Method for producing polyimide resin powder

By controlling the reaction conditions of polyimide resin powder, the problems of particle size distribution and molding processability are solved, and the dielectric loss tangent is suppressed and productivity is improved. It is suitable for applications such as high-frequency circuit substrates.

CN117043232BActive Publication Date: 2024-10-22MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280023900.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-02
Filing Date
2022-03-01
Publication Date
2024-10-22
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

It is difficult to effectively control the particle size distribution and molding processability of thermoplastic polyimide resin powder with the existing technology, leading to problems such as uneven molding, changes in dielectric constant, and low productivity.

Method used

During the manufacturing process of polyimide resin powder, the reaction conditions of the tetracarboxylic acid component and the diamine component in the alkylene glycol solvent are controlled, including setting the solid component concentration and heating rate to obtain volume average particles. Powder with diameter D50 in the range of 5 to 50 μm and good particle size distribution.

Benefits of technology

It achieves uniform particle size distribution and good formability of polyimide resin powder, suppresses the increase in dielectric loss tangent at high temperatures, and is suitable for applications such as high-frequency circuit substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117043232B_ABST
    Figure CN117043232B_ABST
Patent Text Reader

Abstract

A method for producing a polyimide resin powder, wherein the method comprises a step of reacting a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride and a diamine component (B) containing an aliphatic diamine in the presence of a solvent (C) containing an alkylene glycol solvent represented by formula (1), the step comprising the following steps: preparing a solution (a) containing the tetracarboxylic acid component (A) in the solvent (C) and a solution (b) containing the diamine component (B) in the solvent (C), respectively, and adding a solvent (a) to the solution (b). Solution (b) or solution (a) is added to solution (b) to prepare a solution (c) containing a polyimide resin precursor containing polyamic acid, and then the polyimide resin precursor containing polyamic acid is imidized by heating the aforementioned solution (c) to precipitate polyimide resin powder in the solution, the solid content concentration of the aforementioned solution (c) is 15 to 25% by mass, and the average heating rate of the aforementioned solution (c) in the temperature range of 70 to 130°C during the aforementioned heating is 0.5 to 8°C / min. (Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a straight-chain alkylene group having 2 to 6 carbon atoms, and n is an integer of 1 to 3.)#imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a polyimide resin powder, the polyimide resin powder, and a resin film obtained by using the polyimide resin powder. Background Art

[0002] Polyimide resin is a useful engineering plastic having high thermal stability, high strength, and high solvent resistance due to the rigidity, resonance stabilization, and strong chemical bonds of the molecular chain, and is used in a wide range of fields. In addition, crystalline polyimide resins can further improve their heat resistance, strength, and chemical resistance, and therefore, can be expected to be used as metal substitutes, etc. However, although polyimide resins have high heat resistance, they do not show thermoplasticity and have a problem of low molding processability.

[0003] As polyimide molding materials, high heat-resistant resins such as Vespel (registered trademark) are known (Patent Document 1), but their fluidity at high temperatures is extremely low, so they are difficult to mold and must be molded under high temperature and high pressure conditions for a long time, which is disadvantageous in terms of cost. In contrast, if a resin has a melting point and fluidity at high temperatures like a crystalline resin, it can be easily and cheaply molded.

[0004] Therefore, in recent years, polyimide resins with thermoplasticity have been reported. Thermoplastic polyimide resins have excellent molding processability in addition to the heat resistance that polyimide resins originally have. Therefore, thermoplastic polyimide resins can also be used for molded bodies used in harsh environments where general thermoplastic resins such as nylon and polyester cannot be used.

[0005] Thermoplastic polyimide resin can be formed into various shapes by hot melting. Furthermore, if the thermoplastic polyimide resin can be recovered in the form of uniform powder, it is difficult to produce uneven processing during the forming process, so it is highly useful. In recent years, a method for obtaining a uniform powdered thermoplastic polyimide resin has been studied.

[0006] For example, Patent Document 2 discloses a method for producing a polyimide resin powder, which includes: reacting a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride with a diamine component (B) containing an aliphatic diamine in the presence of a solvent (C) containing an alkylene glycol solvent represented by a specific formula. Patent Document 2 also states that a powdered polyimide resin can be produced with little agglomeration.

