Sol-gel treating agent and preparation method and use method thereof
By using solvents such as deionized water and anhydrous ethanol, combining phosphate and ethyl methacrylate substances, the sol-gel process is simplified, and the binding force between titanium alloy, aluminum alloy and organic paint film is improved, and the existing technology is solved. The problems of insufficient solvent cross-linking and complex process have achieved efficient binding and environmentally friendly sol-gel treatment effects.
Patent Information
- Application Number
- CN202310667718.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-07
AI Technical Summary
In the process of increasing the binding force of the surface paint film of titanium alloy and aluminum alloy, there are problems such as insufficient solvent cross-linking, complex process parameters, and water content limitation, resulting in unsatisfactory bonding effect and risk of environmental and health pollution. .
Using deionized water or anhydrous ethanol as solvents, the sol coagulation of components A and B is prepared by adding phosphate and ethyl methacrylate substances to improve the cross-linking ability of the sol gel and the content of metal covalent bonds. The glue treatment agent simplifies process parameters and forms an efficient three-dimensional network structure to improve the binding force between titanium alloy, aluminum alloy and organic paint film.
It realizes rapid film formation under a wide range of construction ambient temperatures, efficiently improves the binding force of titanium alloy, aluminum alloy and organic paint film, and does not require complex process parameters, and the binding force reaches the level 0 standard. It is environmentally friendly and has no harmful substances, and is suitable for aircraft Parts repair.
Smart Images

Figure CN116948433B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal surface treatment, and specifically relates to a sol-gel treatment agent and a preparation method and a use method thereof. The sol-gel treatment agent is mainly used to improve the bonding strength of paint films on the surfaces of titanium alloys and aluminum alloys. Background Art
[0002] Aluminum and aluminum alloys, titanium and titanium alloys are widely used in aviation, aerospace and other fields because of their light weight, strong plasticity and high strength. For example, the upper wall panels, bulkheads, skins and other parts of aircraft wings. In engineering applications, a primer is usually prepared on the surface of the parts first, and then an organic paint layer is coated on the surface of the primer, which can play the role of corrosion resistance, decoration, wear resistance and other functions. The main purpose of the primer is to improve the corrosion resistance of the base material and improve the bonding strength between the base material and the paint film. The primer on the surface of aluminum and aluminum alloys is usually prepared by chemical oxidation, anodizing and micro-arc oxidation. The surface primer of titanium and titanium alloys is usually prepared by anodizing. However, the above methods are used to prepare the primer, and the treatment process will reduce the fatigue performance of the base material, and most of the primers have strong acids, harmful metal ions and other pollutants that are harmful to the environment and the body during the treatment process. Therefore, it is urgent to develop a new treatment process that can improve the bonding strength between titanium alloys, aluminum alloys and organic paint films.
[0003] The sol-gel conversion film layer on the metal surface refers to a solid film layer formed on the metal surface after the sol-gel treatment agent is uniformly applied on the metal surface and cured. The sol-gel conversion film layer can form Me-O-Me' and Me-O-Si covalent bonds with one side of the metal, and can also form covalent bonds with one side of the organic paint film. The bonding strength of the covalent bonds formed on both sides is high, which can play a role in improving the bonding force between the organic paint film and the metal substrate. In addition, due to the structural characteristics of the covalent bond, the sol-gel conversion film layer can also be used as a base layer for the adhesive. Before applying the adhesive, the sol-gel treatment agent is first applied to the surface of the titanium alloy and the aluminum alloy and cured, thereby improving the bonding strength of the adhesive.
[0004] At present, although the sol-gel process has been widely used, it still has many defects, such as: (1) The sol-gel treatment agent usually uses a two-component solvent. Before use, the two-component solvent is mixed to prepare a multi-component sol, and then allowed to stand for a certain period of time to cross-link each other. However, it cannot be fully cross-linked at room temperature or low temperature to form a three-dimensional network, so the improvement of the adhesion of the paint film cannot achieve the expected effect. It is even more difficult to implement processes such as aircraft field surface repair in a low temperature environment; (2) The solvent is generally water-based or water-alcohol-based. After the two components are mixed, the hydrolysis reaction rate of the precursor is relatively fast. After mixing, it needs to be coated as soon as possible, otherwise precipitation will form in the solution, reducing the metal content in the conversion film layer, resulting in a decrease in the number of covalent bonds between it and the metal matrix, thereby affecting the effect of improving the adhesion of the paint film.
