Yellow fluorescent material and preparation method thereof, and yellow fluorescent device

By forming oxygen vacancies defect luminescence in the Ba3MgSi2O8 matrix material, the high cost and environmental protection problems of rare earth ion luminescent materials are solved, and an efficient and stable yellow fluorescent material is achieved, which is suitable for the color temperature adjustment and quantum yield improvement of warm white LEDs.

CN116925752BActive Publication Date: 2024-11-19SONGSHAN LAKE MATERIALS LAB +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310883837.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-18
Publication Date
2024-11-19
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

The existing yellow phosphors mainly rely on rare earth ions to emit light, resulting in high cost, fixed luminescence peaks and unenvironmental protection, making it difficult to achieve color temperature adjustment and high quantum yield of warm white LEDs.

Method used

Ba3MgSi2O8 is used as the matrix material to emit light through oxygen vacancies, and non-rare earth energy level luminescence is achieved. Oxygen vacancies are sintered using reducing atmosphere to generate oxygen vacancies, and luminescence characteristics are adjusted to obtain wide spectrum yellow light.

Benefits of technology

It realizes a low-cost, environmentally friendly yellow fluorescent material, which can adjust the luminous characteristics by controlling the oxygen vacancies concentration, improve quantum yield and stability, and is suitable for warm white LEDs and other lighting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116925752B_ABST
    Figure CN116925752B_ABST
Patent Text Reader

Abstract

The present application relates to the field of luminescent materials, and relates to a yellow fluorescent material and a preparation method thereof, and a yellow fluorescent device. The present application provides a yellow fluorescent material, the chemical formula of which is Ba 3 MgSi 2 O 8 The yellow fluorescent material includes an oxygen vacancy defect level that can emit yellow light. The yellow fluorescent material provided in the present application has a luminescence principle based on the luminescence of the oxygen vacancy defect level, which realizes the 3 MgSi 2 O 8 A new yellow fluorescent material is obtained by utilizing oxygen vacancy defect transition to emit yellow light in a single matrix material. The yellow fluorescent material of the present application has an luminescence principle of oxygen vacancy defect luminescence, which is different from the luminescence principle of common yellow fluorescent materials in the prior art. It is a new non-rare earth energy level luminescent yellow fluorescent material. The yellow fluorescent material of the present application does not rely on rare earth ions, has low cost, is environmentally friendly, can avoid the use of rare earth elements, and reduces the impact on the environment and resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of luminescent materials, and in particular, to a yellow fluorescent material and a preparation method thereof, and a yellow fluorescent device. Background Art

[0002] With the increasing energy consumption and the deterioration of the ecological environment, people are paying more and more attention to the rational use of energy and the research and development of environmentally friendly and energy-saving products. In the field of lighting, white light LED lighting has become the first choice of the new generation of lighting due to its advantages such as low power consumption, long service life, small size, high brightness, low heat and green environmental protection. It has been widely used in many fields such as home decoration, automotive lighting and commercial display.

[0003] At present, there are generally two commercial white light LED implementation solutions:

[0004] 1. White light is formed by mixing red, green and blue LED lights. This method requires the design of circuits for each LED separately, which makes its design complicated and costly, limiting its further application.

[0005] 2. Use a single blue light or ultraviolet light LED, combined with different phosphors, to achieve white light output by adjusting the ratio of phosphors. This method can not only effectively reduce the design cost, but also achieve different white light application requirements by adjusting the characteristics of phosphors.

[0006] For white light LED lighting based on phosphors, the characteristics of the phosphors are directly related to the color temperature, color rendering index and other characteristics of the corresponding white light.

[0007] The patent US599892 of Nichia Company of Japan proposes a method based on blue light LED to excite Y3Al5O 12 :Ce yellow garnet phosphor is the mainstream design solution for commercial white light. However, this method lacks the participation of the red light band, resulting in a high color temperature of white light LEDs, which is not conducive to the realization of warm white light LED lighting (color temperature <4000K). In contrast, Osram's Tb3Al5O 12 :Ce and Gd3Al5O 12 : The main emission peak of Ce yellow phosphor is red-shifted to the long-wave band, which can better improve the R9 color rendering index and better adapt to the needs of modern healthy lighting.