[0007] However, in recent years, research has been conducted on applying resin films obtained using thermoplastic polyimide resins to high-frequency circuit substrates (see, for example, Patent Document 3). On the other hand, it is known that thermoplastic polyimide resins have a high water absorption rate due to the polarity of the imide group, and therefore, when the thermoplastic polyimide resin is used to obtain a resin film, the change in the dielectric constant caused by water absorption becomes large.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2005-28524

[0011] Patent Document 2: International Publication No. 2015 / 020019

[0012] Patent Document 3: Japanese Patent Application Publication No. 2020-177987 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] When using a molding material containing thermoplastic polyimide resin powder to manufacture a film-shaped (also including sheet-shaped) molded body (resin film) for use in high-frequency circuit substrates, etc., the following methods can generally be listed: (i) a method in which the molding material containing the powder is placed in an extrusion molding machine, directly extruded and then subjected to various thermoforming to obtain a film-shaped molded body; (ii) a method in which the material containing the powder is placed in an extrusion molding machine, temporarily formed into pellets, and then subjected to various thermoforming using the pellets as a molding material to obtain a film-shaped molded body; and (iii) a method in which the molding material containing the powder is directly compression-molded using a hot pressing device to obtain a film-shaped molded body, etc.

[0015] However, if the particle size of the thermoplastic polyimide resin powder is too small, the following problems may occur: the handling property when put into an extruder, especially the bite property with the screw of the extruder, is reduced, and melt kneading is difficult. In addition, when the thermoplastic polyimide resin powder is produced, clogging of the filter cloth occurs when filtering is performed to remove the solvent, and the productivity is also reduced.

[0016] On the other hand, if the particle diameter of thermoplastic polyimide resin powder is too large, the high boiling point solvent used in manufacturing and the moisture caused by hygroscopicity are easily retained in the particle interior. Therefore, in order to remove the residual solution (high boiling point solvent, moisture) remaining in the particle interior in the drying process, high temperature drying, extended drying time, etc. are required, more energy is required, and sometimes problems such as being difficult to remove the residual solution are generated. In addition, if the residual solution remaining in the particle interior of thermoplastic polyimide resin powder is many, sometimes the following problems are generated: due to the generation of a large amount of gas in the process of obtaining a film-shaped formed body using the powder, poor forming and film appearance deterioration are caused, and discoloration / deterioration etc. occur as a starting point due to the deterioration caused by heating the residual solution.

[0017] The polyimide resin powder described in Patent Document 2 shows that it has a suitable particle size distribution, but on the other hand, no particular study has been made on a method for controlling the volume average particle size D50 to a specific range, and there is room for further study.

[0018] Therefore, an object of the present invention is to provide a method for producing a polyimide resin powder which can easily control the volume average particle diameter D50 within a specific range and has a good particle diameter distribution.

[0019] Solutions for solving problems

[0020] The present inventors have found that in a method for producing a polyimide resin powder comprising a step of reacting a tetracarboxylic acid component with a diamine component in the presence of a specific solvent, the above-mentioned problem can be solved by setting the solid content concentration of a solution containing a polyimide resin precursor containing polyamic acid prepared in the step to a specific range, and setting the average heating rate within a specific temperature range when heating the solution (c) to imidize the polyimide resin precursor containing polyamic acid to a specific range.

[0021] That is, the present invention provides a method for producing a polyimide resin powder, wherein the method comprises a step of reacting a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride and a diamine component (B) containing an aliphatic diamine in the presence of a solvent (C) containing an alkylene glycol-based solvent represented by formula (1), wherein the step comprises the following steps: preparing a solution (a) containing the tetracarboxylic acid component (A) in the solvent (C) and a solution (b) containing the diamine component (B) in the solvent (C), respectively, and then adding the solution (b) to the solution (a) or adding the solution (a) to the solution (b) to prepare a solution (c) containing a polyimide resin precursor containing polyamic acid, and then, heating the solution (c) to imidize the polyimide resin precursor containing polyamic acid, so that the polyimide resin powder is precipitated in the solution.

[0022] The solid content concentration of the solution (c) is 15 to 25% by mass, and the average temperature increase rate of the solution (c) in the temperature range of 70 to 130° C. during the heating is 0.5 to 8° C. / min.

[0023]

[0024] (Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a straight-chain alkylene group having 2 to 6 carbon atoms, and n is an integer of 1 to 3.)

