High-performance quenched and tempered steel for electric vehicle motor shaft and production method thereof
Through specific chemical composition ratios and manufacturing processes, the problem of insufficient strength and toughness of motor shaft steel at high speeds is solved, and high-performance and low-cost motor shaft steel is achieved, which is suitable for motor shafts of new energy vehicles.
Patent Information
- Application Number
- CN202310705014.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-14
AI Technical Summary
The existing steel for motor shafts is insufficient in strength and toughness when subjected to external forces at high speeds, making it difficult to meet the high-performance needs of motor shafts of new energy vehicles and is relatively expensive.
Specific chemical composition ratios and manufacturing processes are adopted, including C: 0.47-0.52%, Si: 0.40-0.55%, Mn: 0.65-0.85%, Cr: 1.00-1.30%, Ni: 0.35-0.55%, Mo: 0.13 -0.25%, V: 0.05-0.10%, Cu≤0.20%, Al: 0.015~0.035%, H≤0.00015%, O≤0.0012%, Ti≤0.002% high-performance tempered steel, and refine by converter → LF →RH vacuum degassing → continuous casting → rolling → residual temperature normalizing → tempering treatment process to ensure the high yield strength, tensile strength and elongation of the steel.
It achieves a balance of high strength, toughness and fatigue performance, reduces energy consumption and cost, and avoids quenching and cracking, and obtains a more stable and uniform tempering structure, which is suitable for electric vehicle motor shafts.
Smart Images

Figure CN116949355B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to a high-performance quenched and tempered steel for an electric vehicle motor shaft and a production method thereof. Background Art
[0002] With the rapid development of new energy vehicles, a large amount of oil and other energy consumption can be saved, which is an important measure for my country to achieve carbon neutrality and carbon peak. Combined with China's energy resource situation and the development trend of international automobile technology, it is expected that after 2025, ordinary gasoline vehicles in China will only account for about 50% of the total number of passenger cars, while new energy vehicles such as advanced diesel vehicles, gas vehicles, and biofuel vehicles will develop rapidly.
[0003] The motor shaft of an electric vehicle is one of the important parts for transmitting power. It is the main component for transmitting torque and driving the various parts of the rotor to rotate. The motor shaft must have sufficient mechanical strength and precision to complete the transmission of motor power so that there is no vibration or friction between the stator and the rotor when the motor is running. Its performance directly affects the operation of the power system of new energy vehicles. At present, the steel used for motor shafts mainly adopts carburizing steel such as 20CrMnTi, quenched and tempered steel such as 42CrMo, and non-quenched and tempered steel such as 40MnVS. This type of steel can withstand a small torque and cannot adapt to high-speed motor shafts. Some users use 40CrNiMo. Although this steel has high strength and toughness, it is expensive and does not have a competitive advantage.
[0004] The motor shaft of electric vehicles rotates at a very high speed during the transmission process. Some high-quality new energy vehicle motors can even reach a speed of more than 50,000 r / min. The motor shaft is constantly subjected to large external forces during high-speed operation. The motor shaft of new energy vehicles must have high strength, good structural uniformity, and good assembly accuracy to ensure that the motor has a long fatigue life.
[0005] Patent No. CN115094317A discloses a high wear-resistant and high strength and toughness steel, characterized in that the mass percentage of the chemical composition of the steel is: C: 0.25%-0.40%, Si: 0-0.40%, Mn: 0.30%-1.00%, Cr: 1.00%-3.00%, Mo: 0.30%-0.60%, Ni: 1.50%-2.50%, Al: 0-0.030%, B: 0-0.004%, N: 0.004%-0.010%. The diameter of the high wear-resistant and high strength and toughness steel is 150mm-300mm. The patented steel is used for locomotive shafts, which is different from the steel for electric vehicle motor shafts of the present invention. Due to the addition of relatively high Ni, Mo and other precious elements, the cost is relatively high. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-performance quenched and tempered steel for electric vehicle motor shaft and a manufacturing method thereof in view of the above-mentioned prior art. The specifications of the steel are generally Φ50-80mm. The non-metallic inclusions are rated according to the GB / T10561 standard: A coarse ≤ 2.5, B coarse, C coarse, D coarse are all ≤ 0.5, A fine ≤ 1.5, B fine, C fine, D fine are all ≤ 1.0; the austenite grain size is rated according to the GB / T6394 standard and meets the ≥ 7.0 grade; the mechanical properties of the quenched and tempered bar are sampled and tested according to GB / T228 and meet the following requirements: yield strength ≥ 800MPa, tensile strength ≥ 1000MPa, elongation ≥ 13%, cross-sectional shrinkage ≥ 55%, and Charpy longitudinal impact energy ≥ 50J.