[0005] The invention patent with application publication number CN102079947A discloses a method for preparing a sol-gel conversion film on the surface of a titanium alloy, which includes the following steps: metal sample treatment; sol preparation; film coating; and film drying. The sol preparation steps are as follows: preparing a mixed solvent 1, wherein the volume ratio of a lower alcohol to water is 20-50%; preparing an organosiloxane sol 2, pouring the organosiloxane into the mixed solvent 1, wherein the volume content of the organosiloxane is 2-10%, the stirring temperature is 10-50° C., the stirring speed is 500-1000 rpm, and the stirring is performed for 1 hour; preparing a mixture 3 of an organic metal alkoxide and an organic acid, uniformly mixing the organic metal alkoxide and the organic acid at a temperature of 10-50° C., wherein the volume ratio of the organic metal alkoxide and the organic acid is 1-3:1, the stirring speed is 500-1000 rpm, and the stirring is performed for 5-15 minutes; pouring the mixture 3 of the metal alkoxide and the organic acid into the organosiloxane sol 2 under strong stirring at a speed of 1200-1600 rpm, and continuing to stir at a temperature of 10-30° C., a stirring speed of 500-1000 rpm, and a stirring for 1-2 hours, wherein the volume ratio of silane to the metal alkoxide is preferably 2:1. Although the sol-gel prepared by this technical solution has good bonding strength between metal and paint film, there are many requirements for process parameters during the sol preparation process, such as the speed, stirring time, stirring temperature, etc. of the stirrer. When achieving the same technical effect, the more process parameters there are, the more complicated the process is, and the higher the time and labor costs are.
[0006] The invention patent with application publication number CN109207060A discloses a non-aqueous sol-gel for enhancing the adhesion of water-sensitive materials. The method for forming the sol-gel includes: forming a first mixture with mixed metal alkoxide, acid stabilizer and organic solvent, the first mixture having a water content of less than 10wt% based on the total weight of the first mixture; mixing the first mixture with organic silane to form a second mixture, the second mixture having a water content of less than 10wt% based on the total weight of the second mixture. The water content in the sol-gel treating agent of the technical solution is less than 10wt%, and it can only be used for treating the surface of water-sensitive materials, and cannot be used for treating the surface of conventional metal materials. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a sol-gel treating agent, comprising component A and component B; the mass percentage of each substance in the sol-gel treating agent is 80-95wt% of component A and 5-20wt% of component B; the component A comprises a solvent, an inhibitor and a zirconium-containing compound, and the component B comprises a solvent, a compatibilizer and siloxane.
[0008] Preferably, the mass percentages of the substances in the component A are as follows: the solvent accounts for 80-97 wt %, the inhibitor accounts for 2-10 wt %, and the zirconium-containing compound accounts for 1-10 wt %.
[0009] In any of the above schemes, it is preferred that the solvent in component A is deionized water or a mixture of anhydrous ethanol and deionized water, and the mass percentages of the anhydrous ethanol and the deionized water in the solvent in component A are 15-35wt% and 65-85wt%, respectively; the inhibitor in component A is a mixture of an organic acid and a phosphate, and the mass percentages of the organic acid and the phosphate in the inhibitor in component A are 60-90% and 10-40%, respectively.
[0010] In any of the above schemes, preferably, the mass ratio of the phosphate to the zirconium-containing compound is 1:4-10.
[0011] In any of the above schemes, it is preferred that the organic acid includes any one or more of citric acid, acetic acid, oxalic acid, and phytic acid; the phosphate includes sodium dihydrogen phosphate and / or potassium dihydrogen phosphate; and the zirconium-containing compound includes any one or more of zirconium n-propoxide, fluorozirconic acid, potassium fluorozirconate, and sodium fluorozirconate.
[0012] In any of the above schemes, it is preferred that the mass percentages of the substances in the component B are as follows: the solvent accounts for 37-59Wt%, the compatibilizer accounts for 1-3Wt%, and the siloxane accounts for 40-60Wt%.
[0013] In any of the above schemes, it is preferred that the solvent in the component B is anhydrous ethanol; the compatibilizer is a methacrylate functional group organic substance, and the methacrylate functional group organic substance is acetoacetoxyethyl methacrylate; and the siloxane includes any one or more of γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and 3-aminopropyltriethoxysilane.
[0014] The present invention takes into account the sol-gel reaction mechanism, uses water or water-alcohol as a solvent, increases the content of metal covalent bonds in the film-forming reaction by adding phosphates, and improves the ability of mutual cross-linking by using ethyl methacrylate-based organic matter, thereby synergistically improving the bonding strength between titanium alloys, aluminum alloys and organic paint films.
