Concrete mortar for repairing bridge expansion joints and preparation process of concrete mortar
By preparing concrete mortar for bridge expansion joint repair with high bond strength and impact resistance, the problem of easy cracking and deformation of bridge expansion joint repair materials is solved, and the stable repair and long-term use requirements of bridge expansion joints are achieved.
Patent Information
- Application Number
- CN202411044626.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Bridge expansion joint repair materials are prone to cracking, deformation and other problems during long-term use, and their adhesion to the bridge surface is poor, which affects the repair effect and service life.
A concrete mortar for repairing bridge expansion joints and its preparation process are adopted, by using silicate cement, sulfoaluminate cement, ore powder, silica fume, fly ash, quartz sand, tackifier, composite fiber, water reduction Mix agent, retarder and defoaming agent to prepare concrete mortar with high bond strength and impact resistance, and use nanosilica and 3-aminopropyltrimethoxysilane to coordinately modify fibers, reinforce fibers and cement The bonding force of the base material and the chemical reaction between the epoxy groups in the tackifier and the fibers improve the mechanical properties of the mortar.
It significantly improves the bonding strength and impact resistance of concrete mortar, ensures that the repaired bridge expansion joints can withstand the loads of vehicles and pedestrians, extend the service life, and improves the filling effect and stability.
Smart Images

Figure BDA0004973181440000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bridge building materials, in particular to concrete mortar for repairing bridge expansion joints and a preparation process thereof. Background Art
[0002] As one of the important components of the bridge superstructure, the bridge expansion joint is an important auxiliary structure that ensures the free deformation of the bridge deck and plays the role of reinforcing both ends and filling the gap. The concrete of the bridge expansion joint often suffers from wear, broken plates, impact and fatigue damage, and the probability of repeated damage after repair is very high. Therefore, the repair of expansion joints has always been a difficult problem to solve.
[0003] At present, the main forms of bridge expansion joint repair are as follows: ordinary concrete filling, fiber concrete filling, modified asphalt filling and polymer (resin) concrete filling. However, some filling materials may crack, deform and other problems during long-term use, affecting the repair effect and service life. In addition, the poor adhesion of the filling material to the bridge surface may cause the filling layer to delaminate or peel off from the substrate, thus affecting the repair effect.
[0004] Therefore, we propose a concrete mortar for repairing bridge expansion joints and a preparation process thereof. Summary of the invention
[0005] The object of the present invention is to provide a concrete mortar for repairing bridge expansion joints and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A preparation process of concrete mortar for repairing bridge expansion joints comprises the following steps:
[0008] Mix silicate cement, sulphoaluminate cement, mineral powder, silica fume, fly ash, quartz sand, viscosity enhancer, composite fiber, water reducer, retarder and defoamer evenly, add water, stir for 1-5 minutes, and obtain concrete mortar.
[0009] Furthermore, the concrete mortar includes the following components by weight: 350-450 parts of silicate cement, 20-50 parts of sulphoaluminate cement, 5-15 parts of mineral powder, 10-25 parts of silica fume, 20-50 parts of fly ash, 450-550 parts of quartz sand, 10-30 parts of viscosity enhancer, 4-8 parts of composite fiber, 2-4 parts of water reducer, 0.5-1.0 parts of retarder, 0.3-0.5 parts of defoamer, and 80-120 parts of water.
[0010] Furthermore, the preparation method of the tackifier is as follows:
[0011] Step 1: Heat anhydrous ethanol, deionized water, 3-glycidylpropylmethyldimethoxysilane and dimethyldimethoxysilane to 70-80°C, add dibutyltin dilaurate, react for 4-6 hours, then add vinyldimethylethoxysilane, capping reaction for 3-5 hours, and vacuum rotary evaporation to obtain a double bond-containing compound;
[0012] Step 2: Evenly mix acrylic acid, acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, a double bond compound and deionized water, add sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether and mix evenly, ultrasonically emulsify for 10-20 minutes, use sodium hydroxide solution to adjust the system pH to 7-8, introduce nitrogen, heat to 65-75°C, drip initiator aqueous solution, drip for 40-60 minutes, keep warm for reaction for 3-5 hours, cool to room temperature, demulsify, filter, wash and dry to obtain a tackifier.