[0007] The technical solution adopted by the present invention to solve the above problems is: a high-performance quenched and tempered steel for an electric vehicle motor shaft has a chemical composition weight percentage of C: 0.47-0.52%, Si: 0.40-0.55%, Mn: 0.65-0.85%, Cr: 1.00-1.30%, S: 0.010-0.025%, P≤0.015%, Ni: 0.35-0.55%, Mo: 0.13-0.25%, V: 0.05-0.01%, Cu≤0.20%, Al: 0.015-0.035%, H≤0.00015%, O≤0.0012%, Ti≤0.002%, and the balance is Fe and unavoidable impurity elements.
[0008] The chemical composition of the high performance quenched and tempered steel for the motor shaft of the electric vehicle of the present invention is determined as follows:
[0009] C: increases the hardenability, strength and hardness of the material, but reduces the plasticity and impact toughness of the steel. In order to achieve a reasonable combination of comprehensive properties such as material strength and toughness, the C content of the present invention is 0.47-0.52%.
[0010] Si: as a deoxidizing element, Si is also a basic solid solution strengthening element, which improves yield strength, hardenability and surface wear resistance. Therefore, the Si content of the steel of the present invention is determined to be in the range of 0.40-0.55%.
[0011] Mn: Manganese and iron form a solid solution to improve the strength and hardness of ferrite and austenite in steel. Manganese is second only to nickel in its ability to stabilize austenite and strongly increases the hardenability of steel. However, manganese has a tendency to increase the grain coarsening of steel and is sensitive to temper brittleness. Too high manganese content increases the cracking sensitivity of steel. The manganese content of the present invention is controlled at 0.65-0.85%.
[0012] Cr: Chromium increases the hardenability of steel and has a secondary hardening effect. A certain amount of chromium is added to heat-treated steel to improve the strength and hardness of the steel after quenching and tempering. Chromium can combine with carbon to form a variety of carbides, increasing the toughness of the material. The chromium content of the present invention is controlled at 1.00-1.30%.
[0013] Ni: One of the functions of Ni in steel is to improve hardenability, and another function is to improve the impact toughness of steel, and finally improve the fatigue strength of the material. However, the high price of Ni increases the cost of steel. Under the premise of ensuring the performance of the invented steel, the Ni content of the invented steel is controlled to be 0.35-0.55%.
[0014] Mo: Molybdenum increases the hardenability of materials, can improve the strength and tempering resistance of steel, and can also improve the ductility, toughness and wear resistance of steel. In addition, molybdenum improves the thermal strength of steel. The present invention controls the molybdenum content to 0.13-0.25%.
[0015] V: Vanadium exists in the form of carbides in steel. Its main function is to refine the structure and grains of steel and improve the strength and toughness of steel. Vanadium can also increase the tempering stability of quenched steel and reduce overheating sensitivity. The present invention controls the vanadium content to 0.05-0.10%.
[0016] The addition of S can improve the cutting performance of steel, but it will cause hot brittleness of steel and reduce the plasticity and toughness of steel. However, considering the requirements of the part for processing performance, the S content range is determined to be 0.010-0.025%.
[0017] P: Phosphorus is a harmful element in steel, which is easy to aggregate at the grain boundary to cause segregation, increase the temper brittleness of the steel, and significantly reduce the plasticity and toughness of the grain boundary. The phosphorus content of the present invention is controlled to be ≤0.015%.
[0018] H: Hydrogen is a harmful element in steel. Hydrogen dissolved in steel can cause defects such as hydrogen embrittlement and white spots. Hydrogen can sharply reduce the plasticity, toughness and fatigue strength of steel. In severe cases, it can cause hydrogen-induced cracking and brittle fracture. The hydrogen content of the present invention is controlled to be ≤0.00015%.
[0019] O: Oxygen is a harmful element in steel. Oxygen exists in steel in the form of FeO, MnO, SiO 2 、Al 2 O 3 The presence of inclusions such as , reduces the strength and plasticity of steel, especially has a serious impact on the fatigue strength and impact toughness of steel. The oxygen content of the present invention is controlled at ≤ 0.0012%.
[0020] Al: Aluminum is added to steel as a deoxidizer mainly for deoxidation. Its deoxidation ability is stronger than that of Si and Mn. In addition, it can refine the grains and fix the nitrogen in the steel, thereby improving the impact toughness of the steel. However, too high a content will damage the hot working properties of the steel and easily form large non-metallic inclusions that increase the brittleness of the steel. The aluminum content of the present invention is controlled at 0.015-0.035%.