[0015] The sol-gel treating agent of the present invention uses deionized water or a mixture of deionized water and anhydrous ethanol as a solvent, a monobasic or dibasic acid as an inhibitor, and a zirconium-containing compound and an organic siloxane as precursors respectively. By adding phosphate and ethyl methacrylate substances, the cross-linking ability in the sol and the content of metal covalent bonds in the film-forming reaction are improved. The sol-gel treating agent is used for coating, which can effectively improve the bonding force between titanium alloys, aluminum alloys and organic paint films.
[0016] In the present invention, zirconium phosphate can be prepared from zirconium-containing compounds and hydrogen phosphate, which is soluble in organic acids, increases the content of Zr-O bonding, and increases the ratio of Zr-O-Me bonding at the interface between the sol-gel conversion film layer and the titanium alloy and the aluminum alloy. Therefore, an appropriate ratio is required between hydrogen phosphate and the zirconium-containing compound, otherwise the solution will either precipitate or fail to increase the bonding content. In the present invention, the mass ratio of phosphate to zirconium-containing compound is 1:4-10.
[0017] The cross-linking monomer of the β-dihydroxy structure in ethyl acetoacetoxy methacrylate is bonded to the inorganic component, and is easy to undergo cross-linking reaction with other C=C double bonds, and the polymerization process is easy to control, and the self-cross-linking efficiency is high. Adding ethyl acetoacetoxy methacrylate can fully combine the organic component with the inorganic component, effectively inhibit the phase separation of organic / inorganic hybrid materials, and make the sol-gel treatment agent fully cross-linked to form a three-dimensional network.
[0018] The present invention also provides a method for preparing a sol-gel treating agent, wherein the sol-gel treating agent is any one of the sol-gel treating agents described above, and comprises the following steps in chronological order:
[0019] Step 1: According to the designed composition of the sol-gel treating agent, weigh each substance separately for use;
[0020] Step 2: prepare the solvent, inhibitor, and zirconium-containing compound in component A respectively; add the prepared inhibitor to the prepared solvent and mix them evenly to form a mixture of the inhibitor and the solvent; then add the prepared zirconium-containing compound to the mixture of the inhibitor and the solvent and mix them evenly to form component A;
[0021] Step 3: prepare the solvent, the compatibilizer and the siloxane in component B respectively; mix the prepared siloxane and the prepared compatibilizer evenly to form a mixture of the siloxane and the compatibilizer; then add the mixture of the siloxane and the compatibilizer to the prepared solvent and mix evenly to form component B;
[0022] Step 4: Add component B to component A, mix well and let stand to form a sol-gel treating agent.
[0023] Preferably, the pH value of component A is 2.0-4.0, and the pH value of component B is 5.0-8.0; the standing time after component A and component B are evenly mixed is not less than 30 minutes, and the standing temperature is 15-35°C.
[0024] The present invention also provides a method for using a sol-gel treating agent, wherein the sol-gel treating agent is any one of the sol-gel treating agents described above, and comprises the following steps in chronological order:
[0025] Step (1): pretreating the alloy surface by sandblasting, grinding, deoxidation or polishing;
[0026] Step (2): coating the pretreated alloy surface with a sol-gel treatment agent by spraying, brushing or dipping to form a continuous sol-gel liquid film layer, maintaining the film layer for a certain period of time, and then drying the sol-gel film layer with compressed air to remove excess liquid;
[0027] Step (3): curing the sol-gel treatment agent from which excess liquid has been removed, and after the curing is completed, a continuous sol-gel conversion film layer can be formed on the alloy surface;
[0028] Step (4) spraying an organic paint film on the sol-gel conversion film layer.
[0029] Preferably, the alloy is a titanium alloy or an aluminum alloy; the thickness of the sol-gel liquid film layer is 1-2 mm, the holding time is 1-2 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 0.03-2 μm; the curing temperature is room temperature, the curing time is not less than 30 min, and the thickness of the sol-gel conversion film layer after curing is 0.03-2 μm. In the present invention, the sol-gel liquid film layer is liquid, and the sol-gel conversion film layer is solid.
[0030] In step (1), the titanium alloy is surface pretreated by sandblasting or grinding; the aluminum alloy is surface pretreated by deoxidation, polishing or grinding. In step (2), component A and component B are mixed 0.5-168 hours before coating the sol-gel treatment agent on the pretreated alloy surface.
[0031] The present invention does not make special requirements on the mixing parameters of various substances (such as mixing time, stirring speed, mixing temperature, etc.), compressed air drying parameters, alloy surface pretreatment parameters, etc. during the preparation of the sol-gel treating agent and during the use of the sol-gel treating agent.
