolic resin);
[0067] 0.4 parts by weight of triethylenetetramine (curing agent);
[0068] Butyl acetate (diluent) 0.4 parts by weight.
[0069] The preparation of the high thermal conductivity, high toughness and high temperature resistant adhesive comprises the following steps:
[0070] In the first step, 2.8 parts by weight of short-cut high thermal conductivity carbon fiber with a length of 200 μm, a diameter of 11 μm, and an axial thermal conductivity of 800 W / (m·K) at room temperature and 2.4 parts by weight of ZrB2 powder with a particle size of 10-50 μm were selected, 7.9 parts by weight of acetone were added, mechanically stirred for 10 minutes, and then placed in an ultrasonic disperser for ultrasonic dispersion for 10 minutes to obtain a mixed powder filler, and then the mixed powder filler was placed in an oven at 110°C and dried for 2 hours to obtain a high thermal conductivity filler.
[0071] In the second step, the high thermal conductivity filler obtained in the above step is evenly mixed with 4 parts by weight of Si-Ti modified phenolic resin, and after adding 0.4 parts by weight of triethylenetetramine and 0.4 parts by weight of butyl acetate, mechanically stirred for 10 minutes and ultrasonically dispersed for 10 minutes, mixed evenly without obvious bubbles, to obtain the high thermal conductivity, high toughness and high temperature resistant adhesive.
[0072] The high thermal conductivity, high toughness and high temperature resistant adhesive in this embodiment was processed into thermal conductivity and fracture toughness test specimens after being cured at 130°C for 4 hours. It was measured that the thermal conductivity of the high thermal conductivity, high toughness and high temperature resistant adhesive at room temperature was 30W / (m·K) and the room temperature fracture toughness was 13.4MPa·m 1 / 2 .
[0073] In this embodiment, the high thermal conductivity, high toughness and high temperature resistant adhesive is also used to bond two C / SiC ceramic-based composite substrates. After curing at 130°C for 4 hours and keeping at 1500°C in air atmosphere for 5 minutes, the bonding strength is measured to be 6.6 MPa in 1500°C in air atmosphere.
[0074] After the first heat-conducting ceramic-based composite material to be connected and the second heat-conducting ceramic-based composite material to be connected are connected and reinforced by the above-mentioned steps (1) to (4), the bending strength of the obtained heat-conducting ceramic-based composite material integral connection part (component) is 337 MPa, and the room temperature thermal conductivity of the integral connection part in the axial direction of the high thermal conductivity carbon fiber is 152 W / (m·K).
[0075] Example 2
[0076] Embodiment 2 is substantially the same as Embodiment 1, except that:
[0077] The high thermal conductivity adhesive used in this embodiment is different from that in Embodiment 1, specifically, the difference is:
[0078] The high thermal conductivity, high toughness and high temperature resistant adhesive used in this embodiment comprises the following components:
[0079] 5.2 parts by weight of high thermal conductive filler, consisting of 2.8 parts by weight of chopped high thermal conductivity carbon fiber and 2.4 parts by weight of ZrB2 powder;
[0080] Filler additive: 0.52 parts by weight of nano-alumina powder;
[0081] 4.0 parts by weight of Si-Ti modified phenolic resin (silicon-titanium modified phenolic resin);
[0082] 0.4 parts by weight of triethylenetetramine (curing agent);
[0083] Butyl acetate (diluent) 0.4 parts by weight;
[0084] The preparation of the high thermal conductivity, high toughness and high temperature resistant adhesive comprises the following steps:
[0085] In the first step, 2.8 parts by weight of short-cut high thermal conductivity carbon fiber with a length of 200 μm, a diameter of 11 μm, and an axial thermal conductivity of 800 W / (m·K) at room temperature and 2.4 parts by weight of ZrB2 powder with a particle size of 10-50 μm were selected, 7.9 parts by weight of acetone were added, mechanically stirred for 10 minutes, and then placed in an ultrasonic disperser for ultrasonic dispersion for 10 minutes to obtain a mixed powder filler, and then the mixed powder filler was placed in an oven at 110°C and dried for 2 hours to obtain a high thermal conductivity filler.
