Nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, preparation method and application thereof
The nickel-carrying high-entropy oxide catalyst prepared by ball milling and oxidative calcination reduction treatment solves the problem of high cost of precious metal catalysts, achieves the effect of high catalytic stability and high biogas conversion, and promotes the economy of biogas conversion to alcohol-friendly synthesis gas and environmentally friendly applications.
Patent Information
- Application Number
- CN202310763687.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-26
AI Technical Summary
In the prior art, precious metal catalysts that catalyze the conversion of biogas into suitable alcohol synthesis gas are costly and difficult to promote and apply, and lack cheap nickel-carrying high entropy oxide catalysts with high catalytic stability and high biogas conversion.
By ball milling organic nickel, cerium, lanthanum, magnesium, aluminum and calcium, oxidation calcination and reduction treatment were carried out to prepare a nickel element-loaded high-entropy oxide catalyst, using the synergistic effects of nickel element-based and high-entropy oxides. , improve catalytic stability and biogas conversion rate.
The prepared nickel-carrying high entropy oxide catalyst is not only cheap and easy to obtain, but also has high catalytic stability and high biogas conversion when catalyzing the conversion of biogas into a suitable alcohol synthesis gas, which reduces costs and improves the resistance to carbon deposits of the catalyst.
Smart Images

Figure CN117019161B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy catalysis, and in particular to a nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, and a preparation method and application thereof. Background Art
[0002] The energy supply in today's world is mainly based on non-renewable fossil resources. With the sharp increase in population and the rapid growth of the total economy, various resources have been used extensively. Although various fossil resources are still available for development and utilization, humans have also begun to pay attention to the shortage of non-renewable fossil fuel reserves. There are abundant biogas resources in nature. Moreover, biogas is a green and sustainable resource. As an energy consumption, it releases much less harmful gases than equivalent fossil fuels. In the long run, with the reduction of the relative price of biogas to fossil fuels and the advancement of biogas utilization technology, biogas will replace fossil energy as the main energy and chemical raw material in the 21st century. The excessive CO2 concentration produced by human activities has a great negative impact on the climate and ecological balance. With the increasing calls for environmental protection, how to reasonably utilize the CO2 produced by various energy sources to turn waste into treasure will become a problem that countries around the world generally pay attention to.
[0003] As biogas becomes the third largest energy source after oil, replacing oil with gas is an inevitable trend in the future energy and chemical industry route transfer. Biogas, whose main components are methane and carbon dioxide, is a green and easy-to-transfer energy source. Every year, 100 million tons of methane are emitted into the atmosphere through various channels around the world, and the emissions generated by human activities account for about half of the total emissions. Therefore, the rational and effective development and utilization of methane and carbon dioxide in biogas has a dual significance, which can not only effectively utilize resources, but also effectively control the greenhouse effect of methane and reduce the impact of methane on global warming.
[0004] Biogas can be processed into important chemical products as raw materials. For example, biogas steam catalytic conversion can be used to produce synthesis gas, which can be used to prepare various hydrocarbons and oxygen-containing derivatives, and can also be used to produce pure hydrogen through reprocessing and conversion. Synthesis gas refers to a mixture of carbon monoxide and hydrogen. The molar ratio of CO and H2 in the synthesis gas varies with the raw materials and the conversion method. When the molar ratio of CO and H2 is 1:2, the synthesis gas is called alcohol synthesis gas, which plays an important role in carbon-chemical industry and can be converted into liquid and gaseous fuels, bulk chemicals and high-value-added fine organic chemical products. The use of biogas as raw material to prepare alcohol synthesis gas can not only effectively reduce environmental pollution and greenhouse effect, but also generate huge economic value.
[0005] In the research on catalytic conversion of biogas into suitable alcohol synthesis gas, currently the most widely used are noble metal catalysts, such as Pd and Pt. Although the noble metal catalysts have good catalytic stability and biogas conversion rate when catalyzing the conversion of biogas into suitable alcohol synthesis gas, the cost of the noble metal catalysts is high and it is difficult to promote and apply them. Therefore, it is of great significance to develop a preparation method of a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, which is inexpensive and has high catalytic stability and high biogas conversion rate, and to use the obtained nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas to catalyze the conversion of biogas into suitable alcohol synthesis gas. Summary of the invention
[0006] The primary purpose of the present invention is to solve the problem of high cost of precious metal catalysts for catalyzing the conversion of biogas into suitable alcohol synthesis gas in the prior art, and to provide a nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas. The nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas is not only cheap and easy to obtain, but also has high catalytic stability and high biogas conversion rate when catalyzing the conversion of biogas into suitable alcohol synthesis gas.