[0032] The sol-gel treatment agent of the present invention has the ability to simultaneously improve the cross-linking ability of the sol-gel and the metal covalent bond content of the conversion film layer, has a fast film-forming speed, a wide range of construction environment temperature, does not require too many process parameters to be limited (for example, when mixing various substances, does not require the stirring speed, stirring temperature, stirring time, etc. to be limited), and has high film bonding strength. After applying the sol-gel treatment agent, the bonding strength between the titanium alloy, the aluminum alloy and the organic paint film can reach level 0, and the bonding strength test standard refers to GB / T 5210.
[0033] The coating layer of the sol-gel treatment agent of the present invention is uniform, continuous and complete, and can improve the bonding strength between titanium alloy, aluminum alloy and organic paint film without changing the fatigue performance of the alloy matrix. In addition, the composition of the sol-gel treatment agent is environmentally friendly and free of harmful substances. It can be used in a temperature environment above -10°C and is suitable for field repair operations on metal surfaces of parts such as aircraft and engines. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The present invention is a flow chart of a preparation process of a sol-gel treatment agent according to a preferred embodiment of the sol-gel treatment agent and a preparation method and a use method thereof;
[0035] Figure 2 for Figure 1 In the embodiment shown, the cross-hatch morphology after coating the alloy surface with a sol-gel treatment agent and performing a paint film adhesion test at different construction environment temperatures is shown, wherein: (a) is a construction environment temperature of -8°C, (b) is a construction environment temperature of 15°C, and (c) is a construction environment temperature of 28°C. DETAILED DESCRIPTION
[0036] In order to further understand the content of the present invention, the present invention will be described in detail below in conjunction with specific embodiments.
[0037] Embodiment 1:
[0038] According to a preferred embodiment of the sol-gel treating agent of the present invention, it includes component A and component B; the mass percentage of each substance in the sol-gel treating agent is 80Wt% of component A and 20Wt% of component B; the component A includes a solvent, an inhibitor and a zirconium-containing compound, and the component B includes a solvent, a compatibilizer and a siloxane.
[0039] The mass percentages of the substances in the component A are as follows: the solvent accounts for 80 wt%, the inhibitor accounts for 10 wt%, and the zirconium-containing compound accounts for 10 wt%. The solvent in the component A is a mixture of anhydrous ethanol and deionized water, and the anhydrous ethanol and the deionized water account for 15 wt% and 85 wt% of the solvent in the component A respectively; the inhibitor in the component A is a mixture of an organic acid and a phosphate, and the organic acid and the phosphate account for 90 wt% and 10 wt% of the inhibitor in the component A respectively, and the mass ratio of the phosphate to the zirconium-containing compound is 1:10. The organic acid is oxalic acid, the phosphate is sodium dihydrogen phosphate, and the zirconium-containing compound is zirconium n-propoxide.
[0040] The mass percentage of each substance in the component B is 37 wt% of the solvent, 3 wt% of the compatibilizer, and 60 wt% of the siloxane. The solvent in the component B is anhydrous ethanol; the compatibilizer is ethyl acetoacetate methacrylate; and the siloxane is γ-glycidyloxypropyltrimethoxysilane.
[0041] That is, if 100g of sol-gel treatment agent is prepared, component A is 80g and component B is 20g. The mass of each substance in component A is 64g of solvent, 8g of inhibitor, and 8g of zirconium-containing compound; the anhydrous ethanol in the solvent is 9.6g, and the deionized water is 54.4g; the organic acid in the inhibitor is 7.2g, and the phosphate is 0.8g. The mass of each substance in component B is 7.4g of solvent, 0.6g of compatibilizer, and 12g of siloxane.
[0042] In this embodiment, deionized water and anhydrous ethanol are used as solvents based on the sol-gel reaction mechanism. Phosphates are added to increase the content of metal covalent bonds in the film-forming reaction. Ethyl acetoacetate is used to improve the ability of cross-linking, thereby synergistically improving the bonding strength between titanium alloy TC4 and the organic paint film.
[0043] In this embodiment, the zirconium-containing compound and sodium dihydrogen phosphate can produce zirconium phosphate, which is soluble in organic acids, increases the content of Zr-O bonding, and increases the ratio of Zr-O-Me bonding at the interface between the sol-gel conversion film layer and the titanium alloy TC4. Therefore, there needs to be an appropriate ratio between sodium dihydrogen phosphate and the zirconium-containing compound, otherwise the solution will either precipitate or fail to increase the bonding content.