[0086] In the second step, the high thermal conductive filler obtained in the above step, 0.52 parts by weight of nano-alumina powder with a particle size of 20 to 50 nm and 4 parts by weight of Si-Ti modified phenolic resin are uniformly mixed, and after adding 0.4 parts by weight of triethylenetetramine and 0.4 parts by weight of butyl acetate, mechanical stirring is performed for 10 minutes and ultrasonic dispersion is performed for 10 minutes. The mixture is mixed evenly without obvious bubbles to obtain a high thermal conductive, high toughness and high temperature resistant adhesive.
[0087] Example 3
[0088] Embodiment 3 is substantially the same as Embodiment 1, except that:
[0089] The high thermal conductivity adhesive used in this embodiment is different from that in Example 1. Specifically, the high thermal conductivity filler in the high thermal conductivity adhesive in this embodiment is composed of 1.82 parts by weight of chopped high thermal carbon fiber and 3.38 parts by weight of ZrB2 powder;
[0090] In the first step, 1.82 parts by weight of short-cut high thermal conductivity carbon fibers with a length of 200 μm, a diameter of 11 μm, and an axial thermal conductivity of 800 W / (m·K) at room temperature and 3.38 parts by weight of ZrB2 powder with a particle size of 10-50 μm were selected, 7.9 parts by weight of acetone were added, and the mixture was mechanically stirred for 10 minutes and then placed in an ultrasonic disperser for ultrasonic dispersion for 10 minutes to obtain a mixed powder filler. The mixed powder filler was then placed in an oven at 110°C and dried for 2 hours to obtain a high thermal conductivity filler.
[0091] Example 4
[0092] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0093] The high thermal conductivity adhesive used in this embodiment is different from that in Example 1. Specifically, the high thermal conductivity filler in the high thermal conductivity adhesive in this embodiment is composed of 3.9 parts by weight of chopped high thermal conductivity carbon fibers and 1.3 parts by weight of ZrB2 powder;
[0094] In the first step, 3.9 parts by weight of short-cut high thermal conductivity carbon fibers with a length of 200 μm, a diameter of 11 μm, and an axial thermal conductivity of 800 W / (m·K) at room temperature and 1.3 parts by weight of ZrB2 powder with a particle size of 10-50 μm were selected, 7.9 parts by weight of acetone were added, and the mixture was mechanically stirred for 10 minutes and then placed in an ultrasonic disperser for ultrasonic dispersion for 10 minutes to obtain a mixed powder filler. The mixed powder filler was then placed in an oven at 110°C and dried for 2 hours to obtain a high thermal conductivity filler.
[0095] Example 5
[0096] Example 5 is basically the same as Example 1, except that: the high thermal conductivity adhesive used in this embodiment is different from that in Example 1, specifically, the high thermal conductivity filler in the high thermal conductivity adhesive in this embodiment is composed of 2.8 parts by weight of chopped high thermal conductivity carbon fiber and 2.4 parts by weight of B4C powder;
[0097] In the first step, 2.8 parts by weight of short-cut high thermal conductivity carbon fiber with a length of 200 μm, a diameter of 11 μm, and an axial thermal conductivity of 800 W / (m·K) at room temperature and 2.4 parts by weight of B4C powder with a particle size of 10-50 μm were selected, 7.9 parts by weight of acetone were added, and the mixture was mechanically stirred for 10 minutes and then placed in an ultrasonic disperser for ultrasonic dispersion for 10 minutes to obtain a mixed powder filler. The mixed powder filler was then placed in an oven at 110°C and dried for 2 hours to obtain a high thermal conductivity filler.
[0098] It is particularly noted that in each specific embodiment, the unit of weight parts can be unified as a weight unit such as "g" or "kg".