[0025] Effects of the Invention

[0026] According to the manufacturing method of the present invention, a polyimide resin powder having a volume average particle size D50 in a specific range (specifically 5 to 50 μm) and having a good particle size distribution can be obtained. In addition, a resin film obtained by using a polyimide resin powder of a specific composition obtained by the manufacturing method of the present invention can suppress the increase in dielectric loss tangent at high temperatures.

[0027] The above-mentioned resin film can be applied to, for example, high-frequency circuit substrates, copper-clad laminates (CCLs), especially copper-clad laminates obtained using low-roughness (arithmetic mean roughness Ra=1μm or less, maximum height Rz=1μm or less) copper foil, printed wiring substrates, coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines and other transmission lines; microwave antennas, millimeter-wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, three-layer board antennas, microstrip antennas, patch antennas, various sensors, vehicle-mounted radars, aerospace radars, semiconductor component materials, bearing covers (coats), insulating shafts, brackets, seamless belts and other various belts; heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, low-dielectric wire covering materials, antenna covers (radar antenna covers), antenna substrates for 5G smartphones / 5G terminals, 6G smartphones / 6 5G terminal antenna substrates, chip on film (COF) flexible substrates, optical communication modules (TOSA / ROSA), 77GHz automotive millimeter wave radar antenna substrates, terahertz wave radar antenna substrates, aircraft radar antenna substrates, tracked vehicle antenna substrates, 8K-TV cables, WiGig antenna substrates, tablet terminals, notebook PCs, thin TVs, roll-up TVs, digital cameras and other mobile terminals; digital home appliances, macro cell base stations, small cell base stations, C-RAN base stations, commercial drones, long-distance mobile drones, surveillance cameras, smart glasses, smart watches, high-frequency device wafers, wireless communication equipment, Wi-Fi chips, contact sensors, indoor servers, outdoor servers, industrial robot substrates, household robot communication substrates, artificial satellites, space station communication equipment, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Example 1.

[0029] Figure 2 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Example 2.

[0030] Figure 3 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Example 3.

[0031] Figure 4 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Example 4.

[0032] Figure 5 These are the results of laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 1.

[0033] Figure 6 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 2.

[0034] Figure 7 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 3.

[0035] Figure 8 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 4.

[0036] Fig. 9 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 5.

[0037] Fig.10 These are the results of the laser diffraction particle size distribution measurement of the polyimide resin powder obtained in Comparative Example 6.

[0038] Fig.11 The following are the measurement results of the dielectric constant P and the dielectric loss tangent Q of the resin film obtained in Example 1 at each temperature when the measurement frequency was 10 GHz.

[0039] Fig.12 The following are the measurement results of the dielectric constant P and the dielectric loss tangent Q of the resin film obtained in Example 1 at each temperature when the measurement frequency was 20 GHz. DETAILED DESCRIPTION

[0040] <Method for producing polyimide resin powder>

[0041] The method for producing a polyimide resin powder of the present invention comprises a step of reacting a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride and a diamine component (B) containing an aliphatic diamine in the presence of a solvent (C) containing an alkylene glycol-based solvent represented by formula (1), wherein the step comprises the steps of: preparing a solution (a) containing the tetracarboxylic acid component (A) in the solvent (C) and a solution (b) containing the diamine component (B) in the solvent (C), respectively, and then adding the solution (b) to the solution (a). Alternatively, solution (a) is added to solution (b) to prepare a solution (c) containing a polyimide resin precursor containing polyamic acid, and then the polyimide resin precursor containing polyamic acid is imidized by heating the above-mentioned solution (c) to precipitate polyimide resin powder in the solution, wherein the solid content concentration of the above-mentioned solution (c) is 15 to 25% by weight, and the average heating rate of the above-mentioned solution (c) during the above-mentioned heating in the temperature range of 70 to 130°C is 0.5 to 8°C / min.

[0042] The "polyimide resin precursor" herein refers to a product produced by reaction of a tetracarboxylic acid component (A), a diamine component (B) and a solvent (C) containing an alkylene glycol-based solvent, and includes, in addition to polyamic acid, amic acid salts, polyamic acid salts, polyamic acid esters, and polyamic acid amides.

[0043]

[0044] (Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a straight-chain alkylene group having 2 to 6 carbon atoms, and n is an integer of 1 to 3.)