[0044] The cross-linking monomer of the β-dihydroxy structure in ethyl acetoacetoxy methacrylate is bonded to the inorganic component, and is easy to undergo cross-linking reaction with other C=C double bonds, and the polymerization process is easy to control, and the self-cross-linking efficiency is high. Adding ethyl acetoacetoxy methacrylate can fully combine the organic component with the inorganic component, effectively inhibit the phase separation of organic / inorganic hybrid materials, and make the sol-gel treatment agent fully cross-linked to form a three-dimensional network.
[0045] like Figure 1 As shown, this embodiment also provides a method for preparing a sol-gel treating agent, which comprises the following steps in order:
[0046] Step 1: According to the designed composition of the sol-gel treating agent, weigh each substance separately for use;
[0047] Step 2: prepare the solvent, inhibitor, and zirconium-containing compound in component A respectively; add the prepared inhibitor to the prepared solvent and mix them evenly to form a mixture of the inhibitor and the solvent; then add the prepared zirconium-containing compound to the mixture of the inhibitor and the solvent and mix them evenly to form component A;
[0048] Step 3: prepare the solvent, the compatibilizer and the siloxane in component B respectively; mix the prepared siloxane and the prepared compatibilizer evenly to form a mixture of the siloxane and the compatibilizer; then add the mixture of the siloxane and the compatibilizer to the prepared solvent and mix evenly to form component B;
[0049] Step 4: Add component B to component A, mix well and let stand to form a sol-gel treating agent.
[0050] The pH value of the component A is 3.0, and the pH value of the component B is 7.0; the standing time after the components A and B are evenly mixed is 30 minutes, and the standing temperature is 15°C.
[0051] like Figure 1 As shown, this embodiment also provides a method for using a sol-gel treating agent, which includes the following steps in order:
[0052] Step (1): pretreating the surface of titanium alloy TC4 by sand blasting method;
[0053] Step (2): coating the sol-gel treatment agent on the surface of the pretreated titanium alloy TC4 by a spraying method to form a continuous sol-gel liquid film layer, and after maintaining it for a certain period of time, using compressed air to blow dry the sol-gel film layer to remove excess liquid; Step (3): curing the sol-gel treatment agent from which the excess liquid has been removed, and after the curing is completed, a continuous sol-gel conversion film layer can be formed on the surface of the titanium alloy TC4;
[0054] Step (4) spraying an organic paint film on the sol-gel conversion film layer.
[0055] The thickness of the sol-gel liquid film layer is 1 mm, the holding time is 1 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 0.03 μm; the curing temperature is room temperature, the curing time is 30 min, and the thickness of the cured sol-gel conversion film layer is 0.03 μm. Component A and component B can be mixed 168 hours before coating the sol-gel treatment agent on the pretreated titanium alloy TC4 surface.
[0056] In this embodiment, the sol-gel treatment agent is applied to the surface of the titanium alloy TC4 under the conditions of construction environment temperatures of -8°C, 15°C and 28°C, and the prepared sol-gel conversion film layer is uniform, continuous and complete. Then, the organic paint film is sprayed and soaked in deionized water at 60°C for 192 hours. The bonding strength of the paint film is tested. The bonding strength test standard refers to GB / T5210. The test results show that the bonding strength between the titanium alloy TC4 and the organic paint film reaches level 0 under the conditions of construction environment temperatures of -8°C, 15°C and 28°C. The cross-hatch morphology is as follows Figure 2 As shown, (a) is the construction environment temperature of -8°C, (b) is the construction environment temperature of 15°C, and (c) is the construction environment temperature of 28°C. Figure 2 It can be seen that there is no obvious peeling of the organic paint, which shows that the adhesion of the paint film is very strong.
[0057] In the process of preparing the sol-gel treating agent and in the process of using the sol-gel treating agent in this embodiment, no special requirements are made on the mixing parameters of the substances (such as mixing time, stirring speed, mixing temperature, etc.), compressed air drying parameters, alloy surface pretreatment parameters, etc.
[0058] The sol-gel treating agent of this embodiment has the ability to simultaneously improve the cross-linking ability of the sol-gel and the metal covalent bond content of the conversion film layer. It has a fast film-forming speed, a wide range of construction environment temperature, does not require too many process parameters to be limited (for example, when mixing various substances, there is no need to limit the stirring speed, stirring temperature, stirring time, etc.), and has high paint film bonding strength.