[0013] In the above technical scheme, 3-glycidylpropylmethyldimethoxysilane, dimethyldimethoxysilane and vinyldimethylethoxysilane are used as raw materials, and double-bond compounds containing epoxy groups are prepared by hydrolysis and condensation; acrylic acid, acrylamide, 2-acrylamido-2-methylpropanesulfonic acid and double-bond compounds are selected as copolymerization monomers, and a large number of hydrophilic groups with strong polarity such as carboxyl groups, amide groups and sulfonic acid groups can be introduced into the polymer molecular chain. The hydrophilic groups form hydrogen bonds with water molecules, and the free water molecules are adsorbed and fixed on the polymer molecular chain, thereby playing a certain role in viscosity increase and water retention.
[0014] Furthermore, in step 1, the double bond-containing compound includes the following components by weight: 13-14 parts of anhydrous ethanol, 2-3 parts of deionized water, 5-6 parts of 3-glycidylpropylmethyldimethoxysilane, 5.5-6.5 parts of dimethyldimethoxysilane, 6-7 parts of vinyldimethylethoxysilane, and 0.01-0.03 parts of dibutyltin dilaurate.
[0015] Furthermore, in step 2, the tackifier includes the following components by weight: 1-4 parts of acrylic acid, 4-12 parts of acrylamide, 3-8 parts of 2-acrylamido-2-methylpropane sulfonic acid, 2-6 parts of double bond-containing compounds, 100-200 parts of deionized water, 1.4-2.0 parts of sodium dodecyl sulfate, 0.1-0.5 parts of fatty alcohol polyoxyethylene ether, and 5-15 parts of an initiator aqueous solution.
[0016] Furthermore, the concentration of the initiator aqueous solution is 2-5wt%, and the initiator is azobisisobutylimidazoline hydrochloride.
[0017] Furthermore, the composite fiber is compounded by 1-3 parts by mass of polypropylene fiber and 3-5 parts by mass of basalt fiber.
[0018] Furthermore, the composite fiber is subjected to modification treatment, and the specific modification process is as follows:
[0019] Step (1): under nitrogen protection, polypropylene fiber and xylene are mixed evenly, swelled at 70-80° C. for 1-2 hours, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; basalt fiber is heated at 250-300° C. for 1-2 hours, cooled to room temperature, immersed in acetone solution for 1-2 hours, washed, and dried to obtain pretreated basalt fiber;
[0020] Step (2): the pretreated polypropylene fiber and the pretreated basalt fiber are mixed evenly, a mixed solution of anhydrous ethanol, deionized water and 3-aminopropyltrimethoxysilane is added, and then nano-silicon dioxide is added, and the mixture is reacted at 55-65° C. for 4-6 hours, and after filtering, washing and drying, an amino composite fiber is obtained;
[0021] Step (3): Under nitrogen protection, the amino composite fiber, succinic anhydride and diethanolamine are mixed evenly, reacted at 115-125° C. for 6-8 hours, and then diethylenetriamine is added, and reacted at 105-115° C. for 10-12 hours to obtain a modified composite fiber.
[0022] In the above technical scheme, the polypropylene fiber and the basalt fiber are pretreated to improve the micro-roughness of the fiber surface; then, the surface of the pretreated polypropylene fiber and the pretreated basalt fiber are modified by nano-silicon dioxide and 3-aminopropyltrimethoxysilane to obtain amino composite fibers. Nano-silicon dioxide can further increase the surface roughness of the fiber due to its small particle size and high surface activity, improve the wetting effect between the fiber and the cement-based material, promote the stress transfer between the fiber and the cement-based material, and thus increase the fiber. The bonding strength with the interface of cement-based materials; finally, succinic anhydride and diethanolamine react to form hyperbranched macromolecules, which are grafted onto the amino composite fibers, and the toughness of the hyperbranched macromolecules is used to improve the impact resistance of the material; at the same time, the secondary amine of diethylenetriamine is reacted with the terminal hydroxyl groups of the hyperbranched molecules to form amino-terminated hyperbranched composite fibers, i.e. modified fibers, so that chemical reaction anchor points are formed on the fibers, which can further react with the epoxy groups in the tackifier, thereby enhancing the bonding force between the two, thereby improving the mechanical properties of the concrete mortar.