[0045] Here, the "solid content concentration of the solution (c) containing the polyimide resin precursor containing polyamic acid" refers to the ratio of the solute in the solution (c) (mass % converted according to the amount of feed). It should be noted that the "solute" refers to the tetracarboxylic acid component (A) and the diamine component (B), the end-capping agent, etc., which are raw materials of the polyamic acid, and the "solution (c)" refers to the total of the solute and the solvent, and the solvent contains the solvent (C) containing an alkylene glycol solvent.

[0046] In the method for producing a polyimide resin powder of the present invention, a solution (a) containing a tetracarboxylic acid component (A) in the above-mentioned solvent (C) and a solution (b) containing a diamine component (B) in the above-mentioned solvent (C) are prepared separately, and then the solution (b) is added to the solution (a) or the solution (a) is added to the solution (b) to prepare a solution (c) containing a polyimide resin precursor containing polyamic acid (step 1); then, the polyimide resin precursor containing polyamic acid is imidized in the solution (c) by heating the solution (c), and a polyimide resin powder is precipitated in the solution to synthesize a polyimide resin powder (step 2).

[0047] In the method for producing a polyimide resin powder of the present invention, the solid content concentration of the solution (c) containing polyamic acid is set to 15 to 25% by mass in the above step 1, and when the solution (c) is heated in the above step 2, the average heating rate of the solution (c) in the temperature range of 70 to 130° C. is set to 0.5 to 8° C. / min. The mechanism by which a polyimide resin powder having a volume average particle size D50 controlled to a specific range (specifically 5 to 50 μm) and having a good particle size distribution is obtained is not clear, but it can be considered as follows.

[0048] When the temperature of the solution (c) containing the polyimide resin precursor containing polyamic acid is within the range of 70 to 130° C., imidization of the polyimide resin precursor containing polyamic acid proceeds, and polyimide resin powder (hereinafter also referred to as “precipitate”) is precipitated in the solution.

[0049] The solvent of solution (c), i.e., the aforementioned solvent (C), has high compatibility with polyamic acid, but low compatibility with the precipitate precipitated as the imidization rate increases. On the other hand, if the temperature in the system is high, the solubility of the precipitate increases, and if the temperature in the system is low, the solubility of the precipitate decreases.

[0050] Therefore, it is believed that the precipitate is generated rapidly when the balance between the increase in solubility caused by the increase in temperature in the system and the decrease in compatibility caused by the increase in the imidization rate is unbalanced. It is also believed that the time of the unbalance can be controlled by the solid content concentration of the solution (c) and the average temperature increase rate in the temperature range of 70 to 130°C where imidization occurs.

[0051] For example, it can be considered that: when the heating rate when heating the aforementioned solution (c) is slow, the temperature in the system will slowly rise during the imidization process, and therefore, a plurality of crystals (seed crystals) that serve as seeds of precipitates are produced in the early stage of the increase in the imidization rate. As a result, there is a tendency that the particle size of each powder serving as a precipitate will not grow significantly.

[0052] On the other hand, it can be considered that when the heating rate when heating the aforementioned solution (c) is fast, the temperature in the system will rise rapidly during the process of imidization, thereby avoiding the generation of seed crystals in the early stage of the increase in the imidization rate, and precipitation will begin at the stage where the imidization proceeds to a certain extent. As a result, there is a tendency for the particle size of each powder as a precipitate to grow significantly.

[0053] In the method for producing a polyimide resin powder of the present invention, the solid content concentration of the solution (c) containing a polyimide resin precursor containing a polyamic acid prepared in the above step 1 is 15 to 25% by mass, preferably 15 to 23% by mass, and more preferably 17 to 23% by mass.

[0054] When the solid content concentration is less than the above range (less than 15% by mass), the volume average particle size D50 of the polyimide resin powder may exceed 50 μm, and the particle size distribution of the polyimide resin powder may present a multimodal distribution with three or more peaks.

[0055] On the other hand, when the solid content concentration exceeds the above range (exceeds 25 mass %), the particle size distribution of the polyimide resin powder may be bimodal and very broad, or even unimodal and very broad.

[0056] In the method for producing a polyimide resin powder of the present invention, when the solution (c) is heated in the aforementioned step 2, the average heating rate of the solution (c) in the temperature range of 70 to 130°C is set to 0.5 to 8°C / min, preferably 0.8 to 6°C / min, and more preferably 0.8 to 4°C / min.

[0057] When the average temperature increase rate is lower than the above range (lower than 0.5° C. / min), the particle size distribution of the polyimide resin powder may be bimodal and very broad, or even unimodal and very broad.