[0059] Embodiment 2:
[0060] According to another preferred embodiment of the sol-gel treating agent and its preparation method and use method of the present invention, the composition, principle, preparation method, use method, beneficial effects, etc. of the sol-gel treating agent are basically the same as those of the first embodiment, except that:
[0061] The formula of the sol-gel treating agent includes component A and component B. The mass percentage of each substance in the sol-gel treating agent is 95 wt% of component A and 5 wt% of component B. Component A includes a solvent, an inhibitor and a zirconium-containing compound, and component B includes a solvent, a compatibilizer and siloxane.
[0062] The mass percentages of the substances in component A are as follows: the solvent accounts for 97 wt%, the inhibitor accounts for 2 wt%, and the zirconium-containing compound accounts for 1 wt%. The solvent in component A is a mixture of anhydrous ethanol and deionized water, and the anhydrous ethanol and the deionized water account for 35 wt% and 65 wt% of the solvent in component A respectively; the inhibitor in component A is a mixture of organic acid and phosphate, and the organic acid and the phosphate account for 87.4% and 12.6% of the inhibitor in component A respectively, and the mass ratio of the phosphate to the zirconium-containing compound is 1:4. The organic acid is acetic acid, the phosphate is potassium dihydrogen phosphate, and the zirconium-containing compound is potassium fluorozirconate.
[0063] The mass percentages of the substances in the component B are as follows: the solvent accounts for 59 wt%, the compatibilizer accounts for 1 wt%, and the siloxane accounts for 40 wt%. The solvent in the component B is anhydrous ethanol; the compatibilizer is ethyl acetoacetate methacrylate; and the siloxane is 3-aminopropyltriethoxysilane.
[0064] For the preparation method of the sol-gel treating agent: the pH value of the component A is 4.0, and the pH value of the component B is 6.0; the standing time after the components A and B are evenly mixed is 40 minutes, and the standing temperature is 35°C.
[0065] Method for using the sol-gel treating agent: the thickness of the sol-gel liquid film layer is 2 mm, the holding time is 2 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 0.08 μm; the curing temperature is room temperature, the curing time is 40 min, and the thickness of the sol-gel conversion film layer after curing is 0.08 μm.
[0066] Embodiment three:
[0067] According to another preferred embodiment of the sol-gel treating agent and its preparation method and use method of the present invention, the composition, principle, preparation method, use method, beneficial effects, etc. of the sol-gel treating agent are basically the same as those of the first embodiment, except that:
[0068] The formula of the sol-gel treating agent includes component A and component B. The mass percentage of each substance in the sol-gel treating agent is 90 wt% of component A and 10 wt% of component B. Component A includes a solvent, an inhibitor and a zirconium-containing compound, and component B includes a solvent, a compatibilizer and siloxane.
[0069] The mass percentages of the substances in the component A are as follows: the solvent accounts for 90 wt%, the inhibitor accounts for 5 wt%, and the zirconium-containing compound accounts for 5 wt%. The solvent in the component A is a mixture of anhydrous ethanol and deionized water, and the anhydrous ethanol and the deionized water account for 25 wt% and 75 wt% of the solvent in the component A respectively; the inhibitor in the component A is a mixture of an organic acid and a phosphate, and the organic acid and the phosphate account for 83.4% and 16.6% of the inhibitor in the component A respectively, and the mass ratio of the phosphate to the zirconium-containing compound is 1:6. The organic acid is acetic acid, the phosphate is sodium dihydrogen phosphate, and the zirconium-containing compound is zirconium n-propoxide.
[0070] The mass percentage of each substance in the component B is 50wt% of the solvent, 2wt% of the compatibilizer, and 48wt% of the siloxane. The solvent in the component B is anhydrous ethanol; the compatibilizer is ethyl acetoacetate methacrylate; and the siloxane is γ-methacryloxypropyltrimethoxysilane.
[0071] For the preparation method of the sol-gel treating agent: the pH value of the component A is 2.0, and the pH value of the component B is 5.0; the standing time after the components A and B are evenly mixed is 40 minutes, and the standing temperature is 25°C.
[0072] Method for using the sol-gel treating agent: the thickness of the sol-gel liquid film layer is 1.5 mm, the holding time is 1.5 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 0.09 μm; the curing temperature is room temperature, the curing time is 40 min, and the thickness of the sol-gel conversion film layer after curing is 0.09 μm.
[0073] Embodiment 4:
[0074] According to another preferred embodiment of the sol-gel treating agent and its preparation method and use method of the present invention, the composition, principle, preparation method, use method, beneficial effects, etc. of the sol-gel treating agent are basically the same as those of the first embodiment, except that:
[0075] The alloy selected is aluminum alloy 2024-T3.