[0008] However, through the above background research and scientific research, it is found that the existing yellow phosphors are mainly realized by single or multiple doping of rare earth ions. As a non-renewable resource, rare earth ions have the characteristics of high cost, fixed luminescence peak position and environmental pollution. Summary of the invention

[0009] The purpose of the embodiments of the present application is to provide a new yellow fluorescent material and a preparation method thereof, and a yellow fluorescent device.

[0010] In a first aspect, the present application provides a yellow fluorescent material, the chemical formula of which is Ba3MgSi2O8; the yellow fluorescent material includes oxygen vacancy defect energy levels that can emit yellow light.

[0011] The yellow fluorescent material provided in the present application has a luminescence principle of oxygen vacancy defect energy level luminescence, which realizes yellow light emission by utilizing oxygen vacancy defect transition in a single matrix material of Ba3MgSi2O8, thereby obtaining a new yellow fluorescent material.

[0012] Furthermore, the luminescence of the yellow fluorescent material provided in the present application originates from the light generated when the electrons in the valence band are excited to the oxygen vacancy defect energy level and the electrons transition downward. The energy difference between the oxygen vacancy defect energy level and the valence band determines the wavelength of the luminescence. The yellow light of the yellow fluorescent material provided in the present application is due to the long-term reduction, which forms a large number of oxygen vacancy defects with deeper energy levels to obtain yellow light.

[0013] In the prior art, the common Y3Al5O 12 :Ce、Tb3Al5O 12 :Ce and Gd3Al5O 12 :Ce yellow phosphor, the principle of emitting yellow fluorescence is rare earth ion luminescence; that is, the luminescence of the material is achieved by using the luminescence of rare earth ions. However, as a non-renewable resource, rare earth ions have the characteristics of high cost, fixed luminescence peak position and environmental pollution. The yellow fluorescent material of the present application, the luminescence principle of which is oxygen vacancy defect luminescence, is different from the luminescence principle of the common yellow fluorescent materials in the prior art. It is a new non-rare earth energy level luminescent yellow fluorescent material. The yellow fluorescent material of the present application does not rely on rare earth ions, has low cost, is environmentally friendly, can avoid the use of rare earth elements, and reduces the impact on the environment and resources.

[0014] Furthermore, the yellow fluorescent material of the present application has good luminescence properties, and the luminescence properties can be adjusted by controlling the concentration of oxygen vacancies to achieve higher quantum yield and stability.

[0015] In other embodiments of the present application, the yellow light spectrum of the yellow fluorescent material includes 500nm-700nm.

[0016] The yellow fluorescent material of the present application has a wide spectrum and can cover the yellow light spectrum.

[0017] In other embodiments of the present application, the yellow light spectrum of the yellow fluorescent material includes 510nm-690nm.

[0018] In other embodiments of the present application, the excitation light source of the yellow fluorescent material includes 255nm~365nm ultraviolet light.

[0019] In other embodiments of the present application, the yellow fluorescent material can obtain yellow light with a central wavelength of 500nm~700nm by being excited by 255nm~365nm ultraviolet light.

[0020] In other embodiments of the present application, the yellow fluorescent material can obtain yellow light with a central wavelength of 600 nm by being excited by 255 nm to 365 nm ultraviolet light.

[0021] In other embodiments of the present application, the crystal form of the yellow fluorescent material is orthorhombic.

[0022] The yellow fluorescent material of the present application does not change the crystal form of the Ba3MgSi2O8 crystal, but forms a large number of oxygen vacancy defects inside it, thereby obtaining oxygen vacancies that can emit yellow fluorescence, and realizing yellow fluorescence by utilizing oxygen vacancy defect transitions in the Ba3MgSi2O8 single matrix material.

[0023] In a second aspect, the present application provides a method for preparing a yellow fluorescent material, comprising:

[0024] The raw material mixture of Ba3MgSi2O8 is sintered at 1200°C-1400°C for at least 2 hours in a reducing atmosphere, so that oxygen vacancies are generated in Ba3MgSi2O8 and the oxygen vacancies can emit yellow light.