[0058] On the other hand, when the average temperature increase rate exceeds the above range (exceeds 8° C. / min), the volume average particle size D50 of the polyimide resin powder may exceed 50 μm.

[0059] In the present invention, the step of heating the solution (c) is performed at the specific average temperature increase rate as described above within the range of 70 to 130°C.

[0060] On the other hand, when the temperature of the solution (c) exceeds 130°C, the average temperature increase rate may be the same as when the temperature of the solution (c) is in the range of 70 to 130°C, and the rate will not be excessively reduced from the viewpoint of increasing the production rate, but it is preferably not excessively increased from the viewpoint of suppressing the sudden boiling of water produced as a by-product in the reaction. Specifically, it is 0.9 to 5°C / min, and more preferably 1.0 to 4°C / min.

[0061] In addition, within the range where the temperature of the solution (c) exceeds 130°C, from the viewpoint of sufficient molecular growth or sufficient imidization, the solution is preferably heated to 160°C, more preferably heated to 180°C, and further preferably heated to 190°C, and the temperature is preferably maintained for 10 to 120 minutes, and more preferably for 30 to 60 minutes.

[0062] The solvent (C) includes an alkylene glycol solvent represented by the formula (1). When a polyimide resin is produced using an aliphatic diamine as a raw material diamine component, a powdery polyimide resin can be obtained by reacting a tetracarboxylic acid component (A) and a diamine component (B) in the presence of such a specific solvent.

[0063] It is considered that it is ideal to obtain a uniform powdered polyimide resin: in a one-step reaction, (i) the polyamic acid is uniformly dissolved or the nylon salt is uniformly dispersed; (ii) the solvent has the two characteristics of not dissolving or swelling the polyimide resin at all. The above-mentioned solvent (C) generally satisfies these two characteristics. If the above-mentioned (i) is not satisfied, aggregation and agglomeration will occur before imidization, and if the above-mentioned (ii) is not satisfied, aggregation and agglomeration will occur after imidization.

[0064] From the viewpoint of enabling the polymerization reaction to proceed under high temperature conditions at normal pressure, the alkylene glycol solvent preferably has a boiling point of 140° C. or higher, more preferably 160° C. or higher, and even more preferably 180° C. or higher.

[0065] Ra1 in formula (1) is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group.

[0066] Ra2 in the formula (1) is a linear alkylene group having 2 to 6 carbon atoms, preferably a linear alkylene group having 2 to 3 carbon atoms, and more preferably an ethylene group.

[0067] In the formula (1), n ​​is an integer of 1 to 3, and preferably 2 or 3.

[0068] Specific examples of the alkylene glycol solvent include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether (another name: 2-(2-methoxyethoxy)ethanol), triethylene glycol monomethyl ether (another name: 2-[2-(2-methoxyethoxy)ethoxy]ethanol), ethylene glycol monoethyl ether, diethylene glycol monoethyl ether (another name: 2-(2-ethoxyethoxy)ethanol), ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol, 1,3-propylene glycol, etc. These solvents may be used alone or in combination of two or more selected from them. Among these solvents, at least one selected from the group consisting of 2-(2-methoxyethoxy)ethanol, 2-[2-(2-methoxyethoxy)ethoxy]ethanol, 2-(2-ethoxyethoxy)ethanol and 1,3-propylene glycol is preferred, and at least one selected from the group consisting of 2-(2-methoxyethoxy)ethanol and 2-(2-ethoxyethoxy)ethanol is more preferred.

[0069] The content of the alkylene glycol solvent in the solvent (C) is preferably 30% by mass or more, more preferably 50% by mass or more, further preferably 75% by mass or more, and further preferably 95% by mass or more. The solvent (C) may consist only of the alkylene glycol solvent.

[0070] When the solvent (C) contains the aforementioned alkylene glycol solvent and other solvents, specific examples of the “other solvents” include water, toluene, xylene, acetone, hexane, heptane, chlorobenzene, methanol, ethanol, n-propanol, isopropanol, N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, hexamethylphosphine, Amide, tetramethylene sulfone, dimethyl sulfoxide, o-cresol, m-cresol, p-cresol, phenol, p-chlorophenol, 2-chloro-4-hydroxytoluene, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dioxane, γ-butyrolactone, dioxolane, cyclohexanone, cyclopentanone, methylene chloride, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, dibromomethane, tribromoform, 1,2-dibromoethane, 1,1,2-tribromoethane, 2-ethylhexanol, etc. These solvents can be used alone or in combination with two or more solvents selected from them. Among these solvents, 2-ethylhexanol is preferred. That is, solvent (C) preferably also includes 2-ethylhexanol in addition to the aforementioned alkylene glycol solvent.