[0076] The formula of the sol-gel treating agent includes component A and component B. The mass percentage of each substance in the sol-gel treating agent is 85 wt% of component A and 15 wt% of component B. Component A includes a solvent, an inhibitor and a zirconium-containing compound, and component B includes a solvent, a compatibilizer and siloxane.
[0077] The mass percentages of the substances in the component A are as follows: the solvent accounts for 85 wt%, the inhibitor accounts for 7 wt%, and the zirconium-containing compound accounts for 8 wt%. The solvent in the component A is a mixture of anhydrous ethanol and deionized water, and the anhydrous ethanol and the deionized water account for 30 wt% and 70 wt% of the solvent in the component A respectively; the inhibitor in the component A is a mixture of an organic acid and a phosphate, and the organic acid and the phosphate account for 77.1% and 22.9% of the inhibitor in the component A respectively, and the mass ratio of the phosphate to the zirconium-containing compound is 1:5. The organic acid is acetic acid, the phosphate is sodium dihydrogen phosphate, and the zirconium-containing compound is zirconium n-propoxide.
[0078] The mass percentage of each substance in the component B is 45 wt% of the solvent, 2 wt% of the compatibilizer, and 53 wt% of the siloxane. The solvent in the component B is anhydrous ethanol; the compatibilizer is ethyl acetoacetate methacrylate; and the siloxane is γ-methacryloxypropyltrimethoxysilane.
[0079] For the preparation method of the sol-gel treating agent: the pH value of the component A is 4.0, and the pH value of the component B is 8.0; the component A and the component B are evenly mixed and allowed to stand for 40 minutes at a temperature of 20°C.
[0080] Method for using the sol-gel treating agent: the thickness of the sol-gel liquid film layer is 2 mm, the holding time is 2 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 2 μm; the curing temperature is room temperature, the curing time is 40 min, and the thickness of the sol-gel conversion film layer after curing is 2 μm.
[0081] Embodiment five:
[0082] According to another preferred embodiment of the sol-gel treating agent and its preparation method and use method of the present invention, the composition, principle, preparation method, use method, beneficial effects, etc. of the sol-gel treating agent are basically the same as those of the first embodiment, except that:
[0083] The alloy selected is aluminum alloy 2024-T3.
[0084] The formula of the sol-gel treating agent includes component A and component B. The mass percentage of each substance in the sol-gel treating agent is 95 wt% of component A and 5 wt% of component B. Component A includes a solvent, an inhibitor and a zirconium-containing compound, and component B includes a solvent, a compatibilizer and siloxane.
[0085] The mass percentage of each substance in the component A is 85 wt% of the solvent, 5 wt% of the inhibitor, and 10 wt% of the zirconium-containing compound. The solvent in the component A is a mixture of anhydrous ethanol and deionized water, and the anhydrous ethanol and the deionized water account for 20 wt% and 80 wt% of the solvent in the component A respectively; the inhibitor in the component A is a mixture of an organic acid and a phosphate, and the organic acid and the phosphate account for 80 wt% and 20 wt% of the inhibitor in the component A respectively, and the mass ratio of the phosphate to the zirconium-containing compound is 1:10. The organic acid is acetic acid, the phosphate is sodium dihydrogen phosphate, and the zirconium-containing compound is zirconium n-propoxide.
[0086] The mass percentage of each substance in the component B is 55 wt% of the solvent, 3 wt% of the compatibilizer, and 42 wt% of the siloxane. The solvent in the component B is anhydrous ethanol; the compatibilizer is ethyl acetoacetate methacrylate; and the siloxane is γ-methacryloxypropyltrimethoxysilane.
[0087] For the preparation method of the sol-gel treating agent: the pH value of the component A is 4.0, and the pH value of the component B is 7.0; the standing time after the components A and B are evenly mixed is 40 minutes, and the standing temperature is 35°C.
[0088] Method for using the sol-gel treating agent: the thickness of the sol-gel liquid film layer is 1 mm, the holding time is 1 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 1 μm; the curing temperature is room temperature, the curing time is 40 min, and the thickness of the sol-gel conversion film layer after curing is 1 μm.
[0089] Special note: The technical solution of the present invention involves many parameters, and the synergistic effects between the various parameters need to be comprehensively considered to obtain the beneficial effects and significant progress of the present invention. Moreover, the value ranges of the various parameters in the technical solution are obtained after a large number of experiments. For each parameter and the combination of each parameter, the inventor has recorded a large amount of experimental data. Due to space limitations, the specific experimental data will not be disclosed here.