[0007] Another object of the present invention is to provide a method for preparing a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas.
[0008] Another object of the present invention is to provide a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas in the preparation of suitable alcohol synthesis gas.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] The preparation method of the nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas comprises the following steps:
[0011] The organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source are ball-milled, and then oxidatively calcined, and then reduced to nickel element to obtain a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas;
[0012] The molar ratio of cerium, lanthanum, magnesium, aluminum and calcium metal elements in the organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source is 1:1:1:1:1;
[0013] In the nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, the mass percentage of nickel element is 5-15%.
[0014] In the present invention, the organic cerium source, lanthanum source, magnesium source, aluminum source and calcium source will form a high entropy oxide with a large specific surface area after oxidative calcination. When the nickel source is uniformly loaded on the organic cerium source, the nickel source is reduced to a nickel element by a reducing gas, and a nickel-loaded high entropy oxide catalyst that converts all components of biogas into suitable alcohol synthesis gas can be obtained.
[0015] In the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, nickel element is the catalytically active substance, high-entropy oxide is the co-catalyst, and the high-entropy oxide formed by cerium, lanthanum, magnesium, aluminum and calcium has a large number of oxygen vacancies due to its unique phase structure, synergistic effect, high-entropy effect and lattice distortion effect. The oxygen vacancies of the high-entropy oxide will assist the nickel element to have more active oxygen, thereby improving the catalytic stability and biogas conversion rate of the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas when catalyzing the conversion of biogas into suitable alcohol synthesis gas.
[0016] It is worth noting that the oxygen vacancies of the high-entropy oxide in the nickel-loaded high-entropy oxide catalyst that converts all components of biogas into suitable alcohol synthesis gas can only play a role in the presence of Ni element, promoting the production of more active oxygen to catalyze the conversion of biogas into suitable alcohol synthesis gas.
[0017] In addition, the reason why the high entropy oxide of the present invention uses rare earth metals cerium, lanthanum and alkaline earth metals magnesium and calcium is that rare earth metals and alkaline earth metals can increase the basicity of the catalyst, promote the adsorption and dissociation of CO2, and eliminate the carbon deposition and sintering problems in the process of catalyzing the conversion of biogas into alcohol synthesis gas, thereby enhancing the catalytic activity, stability and anti-carbon deposition performance of the catalyst.
[0018] In addition, the present invention evenly disperses the active components by ball milling the organic nickel source, cerium source, lanthanum source, magnesium source, aluminum source and calcium source, thereby enhancing the interaction between the active components and facilitating the formation of a uniform and stable nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, thereby improving the catalytic stability and biogas conversion rate of the nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas when catalyzing the conversion of biogas into suitable alcohol synthesis gas.
[0019] The reduction treatment can not only reduce nickel oxide to nickel element, but also further activate the high entropy effect and lattice distortion effect of high entropy oxides formed by organic cerium source, lanthanum source, magnesium source, aluminum source and calcium source, thereby further increasing the number of oxygen vacancies of the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, promoting the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas to produce more active oxygen, thereby improving the catalytic stability and biogas conversion rate of the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas when catalyzing the conversion of biogas into suitable alcohol synthesis gas.
[0020] Moreover, the reason why the present invention selects organic nickel source, cerium source, lanthanum source, magnesium source, aluminum source and calcium source instead of inorganic nickel source, cerium source, lanthanum source, magnesium source, aluminum source and calcium source including metal oxides and metal nitrates is that if metal oxides of nickel, cerium, lanthanum, magnesium, aluminum and calcium are selected, a high temperature far exceeding 800° C. is required to break the chemical bonds within the single metal oxide and realize the reaction of the single metal oxide with other types of metal oxides to form a high entropy oxide; if inorganic salts such as metal nitrates of nickel, cerium, lanthanum, magnesium, aluminum and calcium are selected, a dense and uniform mixture state cannot be obtained after ball milling, which is not conducive to the dispersion and uniform distribution of nickel in the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, thereby affecting the catalytic stability and biogas conversion rate of the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas when catalyzing the conversion of biogas into suitable alcohol synthesis gas.
[0021] The high entropy oxide of the present invention refers to an oxide with a single structure obtained by solid-dissolving five or more metal elements in an equimolar or nearly molar ratio.
[0022] The alcohol-free synthesis gas described in the present invention refers to the synthesis gas when the molar ratio of CO to H2 is 1:2.
[0023] The biogas or all components of biogas mentioned in the present invention refer to a mixed gas containing CH4 and CO2.