[0025] The present application sintered the raw material mixture of Ba3MgSi2O8 at 1200℃~1400℃ for at least 2 hours in a reducing atmosphere, so that Ba3MgSi2O8 is sintered for a long time in a reducing atmosphere, oxygen vacancies are generated, and the crystal form does not change; the oxygen vacancy defect transition luminescence is utilized to realize a yellow fluorescent material with a wide spectrum yellow fluorescence in a single matrix material of Ba3MgSi2O8. The limitation problem that the luminescence of existing yellow fluorescent materials mainly comes from the luminescence of rare earth ions can be solved.

[0026] Furthermore, the above-mentioned preparation method of the present application can obtain oxygen vacancies capable of emitting yellow fluorescence by controlling the sintering atmosphere to a reducing atmosphere and controlling the sintering time to at least 2 hours. Furthermore, the above-mentioned preparation method of the present application can obtain the desired fluorescence emission by controlling the sintering time, controlling the concentration of oxygen vacancies in Ba3MgSi2O8, and adjusting the energy position of oxygen vacancy defects in Ba3MgSi2O8, so as to achieve higher quantum yield and stability.

[0027] In other embodiments of the present application, the sintering time is greater than or equal to 10 hours.

[0028] Within the above sintering time range, no stray peaks are generated and the yellow fluorescence is pure.

[0029] In other embodiments of the present application, the raw material mixture for preparing Ba3MgSi2O8 includes:

[0030] After the barium carbonate, magnesium oxide and silicon dioxide are uniformly mixed, they are pre-fired at 800°C to 1000°C for 2 hours to 5 hours; and then pressed into a green body.

[0031] In other embodiments of the present application, the green body is pressed, comprising:

[0032] The pre-sintered powder is pressed into a mold and then cold isostatically pressed at 230Mpa~250Mpa for 60 s~240s.

[0033] In other embodiments of the present application, the reducing atmosphere includes:

[0034] An atmosphere formed by a reducing gas; or

[0035] An atmosphere formed by a mixture of reducing gas and inert gas.

[0036] In other embodiments of the present application, the reducing gas includes hydrogen and ammonia; and the inert gas includes nitrogen.

[0037] In a third aspect, the present application provides a yellow fluorescent device, which includes the yellow fluorescent material provided in the first aspect; or the yellow fluorescent device includes the yellow fluorescent material prepared by the method for preparing the yellow fluorescent material provided in the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 XRD pattern of the material obtained in Example 1;

[0040] Figure 2 This is the emission spectrum of the material prepared in Example 1 under 332nm ultraviolet light excitation;

[0041] Figure 3 This is the emission spectrum of the material prepared in Example 2 under 332nm ultraviolet light excitation;

[0042] Figure 4 This is the emission spectrum of the material prepared in Example 3 under 332nm ultraviolet light excitation;

[0043] Figure 5 This is a photo of the luminescence of the material prepared in Example 1 under 332nm ultraviolet light excitation;

[0044] Figure 6 The chromaticity coordinate diagram of the material prepared in Example 1 excited by 332nm ultraviolet light;

[0045] Figure 7 The EPR detection spectrum of the materials obtained in Example 1 and the comparative example ( Figure 7 In the figure, the upper spectrum line having a high peak is Example 1, and the lower spectrum line having a low peak is Comparative Example 1);

[0046] Figure 8 and Fig. 9 The quantum yield results of the material prepared in Example 1 are shown. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.

[0048] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0049] An embodiment of the present application provides a yellow fluorescent material, the chemical formula of the yellow fluorescent material is Ba3MgSi2O8; the yellow fluorescent material includes oxygen vacancies that can emit yellow light.

[0050] The yellow fluorescent material provided in the present application has a luminescence principle of oxygen vacancy luminescence, which realizes yellow fluorescence by utilizing oxygen vacancy defect transition in a single matrix material of Ba3MgSi2O8, thereby obtaining a new yellow fluorescent material.

[0051] In the prior art, the yellow fluorescent materials of phosphate phosphors, silicate phosphors, and perovskite phosphors all emit yellow light based on the principle of rare earth ion luminescence; that is, the luminescence of the material is achieved by utilizing the luminescence of rare earth ions. However, as a non-renewable resource, rare earth ions have the characteristics of high cost, fixed luminescence peak position, and environmental pollution. The yellow fluorescent material of the present application has the luminescence principle of oxygen vacancy defect luminescence, which is different from the luminescence principle of the common yellow fluorescent materials in the prior art. It is a new non-rare earth energy level luminescent yellow fluorescent material. The yellow fluorescent material of the present application does not rely on rare earth ions, has low cost, is environmentally friendly, can avoid the use of rare earth elements, and reduces the impact on the environment and resources.