[0099] Comparative Example 1
[0100] (1) scrubbing the first thermal conductive ceramic-based composite material to be connected and the second thermal conductive ceramic-based composite material to be connected with acetone, then applying a high thermal conductive adhesive to the positions to be connected of the first thermal conductive ceramic-based composite material to be connected and the second thermal conductive ceramic-based composite material to be connected, and then connecting the second thermal conductive ceramic-based composite material to be connected to the position to be connected of the first thermal conductive ceramic-based composite material to be connected, to obtain an assembly;
[0101] (2) Cleaning the holes of the assembly and the high thermal conductivity screws with acetone, applying a high thermal conductivity adhesive on the inner surface of the hole of the assembly and the surface of the high thermal conductivity screw, mechanically fixing and connecting the assembly with the high thermal conductivity screws, and then curing at 130° C. for 4 hours in an air atmosphere, sanding off the excess high thermal conductivity adhesive around the connection with sandpaper to obtain a connection piece; mechanically connecting the assembly with the high thermal conductivity screws to obtain a connection piece; a hole matching the high thermal conductivity screw is provided on the assembly for installing the high thermal conductivity screw; the high thermal conductivity screw is The carbon fiber-reinforced ceramic-based composite material comprises a carbon fiber preform and a ceramic matrix; the carbon fiber preform is woven by mixing high thermal conductivity carbon fiber and non-high thermal conductivity carbon fiber (polyacrylonitrile-based carbon fiber), and the room temperature axial thermal conductivity of the high thermal conductivity carbon fiber is 800W / (m·K); the ceramic matrix is a SiC, TaC and HfC matrix; the room temperature thermal conductivity of the carbon fiber-reinforced ceramic-based composite material used in the high thermal conductivity screw in the axial direction of the high thermal conductivity fiber is 253W / (m·K).
[0102] (3) A ceramic precursor solution is used as an impregnation liquid to treat the connector through a PIP process of impregnation / curing / cracking to obtain a heat-conducting ceramic-based composite material component; the PIP process is specifically as follows: the connector is impregnated, cured and cracked in a silicon-zirconium integrated ceramic precursor solution for 4 rounds, in which the molar ratio of zirconium to silicon is 4:1, the viscosity of the silicon-zirconium integrated ceramic precursor solution is 80 mPa·s, and the ceramic yield is 65%; the impregnation is carried out in the following manner: the connector is immersed in the silicon-zirconium integrated ceramic precursor solution, vacuumed, immersed in a vacuum state for 1 hour, and then immersed at 2 MPa for 1 hour; the curing is carried out at 300°C and 1.5 MPa for 1 hour; the cracking is carried out at 1500°C for 2 hours.
[0103] In step (1) and step (2), the high thermal conductivity adhesive used is the same as that in Example 1.
[0104] The present invention also conducted the same test as in Example 1 on the adhesives used in Examples 2 to 5, and obtained the performance indicators of the adhesives in each example as shown in Table 1.
[0105] Table 1: Performance indicators of the adhesives in Examples 1 to 5.
[0106]
[0107] The present invention also conducted the same tests as in Example 1 on the heat-conducting ceramic-based composite material components of Examples 2 to 5 and Comparative Example 1, and obtained performance indicators of each heat-conducting ceramic-based composite material component as shown in Table 2.
[0108] Table 2: Performance indicators of the heat-conducting ceramic-based composite components in Examples 1 to 5 and Comparative Example 1.
[0109]
[0110] In Table 1 and Table 2, the symbol “-” indicates that the performance indicator has not been tested.
[0111] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for connecting heat-conducting composite material components, It is characterized in that The method comprises the following steps: (1) After coating a high thermal conductivity adhesive on the high thermal conductivity carbon fiber cloth and / or the position to be connected of the first thermal conductive composite material to be connected, the high thermal conductivity carbon fiber cloth is filled in the position to be connected of the first thermal conductive composite material to be connected to obtain a pretreated connecting part; (2) applying a high thermal conductivity adhesive to the connection position of the pre-treated connection piece and / or the second thermal conductive composite material to be connected, and then connecting the second thermal conductive composite material to be connected to the connection position of the pre-treated connection piece to obtain an assembly; (3) After applying a high thermal conductivity adhesive on the inner surface of the hole of the assembly and the surface of the high thermal conductivity pin and / or high thermal conductivity screw, the assembly is mechanically connected using the high thermal conductivity pin and / or high thermal conductivity screw, and then cured at 100 to 130° C. for 4 to 6 hours to obtain