[0021] Ti exists in the steel in the form of titanium carbonitride inclusions, which affects the fatigue life of gears and should be strictly controlled at a low level.
[0022] The specific production process adopted by the present invention to solve the above problems is: converter → LF refining → RH vacuum degassing → continuous casting of 240mm×240mm ingot → ingot reheating → rolling → steel residual temperature normalizing → finishing and grinding → quenching and tempering → steel bar non-destructive testing → inspection. The main processes are described as follows.
[0023] Smelting: The primary refining furnace controls the endpoint C content to be ≥0.15%, the molten steel temperature to be ≥1650℃, and pre-melted slag, strong deoxidizer and some alloys are added to the ladle during the steel-making process; the primary refining ladle is hoisted to the LF refining furnace by a crane, the bottom blowing device is connected to blow argon, 200kg of lime and other slag-making materials are added, and power is supplied for reheating. During the refining process, powdered diffusion deoxidizer is added to the slag surface to keep the slag white or grayish white, the refining time is greater than 40 minutes, and all alloy elements are fine-tuned to the target value 5 minutes before steel-making; the refined ladle is hoisted to the RH station by a crane, and the degassing time of the molten steel under high vacuum is maintained for not less than 15 minutes; after degassing, the ladle is hoisted to the soft argon blowing position, and the soft blowing time is controlled to be 15-30 minutes.
[0024] Continuous casting: The ladle is hoisted to the continuous casting ladle turntable. The pouring is protected throughout the casting process, and the superheat of the molten steel in the tundish is controlled at 15-25℃. The casting speed is controlled at 0.8-1.1m / min by adopting process measures such as automatic control of the crystallizer liquid level, electromagnetic stirring of the crystallizer, and electromagnetic stirring at the end. The casting speed is controlled at 0.8-1.1m / min to obtain qualified continuous casting billets. The billets are slowly cooled to 400-550℃ and hot sent to the steel rolling heating furnace.
[0025] Steel rolling: reheat the continuous casting billet to 1080-1150℃ and then roll it. The total heating time is more than 3.5 hours, and the soaking time is more than 1.5 hours. After the billet is descaled by high-pressure water, the rolling temperature is 1000-1050℃, the final rolling temperature is ≥850℃, and it is rolled into corresponding specifications.
[0026] Residual temperature normalizing treatment: After the steel rolling is completed, the steel is quickly passed on the cooling bed and cut into fixed lengths, then quickly collected and loaded into the steel normalizing furnace. The normalizing furnace controls the temperature at 850-880℃. After keeping warm for 1-1.5 hours according to the size, it is taken out of the furnace and air-cooled.
[0027] Bar quenching and tempering treatment: The steel is treated on a continuous induction quenching and tempering treatment line equipped with 5-stage induction quenching heating coils. The austenitizing temperature is determined to be 780-820℃ for sub-temperature quenching, and the quenching medium is water; the tempering temperature is 560-620℃, the holding time is controlled to be more than 2h, and air cooling is used.
[0028] Inspection: The non-metallic inclusions of each furnace number shall be rated according to GB / T10561 standard and meet the following requirements: A coarse ≤2.5, B coarse, C coarse, D coarse are all ≤0.5, A fine ≤1.5, B fine, C fine, D fine are all ≤1.0; the austenite grain size shall be rated according to GB / T6394 standard and meet the requirement of ≥7.0; the mechanical properties of the bars after quenching and tempering shall be sampled and inspected according to GB / T228 and meet the requirements: yield strength ≥800MPa, tensile strength ≥1000MPa, elongation ≥13%, cross-sectional shrinkage ≥55%, Charpy longitudinal impact energy ≥50J.
[0029] Compared with the prior art, the advantages of the present invention are:
[0030] 1) The present invention adopts a new composition design, starting from the influence on the heat treatment performance of steel, taking into account the fatigue performance of the motor shaft during high-speed rotation, while ensuring the hardenability of the steel, optimizing the ratio between the elements, so that the invented steel has higher strength, toughness and fatigue performance.
[0031] 2) The steel manufactured by the present invention is quickly collected after rolling for residual temperature normalizing treatment, which can avoid quenching cracking caused by large internal stress; multi-stage induction heating tempering treatment is adopted, and the temperature of sub-temperature quenching is determined according to experiments, which reduces energy consumption and cost and can obtain a more stable and uniform tempered structure; water is used as the quenching medium to replace traditional oil or soluble quenching liquid, thereby realizing green and low-carbon manufacturing.