[0052] Furthermore, the yellow fluorescent material of the present application has good luminescence properties, and the luminescence properties can be adjusted by controlling the concentration of oxygen vacancies to achieve higher quantum yield and stability.

[0053] Furthermore, in some embodiments of the present application, the yellow light spectrum of the yellow fluorescent material includes 500nm-700nm.

[0054] The excitation light source of the yellow fluorescent material can be obtained through an excitation spectrum experiment.

[0055] The spectrum obtained by measuring the luminous flux (i.e. intensity) of the yellow fluorescent material as the wavelength of the excitation light changes is called the excitation spectrum.

[0056] Further optionally, in some embodiments of the present application, the above excitation spectrum experiment is carried out according to the following steps:

[0057] By scanning the excitation monochromator, incident light of different wavelengths is irradiated to excite the yellow fluorescent material. The emitted fluorescence is irradiated onto the detector through the emission monochromator of fixed wavelength, and its fluorescence intensity is detected. Finally, the relationship curve between the fluorescence intensity and the wavelength of the excitation light is recorded by a recorder, which is the excitation spectrum. The excitation light wavelength interval corresponding to the maximum fluorescence intensity interval in the excitation spectrum is selected as the optimal excitation light source interval for the yellow fluorescent material.

[0058] The fluorescent material of the present application can be excited by ultraviolet light of 255nm~365nm as an excitation light source to excite the Ba3MgSi2O8 yellow fluorescent material to emit yellow light.

[0059] Further optionally, the yellow fluorescent material uses 255nm-365nm ultraviolet light as an excitation light source to excite the Ba3MgSi2O8 yellow fluorescent material to emit yellow light.

[0060] Furthermore, in some embodiments of the present application, the yellow fluorescent material can obtain yellow light with a central wavelength of 500nm to 700nm by being excited by 255nm-365nm ultraviolet light.

[0061] Illustratively, in some embodiments of the present application, the above-mentioned yellow fluorescent material can obtain yellow light with a central wavelength of 550nm, 580nm, 600nm, 620nm, 650nm, 680nm or 690nm by excitation of ultraviolet light of 260nm, 270nm, 280nm, 290nm, 300nm, 310nm, 320nm, 330nm, 340nm, 350nm or 360nm.

[0062] Further optionally, in some embodiments of the present application, the yellow fluorescent material can obtain yellow light with a central wavelength of 600 nm by being excited by 255 nm-365 nm ultraviolet light.

[0063] Furthermore, a yellow light fluorescence emission spectrum is obtained under the excitation of an optimal excitation light source.

[0064] Furthermore, in some embodiments of the present application, the yellow light spectrum of the yellow fluorescent material includes 500nm-700nm.

[0065] The yellow fluorescent material of the present application has a wide spectrum and can cover the yellow light spectrum.

[0066] Furthermore, in some embodiments of the present application, the yellow light spectrum of the yellow fluorescent material includes 510nm-690nm.

[0067] Illustratively, in some embodiments of the present application, the yellow light spectrum of the yellow fluorescent material is 520 nm, 530 nm, 540 nm, 600 nm, 610 nm, 650 nm, 660 nm or 680 nm.

[0068] Furthermore, in some embodiments of the present application, the crystal form of the yellow fluorescent material is the crystal form of Ba3MgSi2O8, which is an orthorhombic system.

[0069] The yellow fluorescent material of the present application does not change the crystal form of the Ba3MgSi2O8 crystal, but forms a large number of oxygen vacancy defects inside it, thereby obtaining oxygen vacancies that can emit yellow light, and realizes yellow light emission by utilizing oxygen vacancy defect transitions in the Ba3MgSi2O8 single matrix material.

[0070] Some embodiments of the present application provide a method for preparing a yellow fluorescent material, comprising:

[0071] The raw material mixture of Ba3MgSi2O8 is sintered at 1200°C to 1400°C in a reducing atmosphere for at least 2 hours to generate oxygen vacancies in Ba3MgSi2O8 and the oxygen vacancies can emit yellow light.