[0071] The solvent (C) preferably does not contain water, but may contain water as long as it is in the range of forming a long-chain polyamic acid as described above. Specifically, the water content is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 1% by mass or less, and particularly preferably 0% by mass.

[0072] The diamine component (B) contains an aliphatic diamine. In the present invention, when the polyimide resin is produced using the aliphatic diamine as the raw material diamine component, a powdered polyimide resin can be produced. By using the aliphatic diamine as the raw material diamine component, thermoforming processability is imparted to the polyimide resin powder.

[0073] Examples of the aforementioned aliphatic diamine include diamines containing at least one alicyclic hydrocarbon structure and chain aliphatic diamines. In the diamine component (B), as the aforementioned aliphatic diamine, it is preferred to contain a diamine containing at least one alicyclic hydrocarbon structure and a chain aliphatic diamine, and it is more preferred to contain a diamine (B1) represented by the formula (B1-1) described later and a diamine (B2) represented by the formula (B2-1).

[0074] H2N-R1-NH2 (B1-1)

[0075] H2N-R2-NH2 (B2-1)

[0076] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure, and R2 is a divalent chain aliphatic group having 5 to 20 carbon atoms.)

[0077] Hereinafter, the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine will be described.

[0078] The diamine containing at least one alicyclic hydrocarbon structure is preferably a diamine (B1) represented by the following formula (B1-1).

[0079] H2N-R1-NH2 (B1-1)

[0080] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure.)

[0081] Here, the alicyclic hydrocarbon structure refers to a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated, and may be a monocyclic or polycyclic ring.

[0082] Examples of the alicyclic hydrocarbon structure include, but are not limited to, cycloalkane rings such as cyclohexane rings, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane rings, and bicycloalkene rings such as norbornene. Among these, cycloalkane rings are preferred, cycloalkane rings having 4 to 7 carbon atoms are more preferred, and cyclohexane rings are still more preferred.

[0083] The number of carbon atoms in R1 is 6 to 22, preferably 8 to 17.

[0084] R1 contains at least one alicyclic hydrocarbon structure, and preferably contains 1 to 3 alicyclic hydrocarbon structures.

[0085] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2), and more preferably a divalent group represented by the following formula (R1-3).

[0086]

[0087] (m 11 and m 12 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 13 ~m 15 Each independently represents an integer from 0 to 2, preferably 0 or 1.)

[0088]

[0089] It should be noted that in the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be cis or trans, and the ratio of cis to trans may be any value.

[0090] The diamine (B1) is more preferably represented by the following formula (B1-2).

[0091]

[0092] (m 11 and m 12 Each independently represents an integer from 0 to 2, preferably 0 or 1.)

[0093] Specific examples of the diamine (B1) include 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carvonediamine, limonenediamine, isophoronediamine, norbornanediamine, bis(aminomethyl)tricyclo[5.2.1.0 2,6] decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. These compounds can be used alone or in combination with two or more compounds selected from them. Among these, 1,3-bis(aminomethyl)cyclohexane can be suitably used. It should be noted that diamines containing alicyclic hydrocarbon structures usually have structural isomers, but the ratio of cis-isomers / trans-isomers is not limited. In addition, it is known that diamines with low symmetry usually have a tendency to increase the free volume of the resin. Therefore, it can be considered that 1,3-bis(aminomethyl)cyclohexane with a fluffy structure and low symmetry is easy to contribute to low dielectric constant and is therefore more suitable.

[0094] The linear aliphatic diamine is preferably a diamine (B2) represented by the following formula (B2-1).

[0095] H2N-R2-NH2 (B2-1)

[0096] (R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms.)

[0097] Here, the chain aliphatic group refers to a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, may be linear or branched, and may contain heteroatoms such as oxygen atoms.

[0098] R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, further preferably an alkylene group having 7 to 12 carbon atoms, and particularly preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear or branched chain group, and is preferably a linear chain group.

[0099] R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and is particularly preferably an octamethylene group.