[0023] Furthermore, in the step (1), the mass ratio of the polypropylene fiber to xylene is 1:(30-40).
[0024] Furthermore, in step (2), the amino composite fiber includes the following components by weight: 1-3 parts of pretreated polypropylene fiber, 3-5 parts of pretreated basalt fiber, 14-22 parts of anhydrous ethanol, 1.5-2.5 parts of deionized water, 0.5-1.0 parts of 3-aminopropyltrimethoxysilane, and 0.10-0.25 parts of nano-silicon dioxide.
[0025] Furthermore, in step (3), the modified composite fiber comprises the following components by weight: 4-8 parts of amino composite fiber, 6-12 parts of succinic anhydride, 8-16 parts of diethanolamine, and 12-24 parts of diethylenetriamine.
[0026] Furthermore, the water reducer is a polycarboxylate water reducer.
[0027] Furthermore, the retarder is boric acid.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. A concrete mortar for repairing bridge expansion joints and a preparation process thereof of the present invention utilizes nano-silicon dioxide and 3-aminopropyltrimethoxysilane to synergistically modify the surfaces of pretreated polypropylene fibers and pretreated basalt fibers to obtain amino composite fibers, thereby enhancing the interfacial bonding between the composite fibers and cement-based materials; hyperbranched macromolecules are grafted onto the amino composite fibers to improve the impact resistance of the materials; and at the same time, secondary amines of diethylenetriamine are reacted with terminal hydroxyl groups of hyperbranched molecules to introduce amino groups to obtain amino-terminated hyperbranched composite fibers, i.e., modified fibers, so that chemical reaction anchor points are formed on the fibers, which can react with epoxy groups in a tackifier, thereby enhancing the bonding force between the two, thereby improving the bonding strength and impact resistance of the concrete mortar, and ensuring that the repaired bridge expansion joints can withstand the loads of vehicles and pedestrians.
[0030] 2. A concrete mortar for repairing expansion joints of bridges and its preparation process of the present invention use acrylic acid, acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and double-bond compounds as comonomers to obtain a tackifier containing epoxy groups. The tackifier molecular chain contains a large number of polar hydrophilic groups such as carboxyl groups, amide groups, and sulfonic acid groups. The groups can form hydrogen bonds with water molecules, effectively adsorb and fix free water molecules, thereby improving the water retention performance of the concrete mortar. At the same time, the introduction of the tackifier achieves good bonding between the polymer and the cement-based material, increases the adhesion between the repair concrete and the raw materials, and improves the mechanical properties and stability of the repair mortar; by fixing the free water molecules, the hydrophilic group improves the fluidity and plasticity of the repair mortar, which is conducive to fully filling the expansion joints of the bridge, thereby improving the repair effect.
[0031] 3. A concrete mortar for repairing bridge expansion joints of the present invention and a preparation process thereof, by using silicate cement and fast-hardening sulphoaluminate cement composite cementitious material as the main body, mineral powder, silica powder, fly ash as admixtures, quartz sand as filler, and then adding thickeners, composite fibers and other additives, the prepared concrete mortar has excellent early and late strength performance, and at the same time has excellent impact resistance, which can meet the requirements of rapid repair and long-term use of bridge expansion joint anchoring concrete. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In this embodiment, silicate cement: P·O 42.5 grade, sourced from Hunan Xindingli New Materials Technology Co., Ltd.; sulphoaluminate cement: R.SAC 42.5 grade, sourced from Henan Hao Nai Building Materials Co., Ltd.; mineral powder: S95 grade mineral powder, sourced from Shandong Kefa Building Materials Co., Ltd.; silica ash: item number GWF13, particle size 350-400 mesh, sourced from Hebei Si Ruite Mineral Products Co., Ltd.; fly ash: first-class fly ash, particle size 200-300 mesh, sourced from Jining Hengzhi New Building Materials Co., Ltd.; quartz sand: particle size 40-70 mesh, sourced from Changxing Qingsheng Calcium Industry Co., Ltd.; water reducer: powdered polycarboxylic acid water reducer, model PC-1030, sourced from Suzhou Xing Bang Chemical Building Materials Co., Ltd.; defoamer: silicone defoamer BYK-088; polypropylene fiber: fiber diameter 2.5μm, length 5mm, sourced from Shanghai Lingyu Building Materials Co., Ltd.; basalt fiber: chopped fiber, length 6mm, monofilament diameter 15μm, sourced from Tai'an Songze Composite Materials Co., Ltd.; nano-silica: water-based nano-SiO2, particle size 20-30nm, sourced from Shanghai Xiaohuang Nano Technology Co., Ltd.; fatty alcohol polyoxyethylene ether: AEO-9, sourced from BASF (China) Co., Ltd.