[0072] The present application sintered the raw material mixture of Ba3MgSi2O8 at 1200℃~1400℃ for at least 2 hours in a reducing atmosphere, so that Ba3MgSi2O8 is sintered for a long time in a reducing atmosphere, oxygen vacancies are generated, and the crystal form does not change; the oxygen vacancy defect transition luminescence is utilized to realize a yellow fluorescent material with a wide spectrum of yellow light in a single matrix material of Ba3MgSi2O8. The limitation that the existing yellow phosphor luminescence mainly comes from the luminescence of rare earth ions can be solved.

[0073] Furthermore, the above-mentioned preparation method of the present application can obtain a large number of oxygen vacancies capable of emitting yellow light by controlling the sintering atmosphere to a reducing atmosphere and the sintering time to at least 2 hours. Furthermore, the above-mentioned preparation method of the present application can obtain the desired fluorescence emission by controlling the sintering time, controlling the concentration of oxygen vacancies in Ba3MgSi2O8, and adjusting the energy position of oxygen vacancy defects in Ba3MgSi2O8, so as to achieve higher quantum yield and stability.

[0074] Furthermore, in some embodiments of the present application, the sintering time is greater than or equal to 10 hours.

[0075] Within the above sintering time range, no stray peaks are generated and the yellow fluorescence is pure.

[0076] Illustratively, in some embodiments of the present application, the sintering time is 5 hours, 10 hours, 15 hours, 20 hours, 24 hours, 30 hours, 35 hours or 48 hours.

[0077] Further, in some embodiments of the present application, the reducing atmosphere includes:

[0078] An atmosphere formed by reducing gases.

[0079] Further, in some embodiments of the present application, the reducing atmosphere includes:

[0080] An atmosphere formed by a mixture of reducing gas and inert gas.

[0081] Furthermore, in some embodiments of the present application, the reducing gas includes hydrogen and ammonia; and the inert gas includes nitrogen.

[0082] Furthermore, in some embodiments of the present application, a method for preparing a yellow fluorescent material comprises the following steps:

[0083] Step S1, preparing a raw material mixture of Ba3MgSi2O8.

[0084] Furthermore, in some embodiments of the present application, barium carbonate, magnesium oxide, and silicon dioxide are uniformly mixed, pre-fired at 800° C. to 1000° C. for at least 4 hours, and then pressed into a green body.

[0085] Further, in some embodiments of the present application, barium carbonate, magnesium oxide, and silicon dioxide are uniformly mixed, including:

[0086] Barium carbonate, magnesium oxide and silicon dioxide were mixed in a molar ratio of 1:1:1 and then ball-milled.

[0087] Furthermore, in some embodiments of the present application, the ball milling includes: adding appropriate amounts of ethanol and a dispersant to the mixture obtained above, placing the mixture in a ball milling jar, and performing two-way ball milling for 12 h to 24 h.

[0088] Illustratively, in some embodiments of the present application, the ball milling time is 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h or 24 h.

[0089] Further optionally, the above-mentioned dispersant may be oleic acid or the like.

[0090] Further, in some embodiments of the present application, after the barium carbonate, magnesium oxide and silicon dioxide are uniformly mixed, pre-sintering at 800° C. to 1000° C. for at least 4 hours comprises:

[0091] The ball-milled mixture is dried and ground; and then pre-fired in a furnace at 800°C to 1000°C for at least 4 hours.

[0092] For example, in some embodiments of the present application, the pre-firing temperature may be selected from 810°C, 820°C, 830°C, 850°C, 860°C, 870°C or 880°C.

[0093] Illustratively, in some embodiments of the present application, the above-mentioned pre-burning time can be selected as 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.

[0094] Pre-firing can make the material purer, which is conducive to obtaining a yellow fluorescent material with good color rendering.

[0095] Further, in some embodiments of the present application, the pressing into a green body comprises:

[0096] The pre-sintered powder is pressed into a mold and then cold isostatically pressed at 230Mpa~250Mpa for 60 s~240s.

[0097] Further optionally, the pressing into a green body comprises:

[0098] The pre-calcined powder is pressed into a shape, and then cold isostatically pressed at 231 MPa ~ 249 MPa for 61s ~ 239s.