[0032] Instruction Manual
[0033] Figure 1 This is the tempering structure diagram of Φ50mm round steel produced in Example 1 of the present invention.
[0034] Figure 2 This is a diagram of non-metallic inclusions in Φ50mm round steel produced in Example 1 of the present invention.
[0035] Figure 3 This is the austenite grain size diagram of Φ50mm round steel produced in Example 1 of the present invention.
[0036] Figure 4 This is the tempering structure diagram of the Φ40mm round steel produced in Example 2 of the present invention.
[0037] Figure 5 This is a diagram of non-metallic inclusions in Φ40mm round steel produced in Example 2 of the present invention.
[0038] Figure 6 This is the austenite grain size diagram of Φ40mm round steel produced in Example 2 of the present invention. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0040] Example 1
[0041] The high-strength motor shaft steel involved in this embodiment has a diameter of φ50 mm, and its chemical element composition is calculated by mass percentage: C: 0.51%, Si: 0.42%, Mn: 0.75%, P: 0.008%, S: 0.018%, Cr: 1.15%, Ni: 0.42%, Mo: 0.15%, V: 0.07%, Cu: 0.02%, Al: 0.022%, H: 0.00006%, O: 0.0009%, Ti: 0.0015%, and the remainder is iron and unavoidable impurity elements.
[0042] The manufacturing process of the motor shaft steel is as follows: the smelting raw materials are configured according to the chemical composition of the above-mentioned steel products, and converter smelting, LF refining, and RH vacuum degassing are carried out in sequence to obtain high-purity molten steel. After the ingot is off the line, when the surface temperature drops to 400-550℃, it is hot sent to the steel rolling heating furnace for reheating; it is rolled into φ50mm bars by 24 continuous rolling mills, and the final rolling temperature is controlled at 880-920℃. The steel bars are quickly cut on the cooling bed and then sent to the online normalizing furnace with the temperature controlled at 850-880℃. After keeping warm for 1 hour, they are taken out of the furnace for air cooling. The steel is then subjected to sub-temperature quenching + high-temperature tempering and quenching and tempering by the induction heating device.
[0043] The steel bars produced by the above manufacturing process have high strength and toughness. The quenched and tempered mechanical properties are shown in Table 1. The microstructure, non-metallic inclusions and austenite grain size are shown in Table 2. Figure 1 , Figure 2 , Figure 3 .
[0044] Table 1 Quenched and tempered mechanical properties of steel in Example 1
[0045]
[0046] Example 2
[0047] The high-strength motor shaft steel involved in this embodiment has a diameter of φ80 mm, and its chemical element composition, by mass percentage, is: C: 0.48%, Si: 0.50%, Mn: 0.81%, P: 0.011%, S: 0.022%, Cr: 1.25%, Ni: 0.51%, Mo: 0.21%, V: 0.06%, Cu: 0.02%, Al: 0.020%, H: 0.00007%, O: 0.0008%, N: 0.0042%, Ti: 0.0011%, and the remainder is iron and unavoidable impurity elements.
[0048] The manufacturing process of the motor shaft steel is as follows: the smelting raw materials are configured according to the chemical composition of the above-mentioned steel products, and converter smelting, LF refining, and RH vacuum degassing are carried out in sequence to obtain high-purity molten steel. After the ingot is off the line, when the surface temperature drops to 400-550℃, it is hot sent to the steel rolling heating furnace for reheating; it is rolled into φ80mm bars by 24 continuous rolling mills, and the final rolling temperature is controlled at 860-920℃. The steel bars are quickly cut on the cooling bed and then sent to the online normalizing furnace with the temperature controlled at 850-880℃. After keeping warm for 1.5 hours, they are air-cooled out of the furnace. The steel is then subjected to sub-temperature quenching + high-temperature tempering by the induction heating device.
[0049] The steel bars produced by the above manufacturing process have high strength and toughness. The quenched and tempered mechanical properties are shown in Table 2. The microstructure, non-metallic inclusions and austenite grain size are shown in Table 2. Figure 4 , Figure 5 , Figure 6 .