[0034] In the following examples and comparative examples, 1 part is equal to 10 g.
[0035] Embodiment 1: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following process:
[0036] 350 parts of Portland cement, 20 parts of sulphoaluminate cement, 5 parts of mineral powder, 10 parts of silica fume, 20 parts of fly ash, 450 parts of quartz sand, 10 parts of viscosity enhancer, 4 parts of composite fiber (compounded by 1 part of polypropylene fiber and 3 parts of basalt fiber), 2 parts of water reducer, 0.5 parts of retarder and 0.3 parts of defoamer were mixed evenly, 80 parts of water were added, and the mixture was stirred for 1 min to obtain concrete mortar;
[0037] The preparation method of the tackifier is as follows:
[0038] Step 1: 13 parts of anhydrous ethanol, 2 parts of deionized water, 5 parts of 3-glycidylpropylmethyldimethoxysilane and 5.5 parts of dimethyldimethoxysilane are heated to 70°C, 0.01 parts of dibutyltin dilaurate are added, and the reaction is carried out for 4 hours, and then 6 parts of vinyldimethylethoxysilane are added, and the end-capping reaction is carried out for 3 hours, and a double bond-containing compound is obtained by vacuum rotary evaporation;
[0039] Step 2: Mix 1 part of acrylic acid, 4 parts of acrylamide, 3 parts of 2-acrylamido-2-methylpropanesulfonic acid, 2 parts of double bond-containing compounds and 100 parts of deionized water, add 1.4 parts of sodium dodecyl sulfate and 0.1 parts of fatty alcohol polyoxyethylene ether and mix evenly, ultrasonic emulsify for 10 minutes, use sodium hydroxide solution to adjust the system pH to 7, introduce nitrogen, heat to 65°C, add 5 parts of 2wt% initiator aqueous solution, add it for 40 minutes, keep it warm for reaction for 3 hours, cool to room temperature, demulsify, filter, wash and dry to obtain a thickener.
[0040] Embodiment 2: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following process:
[0041] Compared with Example 1, the composite fiber of Example 2 is modified, and the other steps are the same as those of Example 1;
[0042] The composite fiber is modified, and the specific modification process is as follows:
[0043] Step (1): under nitrogen protection, 1 part of polypropylene fiber and 30 parts of xylene are mixed evenly, swelled at 70° C. for 1 hour, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; 3 parts of basalt fiber are heated at 250° C. for 1 hour, cooled to room temperature, immersed in acetone solution for 1 hour, washed, and dried to obtain pretreated basalt fiber;
[0044] Step (2): 1 part of pretreated polypropylene fiber and 3 parts of pretreated basalt fiber are mixed evenly, and a mixed solution of 14 parts of anhydrous ethanol, 1.5 parts of deionized water and 0.5 parts of 3-aminopropyltrimethoxysilane is added, and then 0.10 parts of nano-silicon dioxide is added, and the mixture is reacted at 55° C. for 4 hours, and after filtering, washing and drying, an amino composite fiber is obtained;
[0045] Step (3): Under nitrogen protection, 4 parts of amino composite fiber, 6 parts of succinic anhydride and 8 parts of diethanolamine are mixed evenly, reacted at 115°C for 6 hours, and then 12 parts of diethylenetriamine are added and reacted at 105°C for 10 hours to obtain modified composite fiber.