[0099] Exemplarily, the pressing into a green body comprises:

[0100] The pre-calcined powder is pressed into a shape, and then cold isostatically pressed at 232 MPa, 235 MPa, 236 MPa, 238 MPa, 240 MPa, 242 MPa, 243 MPa, 245 MPa or 248 MPa for 65 s, 70 s, 75 s, 80 s, 100 s, 150 s or 200 s.

[0101] Exemplarily, the pre-sintered powder is ground and sieved, pressed into a green body by dry pressing, and then cold-pressed in a cold isostatic press at 240 MPa for 60 s to 240 s.

[0102] Step S2, sintering the raw material mixture of Ba3MgSi2O8 at 1200°C-1400°C for at least 2 hours in a reducing atmosphere, so that Ba3MgSi2O8 generates oxygen vacancies and the oxygen vacancies can emit yellow light.

[0103] Further optionally, in some embodiments of the present application, the raw material mixture of Ba3MgSi2O8 is sintered at 1201°C~1399°C for at least 2 hours in a reducing atmosphere.

[0104] Illustratively, in some embodiments of the present application, the raw material mixture of Ba3MgSi2O8 is sintered at 1208°C, 1208°C, 1210°C, 1218°C, 1224°C, 1231°C, 1245°C, 1270°C, 1305°C, 1330°C, 1370°C, 1375°C or 1394°C in a reducing atmosphere for at least 26 hours, 27 hours, 31 hours, 32 hours, 38 hours or 42 hours.

[0105] For example, in some embodiments of the present application, the formed blank obtained in the aforementioned step S1 is placed in a tubular furnace and sintered at 1200° C. to 1400° C. in a reducing atmosphere for at least 2 hours to prepare a Ba3MgSi2O8 yellow fluorescent material.

[0106] The preparation method of the yellow fluorescent material of the present application adopts a solid phase method, which has a simple preparation process, a short cycle, simple and cheap raw materials, and is conducive to industrial large-scale production.

[0107] The yellow phosphor of the present application is a wide-spectrum phosphor, whose light emission covers the yellow light region, has a high color rendering index, can more realistically restore the color of an object, and has better effects in lighting, display, etc.

[0108] Compared with rare earth luminescent materials, the yellow phosphor of the present application is a non-rare earth energy level luminescent material that is more environmentally friendly and healthy, because the mining and processing of rare earth elements may cause environmental pollution and human health risks.

[0109] Some embodiments of the present application provide a yellow fluorescent device, which includes the yellow fluorescent material provided by any of the aforementioned embodiments; or the yellow fluorescent device includes the yellow fluorescent material prepared by the method for preparing the yellow fluorescent material provided by any of the aforementioned embodiments.

[0110] Further optionally, in some embodiments of the present application, the yellow fluorescent device can be a yellow light LED yellow fluorescent device, a white light LED yellow fluorescent device, a display, a security sign, etc. It can also be applied to biological imaging and photocatalysis.

[0111] Some specific embodiments are listed below to better illustrate the present application.

[0112] Example 1

[0113] A yellow fluorescent material is provided, which is prepared according to the following steps:

[0114] (a) Weighing: Accurately weigh barium carbonate (BaCO3), magnesium oxide (MgO), and silicon dioxide (SiO2) at a molar ratio of 1:1:1;

[0115] (b) ball milling: add appropriate amount of ethanol and dispersant to all the raw materials weighed in step (a), place them in a ball mill, and perform two-way ball milling for 25 hours;

[0116] (c) Calcination: The slurry after ball milling in step (b) was transferred to a glass dish, dried and ground, and pre-calcined in a box furnace at 800° C. for 3 h.

[0117] (e) Molding: The pre-fired powder in step (c) is ground and sieved, pressed into a green billet by dry pressing, and then cold-pressed in a cold isostatic press at 230 MPa for 100 seconds.

[0118] (f) Sintering: The green blank formed in step (e) is placed in a tubular furnace and sintered at 1200° C. for 24 h in a mixed gas atmosphere of hydrogen and nitrogen to prepare Ba3MgSi2O8 fluorescent ceramics.