[0024] The biogas conversion rate of the present invention is a methane (CH4) conversion rate and a carbon dioxide (CO2) conversion rate.
[0025] Specifically, in the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, the mass percentage of nickel element is 8-12%.
[0026] Specifically, the temperature of the oxidation calcination is 500-700°C.
[0027] Specifically, the heating rate of the oxidation calcination is 3-5°C / min.
[0028] Specifically, the oxidative calcination is performed in an atmosphere containing oxygen.
[0029] Furthermore, the oxygen-containing gas is air.
[0030] Specifically, the reduction treatment is a reduction calcination treatment performed in a reducing gas atmosphere.
[0031] Furthermore, the reduction calcination temperature is 750-850°C.
[0032] Furthermore, the reduction calcination time is 1 to 3 hours.
[0033] Furthermore, the reducing gas is one or more of hydrogen, a hydrogen-nitrogen mixed gas, a hydrogen-argon mixed gas or a hydrogen-helium mixed gas.
[0034] In the present invention, the hydrogen-nitrogen mixed gas may be a hydrogen-nitrogen mixed gas with a hydrogen gas volume fraction of 5%.
[0035] Specifically, the ball milling time is 8 to 12 hours.
[0036] Specifically, the rotation speed of the ball mill is 400-600 rpm.
[0037] Specifically, the organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source are one or more of acetates, acetylacetonates or isopropoxides of nickel, cerium, lanthanum, magnesium, aluminum and calcium.
[0038] The use of the above-mentioned nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas in the preparation of suitable alcohol synthesis gas should also be within the scope of protection of the present invention.
[0039] A method for preparing alcohol synthesis gas comprises the following steps:
[0040] The nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas is used to catalyze the reaction of CH4, CO2 and water to generate suitable alcohol synthesis gas.
[0041] Specifically, the reaction temperature is 700-800°C.
[0042] Specifically, the volume ratio of CH4 and CO2 is (6~7):(3~4).
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] In the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas of the present invention, nickel element is a catalytically active substance, high-entropy oxide is a co-catalytic substance, and the high-entropy oxide formed by cerium, lanthanum, magnesium, aluminum and calcium has a large number of oxygen vacancies due to its unique phase structure, synergistic effect, high-entropy effect and lattice distortion effect. The oxygen vacancies of the high-entropy oxide can assist the nickel element to generate more active oxygen, thereby improving the catalytic stability and biogas conversion rate of the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas when catalyzing the conversion of biogas into suitable alcohol synthesis gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a TEM image of the nickel-supported high entropy oxide catalyst used in Example 1 to convert all components of biogas into suitable alcohol synthesis gas.
[0046] Figure 2This is a graph showing the conversion rate and H2 / CO molar ratio when the nickel-supported high entropy oxide catalyst catalyzes the conversion of biogas into suitable alcohol synthesis gas at different times when all components of biogas are converted into suitable alcohol synthesis gas in Example 1. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.
[0048] In the present invention, the mass percentage of nickel in the nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas is measured by inductively coupled plasma mass spectrometry ICP-MS.
[0049] Example 1
[0050] This embodiment provides a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, and the preparation method thereof comprises the following steps:
[0051] 0.83g nickel acetate, 0.95g (0.003mol) cerium acetate, 0.95g (0.003mol) lanthanum acetate, 0.43 (0.003mol) magnesium acetate, 0.61g (0.003mol) aluminum acetate and 0.48g (0.003mol) calcium acetate were ball-milled at a speed of 600rpm for 8h, and then heated to 550℃ at a heating rate of 5℃ / min in a muffle furnace under air atmosphere, oxidatively calcined for 4h, and then reduced and calcined at 800℃ for 2h in a hydrogen-nitrogen mixed gas atmosphere with a hydrogen gas volume fraction of 5%, thereby obtaining a nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas;
[0052] The molar ratio of cerium acetate, lanthanum acetate, magnesium acetate, aluminum acetate and calcium acetate is 1:1:1:1:1, that is, the molar ratio of cerium, lanthanum, magnesium, aluminum and calcium metal elements is 1:1:1:1:1; in the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, the mass percentage of nickel element is 10%.