[0090] It is not difficult for those skilled in the art to understand that the sol-gel treatment agent and its preparation method and use method of the present invention include any combination of the invention content and specific implementation method of the above-mentioned invention specification and the various parts shown in the drawings. Due to the limited space and to make the specification concise, the various schemes composed of these combinations are not described one by one. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sol-gel treating agent comprising component A and component B, Features: The mass percentage of each substance in the sol-gel treating agent is 80-95wt% of component A and 5-20wt% of component B; the component A includes a solvent, an inhibitor and a zirconium-containing compound, and the component B includes a solvent, a compatibilizer and siloxane; The mass percentage of each substance in the component A is 80-97wt% of the solvent, 2-10wt% of the inhibitor, and 1-10wt% of the zirconium-containing compound; the inhibitor in the component A is a mixture of an organic acid and a phosphate, the organic acid includes any one or more of citric acid, acetic acid, oxalic acid, and phytic acid, the phosphate includes sodium dihydrogen phosphate and / or potassium dihydrogen phosphate; the zirconium-containing compound includes any one or more of zirconium n-propoxide, fluorozirconic acid, potassium fluorozirconate, and sodium fluorozirconate; The mass percentage of each substance in the component B is as follows: the solvent accounts for 37-59wt%, the compatibilizer accounts for 1-3wt%, and the siloxane accounts for 40-60wt%; the compatibilizer is a methacrylate functional group organic substance, and the methacrylate functional group organic substance is acetoacetoxyethyl methacrylate; the siloxane includes any one or more of γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and 3-aminopropyltriethoxysilane.
2. The sol-gel treating agent according to claim 1, Features: The solvent in component A is deionized water or a mixture of anhydrous ethanol and deionized water, wherein the mass percentages of the anhydrous ethanol and the deionized water in the solvent in component A are 15-35wt% and 65-85wt%, respectively; the mass percentages of the organic acid and the phosphate in the inhibitor in component A are 60-90wt% and 10-40wt%, respectively.
3. The sol-gel treating agent according to claim 2, Features: The solvent in the component B is anhydrous ethanol.
4. A method for preparing a sol-gel treating agent, Features: The sol-gel treating agent is the sol-gel treating agent according to any one of claims 1 to 3, and comprises the following steps in chronological order: Step 1: According to the designed composition of the sol-gel treating agent, weigh each substance separately for use; Step 2: prepare the solvent, inhibitor, and zirconium-containing compound in component A respectively; add the prepared inhibitor to the prepared solvent and mix them evenly to form a mixture of the inhibitor and the solvent; then add the prepared zirconium-containing compound to the mixture of the inhibitor and the solvent and mix them evenly to form component A; Step 3: prepare the solvent, the compatibilizer and the siloxane in component B respectively; mix the prepared siloxane and the prepared compatibilizer evenly to form a mixture of the siloxane and the compatibilizer; then add the mixture of the siloxane and the compatibilizer to the prepared solvent and mix evenly to form component B; Step 4: Add component B to component A, mix well and let stand to form a sol-gel treating agent.
5. The method for preparing the sol-gel treating agent according to claim 4, Features: The pH value of the component A is 2.0-4.0, and the pH value of the component B is 5.0-8.0; the standing time after the components A and B are evenly mixed is not less than 30 minutes, and the standing temperature is 15-35°C.
6. A method for using a sol-gel treatment agent, Features: The sol-gel treating agent is the sol-gel treating agent according to any one of claims 1 to 3, and comprises the following steps in chronological order: Step (1): pretreating the alloy surface by sandblasting, grinding, deoxidation or polishing; Step (2): coating the pretreated alloy surface with a sol-gel treatment agent by spraying, brushing or dipping to form a continuous sol-gel liquid film layer, maintaining the film layer for a certain period of time, and then drying the sol-gel film layer with compressed air to remove excess liquid; Step (3): curing the sol-gel treatment agent from which excess liquid has been removed, and after the curing is completed, a continuous sol-gel conversion film layer can be formed on the alloy surface; Step (4) spraying an organic paint film on the sol-gel conversion film layer.
7. The method for using the sol-gel treating agent according to claim 6, Features: The alloy is a titanium alloy or an aluminum alloy; the thickness of the sol-gel liquid film layer is 1-2 mm, the holding time is 1-2 min, and the thickness of the sol-gel liquid film layer after removing excess liquid is 0.03-2 μm; the curing temperature is room temperature, the curing time is not less than 30 min, and the thickness of the cured sol-gel conversion film layer is 0.03-2 μm.