[0119] Example 2

[0120] A yellow fluorescent material is provided, which is prepared according to the following steps:

[0121] (a) Weighing: Accurately weigh barium carbonate (BaCO3), magnesium oxide (MgO), and silicon dioxide (SiO2) at a molar ratio of 1:1:1;

[0122] (b) ball milling: add appropriate amount of ethanol and dispersant to all the raw materials weighed in step (a), place them in a ball mill, and perform two-way ball milling for 25 hours;

[0123] (c) Calcination: The slurry after ball milling in step (b) was transferred to a glass dish, dried and ground, and pre-calcined in a box furnace at 800° C. for 3 h.

[0124] (e) Molding: The pre-fired powder in step (c) is ground and sieved, pressed into a green billet by dry pressing, and then cold-pressed in a cold isostatic press at 230 MPa for 100 seconds.

[0125] (f) Sintering: The green blank formed in step (e) is placed in a tubular furnace and sintered at 1200° C. for 10 h in a mixed gas atmosphere of hydrogen and nitrogen to prepare Ba3MgSi2O8 fluorescent ceramics.

[0126] Example 3

[0127] A yellow fluorescent material is provided, which is prepared according to the following steps:

[0128] (a) Weighing: Accurately weigh barium carbonate (BaCO3), magnesium oxide (MgO), and silicon dioxide (SiO2) at a molar ratio of 1:1:1;

[0129] (b) ball milling: add appropriate amount of ethanol and dispersant to all the raw materials weighed in step (a), place them in a ball mill, and perform two-way ball milling for 25 hours;

[0130] (c) Calcination: The slurry after ball milling in step (b) was transferred to a glass dish, dried and ground, and pre-calcined in a box furnace at 800° C. for 3 h.

[0131] (e) Molding: The pre-fired powder in step (c) is ground and sieved, pressed into a green billet by dry pressing, and then cold-pressed in a cold isostatic press at 230 MPa for 100 seconds.

[0132] (f) Sintering: The green blank formed in step (e) is placed in a tubular furnace and sintered at 1200° C. for 2 h in a mixed gas atmosphere of hydrogen and nitrogen to prepare Ba3MgSi2O8 fluorescent ceramics.

[0133] Comparative Example 1

[0134] The preparation steps are the same as those in Example 1, except that the sintering is performed in air atmosphere in step (f).

[0135] Experimental example

[0136] The properties of the materials obtained in Examples 1-3 and Comparative Example 1 were tested.

[0137] 1. Crystal form detection

[0138] The crystal form of the material obtained in Example 1 was detected by X-ray diffraction. Figure 1 .

[0139] from Figure 1 It can be seen that the material prepared in Example 1 has a single component and is pure, indicating that the preparation method of the present application will not change the Ba3MgSi2O8 crystal form.

[0140] 2. Luminescence performance test

[0141] (1) Emission Spectra The emission spectra of the materials prepared in Examples 1-3 were tested. The results are as follows: Figure 2-Figure 4 .

[0142] from Figure 2-Figure 4 The emission spectra of the materials prepared in Examples 1-3 under 332nm ultraviolet light excitation are shown respectively;

[0143] It can be seen that the material of Example 1-2 can generate yellow light with a central wavelength of 520 nm by being excited by 332 nm ultraviolet light.

[0144] The material of Example 3 can also obtain yellow light with a central wavelength of 520 nm by being excited by 332 nm ultraviolet light, but there will be stray peaks in the low-wave band.

[0145] It can be seen that when the sintering time is more than 10, the luminescence is purer.

[0146] (2) Launching physical objects

[0147] The material obtained in Example 1 was excited by 332nm ultraviolet light, and the results were as follows: Figure 5 .

[0148] from Figure 5 It can be seen that the material prepared in Example 1 can emit yellow light when excited by 332nm ultraviolet light.

[0149] 3. Chromaticity performance test

[0150] The material obtained in Example 1 was excited by 332nm ultraviolet light and the chromaticity coordinates were examined. The results are as follows: Figure 6 .

[0151] from Figure 6 It can be seen that the chromaticity coordinates of the material prepared in Example 1 of the present application are within the yellow range, the chromaticity is pure, there is no stray light, and the color rendering index is high.

[0152] 4. Oxygen vacancy detection

[0153] The oxygen vacancies of the materials prepared in Example 1 and Comparative Example 1 were detected by electron paramagnetic resonance spectrometer (EPR). Figure 7 .