[0053] Embodiment 2~5
[0054] Examples 2 to 5 provide different nickel-supported high entropy oxide catalysts for converting all components of biogas into suitable alcohol synthesis gas. The difference from Example 1 is that the amount of nickel acetate used is different. The difference in the amount of nickel acetate used leads to different mass percentages of nickel in the nickel-supported high entropy oxide catalysts for converting all components of biogas into suitable alcohol synthesis gas. The rest is consistent with Example 1, as shown in the following table:
[0055] Table 1 Amounts of nickel acetate used in Examples 1 to 5 and the mass percentage of nickel in the nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas
[0056]
[0057] Embodiment 6-8
[0058] Examples 6 to 8 provide different nickel-supported high entropy oxide catalysts for converting all components of biogas into suitable alcohol synthesis gas. The difference from Example 1 is that the temperature of oxidation calcination is different, and the rest is consistent with Example 1, as shown in the following table:
[0059] Table 2 Temperature of oxidative calcination of Examples 1 and 6-8
[0060]
[0061] Comparative Example 1
[0062] This comparative example provides a high entropy oxide catalyst, which differs from Example 1 in that 0.83 g of nickel acetate is not added, and the rest is consistent with Example 1.
[0063] Comparative Example 2
[0064] This comparative example provides a nickel-supported catalyst, the preparation method of which comprises the following steps:
[0065] 0.011 g of nickel oxide, 0.2024 g (0.001176 mol) of cerium oxide, 0.1916 g (0.000588 mol) of lanthanum oxide, 0.0474 g (0.001176 mol) of magnesium oxide, 0.0600 g (0.000588 mol) of aluminum oxide and 0.0660 g (0.001176 mol) of calcium oxide were ball-milled at a speed of 600 rpm in a ball mill for 6 hours, and then heated to 800° C. at a heating rate of 5° C. / min in a muffle furnace in an air atmosphere, oxidized and calcined for 4 hours, and then reduced and calcined at 800° C. for 2 hours in a hydrogen atmosphere with a volume fraction of 5%, to obtain a nickel-supported catalyst;
[0066] The molar ratio of cerium oxide, lanthanum oxide, magnesium oxide, aluminum oxide and calcium oxide is 2:1:2:1:2, that is, the molar ratio of cerium, lanthanum, magnesium, aluminum and calcium metal elements is 1:1:1:1:1.
[0067] In the nickel-loaded catalyst of this comparative example, the calcination temperature of 800°C is not enough to break the chemical bonds within a single metal oxide (cerium oxide, lanthanum oxide, magnesium oxide, aluminum oxide or calcium oxide), so as to enable the single metal oxide to react with other types of metal oxides to form a high-entropy oxide. In other words, the cerium oxide, lanthanum oxide, magnesium oxide, aluminum oxide and calcium oxide in this comparative example cannot synthesize a high-entropy oxide, and a nickel-loaded high-entropy oxide catalyst having a high-entropy oxide for converting all components of biogas into suitable alcohol synthesis gas cannot be obtained.
[0068] Sample characterization
[0069] Figure 1 TEM image of the nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas in Example 1. Figure 1 It can be seen that elemental nickel particles are evenly distributed on the surface of the reduced nickel-loaded high-entropy oxide, indicating that elemental nickel has excellent dispersibility in the nickel-loaded high-entropy oxide.
[0070] The TEM images of the nickel-supported high entropy oxide catalysts for converting all components of biogas into suitable alcohol synthesis gas in Examples 2 to 8 are similar to that in Example 1.
[0071] Performance Testing
[0072] The catalysts of the examples and comparative examples were used to catalyze the conversion of biogas into alcohol synthesis gas, and the catalytic stability test was carried out by extending the reaction time. The experimental results are shown in Table 3, where:
[0073] (1) Experiment on catalytic conversion of biogas into alcohol synthesis gas
[0074] 0.2 g of the catalyst of each embodiment or comparative example was put into a reactor, and CH4, CO2 and nitrogen with a volume ratio of 30:20:10 were continuously introduced into the reactor. At the same time, liquid water with a flow rate of 0.029 mL / h was injected into the reactor through a syringe pump, and the reaction was carried out at 750°C to obtain an appropriate alcohol synthesis gas. The generated appropriate alcohol synthesis gas was passed through a gas-liquid separator to remove residual water vapor, and then detected by gas chromatography; gas chromatography found that the appropriate alcohol synthesis gas contained H2 and CO, and then the gas chromatography was used to continuously track the content of each gas in the appropriate alcohol synthesis gas.
[0075] (2) Catalytic stability test
[0076] The stability of the catalyst of each embodiment or comparative example is characterized by comparing its initial activity (CH4 / CO2 conversion rate, % / %) at 750°C and the final activity (CH4 / CO2 conversion rate, % / %) after 100h or 500h of reaction. The closer the initial activity and the final activity are, the better the stability of the catalyst.
[0077] (3) Biogas conversion rate
[0078] The biogas conversion rate in the present invention refers to the CH4 conversion rate and the CO2 conversion rate.