[0046] Embodiment 3: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following process:
[0047] 400 parts of Portland cement, 35 parts of sulphoaluminate cement, 10 parts of mineral powder, 15 parts of silica fume, 40 parts of fly ash, 500 parts of quartz sand, 20 parts of viscosity enhancer, 6 parts of composite fiber (formed by 2 parts of polypropylene fiber and 4 parts of basalt fiber), 3 parts of water reducer, 0.8 parts of retarder and 0.4 parts of defoamer were mixed evenly, 100 parts of water were added, and the mixture was stirred for 3 minutes to obtain concrete mortar;
[0048] The preparation method of the tackifier is as follows:
[0049] Step 1: 13.5 parts of anhydrous ethanol, 2.5 parts of deionized water, 5.5 parts of 3-glycidylpropylmethyldimethoxysilane and 6 parts of dimethyldimethoxysilane are heated to 75°C, 0.02 parts of dibutyltin dilaurate are added, and the reaction is carried out for 4-6 hours, and then 6.5 parts of vinyldimethylethoxysilane are added, and the end-capping reaction is carried out for 4 hours, and a double bond-containing compound is obtained by vacuum rotary evaporation;
[0050] Step 2: 3 parts of acrylic acid, 8 parts of acrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of double bond-containing compounds and 150 parts of deionized water are mixed evenly, 1.6 parts of sodium dodecyl sulfate and 0.4 parts of fatty alcohol polyoxyethylene ether are added and mixed evenly, ultrasonic emulsification is performed for 15 minutes, the pH value of the system is adjusted to 7.5 with sodium hydroxide solution, nitrogen is introduced, the temperature is raised to 70°C, 10 parts of 3wt% initiator aqueous solution are added dropwise, the dripping is completed within 50 minutes, the reaction is kept warm for 4 hours, the mixture is cooled to room temperature, and a tackifier is obtained after demulsification, filtration, washing and drying;
[0051] The composite fiber is modified, and the specific modification process is as follows:
[0052] Step (1): Under nitrogen protection, 2 parts of polypropylene fiber and 70 parts of xylene are mixed evenly, swelled at 75° C. for 1.5 hours, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; basalt fiber is heated at 300° C. for 1.5 hours, cooled to room temperature, immersed in acetone solution for 1.5 hours, washed, and dried to obtain pretreated basalt fiber;
[0053] Step (2): 2 parts of pretreated polypropylene fiber and 4 parts of pretreated basalt fiber are mixed evenly, and a mixed solution of 18 parts of anhydrous ethanol, 2 parts of deionized water and 0.8 parts of 3-aminopropyltrimethoxysilane is added, and then 0.2 parts of nano-silicon dioxide is added, and the mixture is reacted at 60° C. for 5 hours, and after filtering, washing and drying, an amino composite fiber is obtained;
[0054] Step (3): Under nitrogen protection, 6 parts of amino composite fiber, 8 parts of succinic anhydride and 12 parts of diethanolamine were mixed evenly, reacted at 120°C for 7 hours, and then 18 parts of diethylenetriamine were added and reacted at 110°C for 11 hours to obtain modified composite fiber.