[0050] Table 2 Quenched and tempered mechanical properties of steel in Example 2
[0051]
[0052] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing high-performance quenched and tempered steel for electric vehicle motor shafts, characterized in that: The chemical composition weight percentage of the quenched and tempered steel is C: 0.47-0.52%, Si: 0.40-0.55%, Mn: 0.65-0.85%, Cr: 1.00-1.30%, S: 0.010-0.025%, P≤0.015%, Ni: 0.35-0.55%, Mo: 0.13-0.25%, V: 0.05-0.01%, Cu≤0.20%, Al: 0.015-0.035%, H≤0.00015%, O≤0.0012%, Ti≤0.002%, and the balance is Fe and unavoidable impurity elements; the method comprises the following steps: 1) Smelting: First, the raw materials are subjected to converter smelting, LF refining, and RH vacuum degassing in sequence to obtain molten steel with high purity; 2) Continuous casting: The ladle is hoisted to the continuous casting ladle turntable, and the pouring process is protected. Automatic control of the mold liquid level, electromagnetic stirring of the mold and electromagnetic stirring at the end are adopted to obtain qualified continuous casting billets. The billets are slowly cooled to 400-550℃ and hot sent to the steel rolling heating furnace; 3) Steel rolling: The continuous casting billet is reheated to 1080-1150℃ and then rolled. The total heating time is more than 3.5 hours, and the soaking time is more than 1.5 hours. After the billet is descaled by high-pressure water, the rolling temperature is 1000-1050℃, and the final rolling temperature is ≥850℃, and rolled into corresponding specifications; 4) Residual temperature normalizing treatment: After the steel is rolled, it is quickly passed through the cooling bed and cut into fixed lengths, then quickly collected and loaded into the steel normalizing furnace. The normalizing furnace controls the temperature at 850-880℃. After keeping warm for 1-1.5 hours according to the size, it is taken out of the furnace and air-cooled; 5) Bar quenching and tempering treatment: The steel is quenched and tempered on a continuous induction quenching and tempering treatment line equipped with 5-stage induction quenching heating coils. After tempering, it is air-cooled and the austenitizing temperature is determined to be 780-820℃ for sub-temperature quenching. The quenching medium is water; the tempering temperature is 560-620℃, and the holding time is controlled to be more than 2h; 6) Inspection: The non-metallic inclusions of each furnace number shall be rated according to GB / T10561 standard and meet the following requirements: A coarse ≤2.5, B coarse, C coarse, D coarse are all ≤0.5, A fine ≤1.5, B fine, C fine, D fine are all ≤1.0; the austenite grain size shall be rated according to GB / T6394 standard and meet the requirement of ≥7.0; the mechanical properties of the bars after quenching and tempering shall be sampled and inspected according to GB / T228 and meet the requirements: yield strength ≥800MPa, tensile strength ≥1000MPa, elongation ≥13%, cross-sectional shrinkage ≥55%, Charpy longitudinal impact energy ≥50J.
2. The method for producing high performance quenched and tempered steel for electric vehicle motor shaft according to claim 1, characterized in that The diameter of the quenched and tempered steel is Φ50-80mm.
3. The method for producing high performance quenched and tempered steel for electric vehicle motor shaft according to claim 1, characterized in that The non-metallic inclusions of the quenched and tempered steel are rated according to GB / T10561 standard: A coarse ≤ 2.5, B coarse, C coarse, D coarse are all ≤ 0.5, A fine ≤ 1.5, B fine, C fine, D fine are all ≤ 1.0; the austenite grain size is rated according to GB / T6394 standard and meets ≥ 7.0; the mechanical properties of the quenched and tempered bars are sampled and tested according to GB / T228 and meet the following requirements: yield strength ≥ 800MPa, tensile strength ≥ 1000MPa, elongation ≥ 13%, cross-sectional shrinkage ≥ 55%, and Charpy longitudinal impact energy ≥ 50J.
4. The method for producing high-performance quenched and tempered steel for electric vehicle motor shaft according to claim 1, characterized in that: In step 1), the content of C at the endpoint of the primary refining furnace is controlled to be ≥0.15%, and the temperature of the molten steel is ≥1650°C. Pre-melted slag, strong deoxidizer and part of the alloy are added to the ladle during the steel tapping process; the primary refining ladle is hoisted to the LF refining furnace by a crane, the bottom blowing device is connected to blow argon gas, slag-making materials are added, and power is supplied for reheating. During the refining process, a powdered diffusion deoxidizer is added to the slag surface to keep the slag white or grayish white. The refining time is greater than 40 minutes. All alloy elements are fine-tuned to the target values 5 minutes before steel tapping; the refining ladle is hoisted to the RH station by a crane, and the degassing time of the molten steel under high vacuum is maintained for not less than 15 minutes; after the degassing is completed, the ladle is hoisted to the soft argon blowing position, and the soft blowing time is controlled to be 15-30 minutes.
5. The method for producing high-performance quenched and tempered steel for electric vehicle motor shaft according to claim 1, characterized in that: Step 2) During the continuous casting process, the superheat of the molten steel in the tundish is controlled at 15-25°C, and the casting speed is controlled at 0.8-1.1 m / min.