[0079]
[0080]
[0081] In the above formula, (CH4 / N2) 进 Refers to the volume ratio of CH4 and N2 introduced into the reactor before the reaction, (CH4 / N2) 出 Refers to the volume ratio of CH4 and N2 remaining after the reaction; (CO2 / N2) 进 Refers to the volume ratio of CO2 and N2 introduced into the reactor before the reaction, (CO2 / N2) 出 It refers to the volume ratio of CO2 and N2 remaining after the reaction.
[0082] Table 3 Performance test results of various embodiments and comparative examples
[0083]
[0084] Note: In the above table, “CH4 / CO2 conversion rate” refers to CH4 conversion rate / CO2 conversion rate.
[0085] From Table 3, we can see that:
[0086] (1) The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas of the present invention has high catalytic stability and high biogas conversion rate when catalyzing the conversion of biogas into suitable alcohol synthesis gas;
[0087] (2) When the mass percentage of nickel is 8-12%, the nickel-supported high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas has higher catalytic stability and biogas conversion rate;
[0088] (3) When the mass percentage of nickel is 10%, the final activity (94 / 59%) of the nickel-supported high entropy oxide catalyst for converting all biogas components into suitable alcohol synthesis gas after 500 hours of catalytic conversion of biogas into suitable alcohol synthesis gas is almost the same as its initial activity (95 / 60%), indicating that the nickel-supported high entropy oxide catalyst for converting all biogas components into suitable alcohol synthesis gas has a high catalytic stability;
[0089] (4) By comparing Example 1 and Comparative Example 1, it was found that the high entropy oxide catalyst that does not contain nickel cannot catalyze the conversion of biogas into suitable alcohol synthesis gas. This is because the oxygen vacancies of the high entropy oxide in the nickel-loaded high entropy oxide catalyst that converts all components of biogas into suitable alcohol synthesis gas can only play a role in the presence of nickel, thereby promoting the production of more active oxygen to catalyze the conversion of biogas into suitable alcohol synthesis gas.
[0090] Figure 2 The graphs of conversion rate and H2 / CO molar ratio when the nickel-supported high entropy oxide catalyst catalyzes the conversion of biogas into suitable alcohol synthesis gas at different times in Example 1 are shown. Figure 2 It can be seen that in Example 1, the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas catalyzes the conversion of biogas (CH4 and CO2) into suitable alcohol gas with a H2 / CO molar ratio of 2, and within 500 hours, the average CH4 conversion rate is 95%, and the average CO2 conversion rate is 60%, indicating that the nickel-loaded high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas has excellent catalytic activity, high catalytic stability, and high biogas conversion rate.
[0091] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, characterized in that: The preparation method thereof comprises the following steps: The organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source are ball-milled, and then oxidatively calcined, and then reduced to nickel element, thereby obtaining a nickel-supported high entropy oxide catalyst capable of converting all components of biogas into suitable alcohol synthesis gas; The molar ratio of cerium, lanthanum, magnesium, aluminum and calcium metal elements in the organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source is 1:1:1:1:1; In the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, the mass percentage of nickel element is 5-15%.
2. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 1, characterized in that: In the nickel-loaded high-entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas, the mass percentage of nickel element is 8-12%.
3. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 1, characterized in that: The organic nickel source, organic cerium source, organic lanthanum source, organic magnesium source, organic aluminum source and organic calcium source are one or more of acetate, acetylacetonate or isopropoxide of nickel, cerium, lanthanum, magnesium, aluminum and calcium.
4. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 1, characterized in that: The temperature of the oxidation calcination is 500-700°C.
5. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 1, characterized in that: The oxidative calcination is performed in an atmosphere containing oxygen.
6. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 1, characterized in that: The reduction treatment is a reduction calcination treatment performed in a reducing gas atmosphere.
7. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 6, characterized in that: The reducing gas is one or more of hydrogen, hydrogen-nitrogen mixed gas, hydrogen-argon mixed gas or hydrogen-helium mixed gas.
8. The nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas according to claim 6, characterized in that: The temperature of the reduction calcination is 750-850°C.
9. Use of the nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas as claimed in any one of claims 1 to 8 in preparing suitable alcohol synthesis gas.
10. A method for preparing alcohol synthesis gas, characterized in that: The following steps are involved: A nickel-supported high entropy oxide catalyst for converting all components of biogas into suitable alcohol synthesis gas as described in any one of claims 1 to 8 is used to catalyze the reaction of CH4, CO2 and water to generate suitable alcohol synthesis gas.