[0055] Embodiment 4: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following process:
[0056] 450 parts of Portland cement, 50 parts of sulphoaluminate cement, 15 parts of mineral powder, 25 parts of silica fume, 50 parts of fly ash, 550 parts of quartz sand, 30 parts of viscosity enhancer, 8 parts of composite fiber (compounded by 3 parts of polypropylene fiber and 5 parts of basalt fiber), 4 parts of water reducer, 1.0 part of retarder and 0.5 part of defoamer were mixed evenly, 120 parts of water were added, and the mixture was stirred for 5 minutes to obtain concrete mortar;
[0057] The preparation method of the tackifier is as follows:
[0058] Step 1: 14 parts of anhydrous ethanol, 3 parts of deionized water, 6 parts of 3-glycidylpropylmethyldimethoxysilane and 6.5 parts of dimethyldimethoxysilane are heated to 80°C, 0.03 parts of dibutyltin dilaurate are added, and the reaction is carried out for 6 hours, and then 7 parts of vinyldimethylethoxysilane are added, and the end-capping reaction is carried out for 5 hours, and a double bond-containing compound is obtained by vacuum rotary evaporation;
[0059] Step 2: 4 parts of acrylic acid, 12 parts of acrylamide, 8 parts of 2-acrylamido-2-methylpropanesulfonic acid, 6 parts of double bond-containing compounds and 200 parts of deionized water are mixed evenly, 2.0 parts of sodium dodecyl sulfate and 0.5 parts of fatty alcohol polyoxyethylene ether are added and mixed evenly, ultrasonic emulsification is performed for 20 minutes, the pH value of the system is adjusted to 8 with sodium hydroxide solution, nitrogen is introduced, the temperature is raised to 75°C, 15 parts of 5wt% initiator aqueous solution are added dropwise, the dripping is completed within 60 minutes, the reaction is kept warm for 5 hours, and the mixture is cooled to room temperature. After demulsification, filtration, washing and drying, a tackifier is obtained;
[0060] The composite fiber is modified, and the specific modification process is as follows:
[0061] Step (1): under nitrogen protection, 3 parts of polypropylene fiber and 120 parts of xylene are mixed evenly, swelled at 80° C. for 2 hours, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; 5 parts of basalt fiber are heated at 300° C. for 2 hours, cooled to room temperature, immersed in an acetone solution for 2 hours, washed, and dried to obtain pretreated basalt fiber;
[0062] Step (2): 3 parts of pretreated polypropylene fiber and 5 parts of pretreated basalt fiber are mixed evenly, and a mixed solution of 22 parts of anhydrous ethanol, 2.5 parts of deionized water and 1.0 parts of 3-aminopropyltrimethoxysilane is added, and then 0.25 parts of nano-silicon dioxide is added, and the mixture is reacted at 65° C. for 6 hours, and after filtering, washing and drying, an amino composite fiber is obtained;
[0063] Step (3): Under nitrogen protection, 8 parts of amino composite fiber, 12 parts of succinic anhydride and 16 parts of diethanolamine are mixed evenly, reacted at 125°C for 8 hours, and then 24 parts of diethylenetriamine are added and reacted at 115°C for 12 hours to obtain modified composite fiber.
[0064] Comparative Example 1: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following processes:
[0065] Compared with Example 3, Comparative Example 1 added 40 parts of tackifier, and the other steps were the same as Example 3.
[0066] Comparative Example 2: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following processes:
[0067] The preparation method of the tackifier is as follows:
[0068] Step 2: 3 parts of acrylic acid, 8 parts of acrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of vinyldimethylethoxysilane and 150 parts of deionized water are mixed evenly, 1.6 parts of sodium dodecyl sulfate and 0.4 parts of fatty alcohol polyoxyethylene ether are added and mixed evenly, ultrasonic emulsification is performed for 15 minutes, the pH value of the system is adjusted to 7.5 with sodium hydroxide solution, nitrogen is introduced, the temperature is raised to 70°C, 10 parts of 3wt% initiator aqueous solution are added dropwise, the dripping is completed within 50 minutes, the reaction is kept warm for 4 hours, the mixture is cooled to room temperature, and a tackifier is obtained after demulsification, filtration, washing and drying;
[0069] Compared with Example 3, Comparative Example 2 does not include step 1, and the double bond-containing compound in step 2 is replaced by vinyl dimethyl ethoxy silane of the same mass, and the other steps are the same as Example 3.
[0070] Comparative Example 3: A preparation process of concrete mortar for repairing bridge expansion joints, comprising the following processes:
[0071] The composite fiber is modified, and the specific modification process is as follows:
[0072] Step (1): Under nitrogen protection, 2 parts of polypropylene fiber and 70 parts of xylene are mixed evenly, swelled at 75° C. for 1.5 hours, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; basalt fiber is heated at 300° C. for 1.5 hours, cooled to room temperature, immersed in acetone solution for 1.5 hours, washed, and dried to obtain pretreated basalt fiber;
[0073] Step (2): 2 parts of pretreated polypropylene fiber and 4 parts of pretreated basalt fiber are mixed evenly, and a mixed solution of 18 parts of anhydrous ethanol, 2 parts of deionized water and 0.8 parts of 3-aminopropyltrimethoxysilane is added, and then 0.2 parts of nano-silicon dioxide is added, and the mixture is reacted at 60° C. for 5 hours, and after filtering, washing and drying, an amino composite fiber is obtained;
[0074] Compared with Example 3, Comparative Example 3 does not include step (3), and the other steps are the same as Example 3.