a connecting piece; the high thermal conductivity pin and / or high thermal conductivity screw are made of a carbon fiber toughened ceramic matrix composite material; the carbon fiber toughened ceramic matrix composite material comprises a carbon fiber preform and a ceramic matrix; the carbon fiber preform is woven from high thermal conductivity carbon fiber or woven from a mixture of high thermal conductivity carbon fiber and non-high thermal conductivity carbon fiber; (4) The connecting piece is treated by a PIP process of impregnation / curing / cracking using a ceramic precursor solution as an impregnation liquid to obtain a heat-conducting composite material component; the flexural strength of the heat-conducting composite material component is not less than 337 MPa, and the room temperature thermal conductivity of the heat-conducting composite material component in the axial direction of the high thermal conductivity fiber is not less than 152 W / (m·K); In step (1), step (2) and step (3), the high thermal conductivity adhesive is a high thermal conductivity, high toughness and high temperature resistant adhesive, and the high thermal conductivity, high toughness and high temperature resistant adhesive comprises a high thermal conductivity filler, a modified phenolic resin, a curing agent and a diluent; The mass ratio of the high thermal conductive filler to the modified phenolic resin is (1.2-1.5):1; The high thermal conductivity filler comprises 50-60% by mass of chopped high thermal conductivity carbon fibers and 40-50% by mass of boride inorganic powder; The length of the short-cut high thermal conductivity carbon fiber is 100-500 μm, and the single fiber diameter of the short-cut high thermal conductivity carbon fiber is 8-12 μm; The boride inorganic powder contains ZrB 2 Powder and / or HfB 2 The boride inorganic powder has a particle size of 10 to 50 μm; the room temperature thermal conductivity of the high thermal conductivity, high toughness and high temperature resistant adhesive is 25 to 30 W / (m·K); the room temperature fracture toughness of the high thermal conductivity, high toughness and high temperature resistant adhesive is 10 to 16 MPa·m 1 / 2 The bonding strength of the high thermal conductivity, high toughness and high temperature resistant adhesive at 1500°C is 5 to 8 MPa.
2. The connection method according to claim 1, Features: The single fiber diameter of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is 8 to 12 μm; The room temperature axial thermal conductivity of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 800 W / (m·K); The density of the high thermal conductivity carbon fiber in the high thermal conductivity carbon fiber cloth is not less than 2.15g / cm 3 ; The high thermal conductivity carbon fiber cloth is a unidirectional high thermal conductivity carbon fiber cloth or a bidirectional high thermal conductivity carbon fiber cloth, the high thermal conductivity carbon fibers in the bidirectional high thermal conductivity carbon fiber cloth are arranged in two directions, the ratio of the high thermal conductivity carbon fibers in the two directions is in the range of (1-5):1, and the angle between the high thermal conductivity carbon fibers in the two directions is in the range of 30°-90°; and / or The thickness of the high thermal conductivity carbon fiber cloth is in the range of 0.1 to 0.3 mm.
3. The connection method according to claim 1, Features: The room temperature axial thermal conductivity of the short-cut high thermal conductivity carbon fiber is not less than 800 W / (m·K), and the density of the short-cut high thermal conductivity carbon fiber is not less than 2.15 g / cm 3 ; and / or The modified phenolic resin is a phenolic resin modified by one or more elements of Si, Ti, Zr and B.
4. The connection method according to claim 3, Features: The modified phenolic resin is Si-Ti modified phenolic resin, and / or the viscosity of the modified phenolic resin is 500-800 mPa·s.
5. The connection method according to claim 1, Features: The room temperature axial thermal conductivity of the high thermal conductivity carbon fiber used in the carbon fiber preform is not less than 800 W / (m·K); The ceramic matrix is one or more of SiC, ZrC, HfC, TaC, SiBCN, and SiCN; The density of the high thermal conductivity pin and / or high thermal conductivity screw is 2.2-3.5 g / cm 3 ; The room temperature thermal conductivity of the high thermal conductivity pin and / or high thermal conductivity screw in the axial direction of the high thermal conductivity fiber is 200 to 300 W / (m·K).
6. The connection method according to claim 1, Features: The ceramic precursor solution is one or more of a SiC ceramic precursor solution, a ZrC ceramic precursor solution, a HfC ceramic precursor solution, a TaC ceramic precursor solution, a SiBCN ceramic precursor solution, a SiCN ceramic precursor solution, and a silicon-zirconium integrated precursor; The ceramic yield of the ceramic precursor is not less than 60%; and / or The viscosity of the ceramic precursor solution is 50-100 mPa·s.
7. The connection method according to claim 1, Features: In step (4), the number of times of impregnation-curing-cracking is 3 to 5 times, and the temperature of cracking is 1000 to 1500°C.
8. A heat conducting composite material component obtained by the connection method according to any one of claims 1 to 7.