[0154] Depend on Figure 7It can be seen that the g value peak at 2.004 in the EPR spectrum of the yellow fluorescent material prepared in Example 1 is the peak of oxygen vacancies. The greater the intensity, the higher the content. It can be clearly seen that the oxygen vacancy content in the reducing atmosphere sintering is much higher than that in the air sintering; it can emit yellow light. The oxygen vacancy defect energy level position of the material in Comparative Example 1 is different from that in Example 1. The peak intensity of Comparative Example 1 is lower than that of Example 1, and it cannot emit yellow light.

[0155] 5. Quantum yield detection

[0156] The quantum yield of the material prepared in Example 1 was tested. Figure 8~Figure 9 .

[0157] from Figure 8~Figure 9 It can be seen that the quantum yield of the yellow fluorescent material prepared in Example 1 of the present application is 47.49%.

[0158] It can be seen that the yellow fluorescent material prepared in the embodiment of the present application effectively improves the quantum yield.

[0159] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

Claims

1. A yellow fluorescent material, characterized in that: The chemical formula of the yellow fluorescent material is Ba3MgSi2O8; the yellow fluorescent material includes oxygen vacancy defect energy levels capable of emitting yellow light; The yellow fluorescent material is prepared according to the following steps: (a) Weighing: Accurately weigh barium carbonate (BaCO3), magnesium oxide (MgO), and silicon dioxide (SiO2) at a molar ratio of 1:1:1; (b) ball milling: add appropriate amount of ethanol and dispersant to all the raw materials weighed in step (a), place them in a ball mill, and perform two-way ball milling for 25 hours; (c) Calcination: The slurry after ball milling in step (b) was transferred to a glass dish, dried and ground, and pre-calcined in a box furnace at 800°C for 3h; (e) Molding: The pre-sintered powder in step (c) is ground and sieved, pressed into a green billet by dry pressing, and then cold-pressed in a cold isostatic press at 230 MPa for 100 seconds; (f) Sintering: The green blank formed in step (e) is placed in a tubular furnace and sintered at 1200° C. for 24 h in a mixed gas atmosphere of hydrogen and nitrogen to prepare Ba3MgSi2O8 fluorescent ceramics.

2. The yellow fluorescent material according to claim 1, characterized in that: The yellow light spectrum of the yellow fluorescent material includes 500nm-700nm.

3. The yellow fluorescent material according to claim 1, characterized in that: The yellow light spectrum of the yellow fluorescent material includes 510nm-690nm.

4. The yellow fluorescent material according to claim 1, characterized in that: The yellow fluorescent material can obtain yellow light with a central wavelength of 500nm to 700nm by being excited by 255nm to 365nm ultraviolet light.

5. The yellow fluorescent material according to claim 4, characterized in that: The yellow fluorescent material can obtain yellow light with a central wavelength of 600 nm by being excited by 255 nm to 365 nm ultraviolet light.

6. The yellow fluorescent material according to any one of claims 1 to 5, characterized in that: The crystal form of the yellow fluorescent material is orthorhombic.

7. The method for preparing the yellow fluorescent material according to any one of claims 1 to 6, characterized in that: include: (a) Weighing: Accurately weigh barium carbonate (BaCO3), magnesium oxide (MgO), and silicon dioxide (SiO2) at a molar ratio of 1:1:1; (b) ball milling: add appropriate amount of ethanol and dispersant to all the raw materials weighed in step (a), place them in a ball mill, and perform two-way ball milling for 25 hours; (c) Calcination: The slurry after ball milling in step (b) was transferred to a glass dish, dried and ground, and pre-calcined in a box furnace at 800°C for 3h; (e) Molding: The pre-sintered powder in step (c) is ground and sieved, pressed into a green billet by dry pressing, and then cold-pressed in a cold isostatic press at 230 MPa for 100 seconds; (f) Sintering: The green blank formed in step (e) is placed in a tubular furnace and sintered at 1200° C. for 24 h in a mixed gas atmosphere of hydrogen and nitrogen to prepare Ba3MgSi2O8 fluorescent ceramics.

8. A yellow fluorescent device, characterized in that: The yellow fluorescent device comprises the yellow fluorescent material according to any one of claims 1 to 6; or the yellow fluorescent device comprises the yellow fluorescent material prepared by the method for preparing the yellow fluorescent material according to claim 7.