[0075] Experiment: Take the concrete mortars obtained in Examples 1-4 and Comparative Examples 1-3, prepare samples, test their properties respectively and record the test results:
[0076] The compressive strength was measured in accordance with GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", with a sample size of 160mm×40mm×40mm. The compressive strength of the samples after standard curing for 2h and 28d was tested and the data was recorded. The impact resistance was measured in accordance with GB / T 21120-2018 "Synthetic Fibers for Cement Concrete and Mortar", with a sample size of 152mm in diameter and 63.5mm in thickness. The samples were cured for 28d, and the impact test was performed and the data was recorded.
[0077] Test Results
[0078]
[0079] According to the data in the above table, we can clearly draw the following conclusions:
[0080] 1. Compared with Examples 2-4, the compressive strength and impact resistance of the product obtained in Example 1 are both reduced, indicating that the present invention can enhance the bonding between the composite fiber and the matrix material by modifying the composite fiber, thereby improving the mechanical properties of the concrete mortar.
[0081] 2. Compared with Examples 2-4, the compressive strength of the product obtained in Comparative Example 1 is reduced, which shows that increasing the amount of thickener added will reduce the mechanical properties of the mortar.
[0082] 3. Compared with Examples 2-4, the compressive strength and impact resistance of the product obtained in Example 2 are reduced, indicating that if no double bond-containing compound is added when preparing the thickener, it will lead to a lack of epoxy groups, thereby affecting its combination with the modified composite fiber; the impact resistance of the product obtained in Example 3 is reduced, indicating that compared with the amino composite fiber, the modified fiber prepared by the present invention is grafted with hyperbranched macromolecules, thereby improving the impact resistance of the material.
[0083] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of concrete mortar for repairing bridge expansion joints, Features: The steps include: Mix silicate cement, sulphoaluminate cement, mineral powder, silica fume, fly ash, quartz sand, viscosity enhancer, composite fiber, water reducer, retarder and defoamer evenly, add water, stir for 1-5 minutes, and obtain concrete mortar.
2. A preparation process for concrete mortar for repairing bridge expansion joints according to claim 1, Features: The concrete mortar comprises the following components by weight: 350-450 parts of silicate cement, 20-50 parts of sulphoaluminate cement, 5-15 parts of mineral powder, 10-25 parts of silica fume, 20-50 parts of fly ash, 450-550 parts of quartz sand, 10-30 parts of viscosity enhancer, 4-8 parts of composite fiber, 2-4 parts of water reducer, 0.5-1.0 parts of retarder, 0.3-0.5 parts of defoamer and 80-120 parts of water.
3. A preparation process for concrete mortar for repairing bridge expansion joints according to claim 2, Features: The preparation method of the tackifier is as follows: Step 1: Heat anhydrous ethanol, deionized water, 3-glycidylpropylmethyldimethoxysilane and dimethyldimethoxysilane to 70-80°C, add dibutyltin dilaurate, react for 4-6 hours, then add vinyldimethylethoxysilane, capping reaction for 3-5 hours, and vacuum rotary evaporation to obtain a double bond-containing compound; Step 2: Evenly mix acrylic acid, acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, a double bond compound and deionized water, add sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether and mix evenly, ultrasonically emulsify for 10-20 minutes, use sodium hydroxide solution to adjust the system pH to 7-8, introduce nitrogen, heat to 65-75°C, drip initiator aqueous solution, drip for 40-60 minutes, keep warm for reaction for 3-5 hours, cool to room temperature, demulsify, filter, wash and dry to obtain a tackifier.
4. A preparation process for concrete mortar for repairing bridge expansion joints according to claim 3, Features: In the step 1, the double bond-containing compound includes the following components by weight: 13-14 parts of anhydrous ethanol, 2-3 parts of deionized water, 5-6 parts of 3-glycidylpropylmethyldimethoxysilane, 5.5-6.5 parts of dimethyldimethoxysilane, 6-7 parts of vinyldimethylethoxysilane, and 0.01-0.03 parts of dibutyltin dilaurate.
5. A process for preparing concrete mortar for repairing bridge expansion joints according to claim 3, Features: In the step 2, the tackifier includes the following components by weight: 1-4 parts of acrylic acid, 4-12 parts of acrylamide, 3-8 parts of 2-acrylamido-2-methylpropanesulfonic acid, 2-6 parts of double bond-containing compounds, 100-200 parts of deionized water, 1.4-2.0 parts of sodium lauryl sulfate, 0.1-0.5 parts of fatty alcohol polyoxyethylene ether, and 5-15 parts of initiator aqueous solution.
6. A preparation process of concrete mortar for repairing bridge expansion joints according to claim 2, Features: The composite fiber is compounded by 1-3 parts by mass of polypropylene fiber and 3-5 parts by mass of basalt fiber.
7. A process for preparing concrete mortar for repairing bridge expansion joints according to claim 6, Features: The composite fiber is modified, and the specific modification process is as follows: Step (1): under nitrogen protection, polypropylene fiber and xylene are mixed evenly, swelled at 70-80° C. for 1-2 hours, filtered, washed with acetone, and dried to obtain pretreated polypropylene fiber; basalt fiber is heated at 250-300° C. for 1-2 hours, cooled to room temperature, immersed in acetone solution for 1-2 hours, washed, and dried to obtain pretreated basalt fiber; Step (2): the pretreated polypropylene fiber and the pretreated basalt fiber are mixed evenly, a mixed solution of anhydrous ethanol, deionized water and 3-aminopropyltrimethoxysilane is added, and then nano-silicon dioxide is added, and the mixture is reacted at 55-65° C. for 4-6 hours, and after filtering, washing and drying, an amino composite fiber is obtained; Step (3): Under nitrogen protection, the amino composite fiber, succinic anhydride and diethanolamine are mixed evenly, reacted at 115-125° C. for 6-8 hours, and then diethylenetriamine is added, and reacted at 105-115° C. for 10-12 hours to obtain a modified composite fiber.
8. A process for preparing concrete mortar for repairing bridge expansion joints according to claim 7, Features: In the step (2), the amino composite fiber includes the following components by weight: 1-3 parts of pretreated polypropylene fiber, 3-5 parts of pretreated basalt fiber, 14-22 parts of anhydrous ethanol, 1.5-2.5 parts of deionized water, 0.5-1.0 parts of 3-aminopropyltrimethoxysilane, and 0.10-0.25 parts of nano-silicon dioxide.
9. A process for preparing concrete mortar for repairing bridge expansion joints according to claim 7, Features: In the step (3), the modified composite fiber comprises the following components by weight: 4-8 parts of amino composite fiber, 6-12 parts of succinic anhydride, 8-16 parts of diethanolamine, and 12-24 parts of diethylenetriamine.
10. A concrete mortar for repairing bridge expansion joints obtained according to the preparation process according to any one of claims 1 to 9.
Citation Information
Patent Citations
Organosilicon-fluorine modified epoxy resin, organosilicon-fluorine sol furfural acetone composite modified coating material and preparation method thereof
CN108727943A
Concrete for repairing bridge expansion joints as well as preparation method and use method of concrete
CN114790104A
Preparation method and application of high-strength waterproof concrete for house construction
CN115159910A
Self-compacting shrinkage-compensating concrete and preparation method thereof
CN116143462A
Quick-setting repair mortar for cement concrete bridge bottom plate cracks and preparation process of quick-setting repair mortar
CN117164315A
Cited By
Quick-drying green low-carbon waterproof mortar for repairing gaps of outdoor doors and windows and preparation method of quick-drying green low-carbon waterproof mortar
CN119306457A
Anti-seepage repairing material for building expansion joints and preparation method of anti-seepage repairing material
CN120247501A
Cement-based repairing mortar material for bridge expansion joints and preparation process of cement-based repairing mortar material
CN120271302A
Concrete antirust mortar and preparation method thereof
CN121159206A
A concrete rustproof mortar and a preparation method thereof
CN121159206B