[0100] In addition, other suitable forms of R2 include divalent chain aliphatic groups having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms) containing an ether group. Among them, divalent groups represented by the following formula (R2-1) or (R2-2) are preferred.

[0101]

[0102] (m 21 and m 22 Each independently represents an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and further preferably 1 to 9. 23 ~m 25 Each independently represents an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8.)

[0103] It should be noted that R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). Therefore, m in formula (R2-1) 21 and m 22 The divalent group represented by formula (R2-1) is selected so that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 21 +m 22 It is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10).

[0104] Similarly, m in formula (R2-2) 23 ~m 25 The divalent group represented by formula (R2-2) is selected so that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 23 +m 24 +m 25 The carbon number is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms).

[0105] Specific examples of diamine (B2) include 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 3-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, 2,2'-(ethylenedioxy)bis(ethyleneamine), etc. These compounds may be used alone or in combination of two or more selected from them. Among these, chain aliphatic diamines having 8 to 10 carbon atoms may be suitably used, and at least one selected from the group consisting of 1,8-octamethylenediamine and 1,10-decamethylenediamine may be particularly suitably used.

[0106] The diamine component (B) preferably contains the above-mentioned diamine (B1) and the above-mentioned diamine (B2) as the above-mentioned aliphatic diamine, and more preferably contains 1,3-bis(aminomethyl)cyclohexane and 1,8-octamethylenediamine.

[0107] From the viewpoint of obtaining a polyimide resin powder suitable for producing a high-frequency circuit substrate described later, the amount of diamine (B1) is preferably 20 to 70 mol%, more preferably 20 to 65 mol%, further preferably 20 to 60 mol%, further preferably 20 to 50 mol%, further preferably 20 mol% or more and less than 40 mol%, relative to the total amount of diamine (B1) and diamine (B2).

[0108] The diamine component (B) may consist of only an aliphatic diamine, or may contain a diamine including an aromatic ring in addition to the aliphatic diamine.

[0109] The diamine containing an aromatic ring is preferably a diamine containing at least one aromatic ring, and more preferably a diamine (B3) represented by the following formula (B3-1).

[0110] H2N-R3-NH2 (B3-1)

[0111] (R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)

[0112] The aromatic ring may be a single ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.

[0113] The number of carbon atoms in R3 is 6-22, preferably 6-18.

[0114] R3 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.

[0115] In addition, the aromatic ring may be bonded with a monovalent or divalent electron-withdrawing group. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, a halogen group, a haloalkyl group, a phenyl group, and an acyl group. Examples of the divalent electron-withdrawing group include fluoroalkylene (e.g., -C(CF3)2-, -(CF2) p- (here, p is an integer of 1 to 10))) In addition to the halogenated alkylene group, -CO-, -SO2-, -SO-, -CONH-, -COO-, etc. can be mentioned.

[0116] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2).

[0117]

[0118] (m 31 and m 32 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 33 and m 34 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 21, R 22 and R 23 Each is independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 、p 22 and p 23 is an integer of 0 to 4, preferably 0. 21 It is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.)

[0119] It should be noted that R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, m in formula (R3-1) 31 、m 32 , R 21 and p 21 The divalent group represented by the formula (R3-1) is selected so that the number of carbon atoms falls within the range of 6 to 22.

[0120] Similarly, L in formula (R3-2) 21 、m 33 、m 34 , R 22 , R 23 、p 22 and p 23 The divalent group represented by the formula (R3-2) is selected so that the number of carbon atoms falls within the range of 12 to 22.

[0121] Specific examples of the diamine (B3) include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 1,2-diethynylphenylenediamine, 1,3-diethynylphenylenediamine, 1,4-diethynylphenylenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2'-bis(4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, and 1,5-diaminonaphthalene.

[0122] When the diamine component (B) contains both an aliphatic diamine and a diamine containing an aromatic ring, the diamine (B3) is further contained in addition to the diamine (B1) and the diamine (B2), and the amount of the diamine (B3) is preferably 25 mol% or less relative to the total amount of the diamine (B1) and the diamine (B2). On the other hand, the lower limit is not particularly limited as long as it exceeds 0 mol%.

[0123] The diamine component (B) may contain a diamine (B4) represented by the following formula (B4-1).

[0124] H2N-R4-NH2 (B4-1)

[0125] (R4 is -SO2- or -Si(R x )(R y )O-divalent group, R x and R y Each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group.

[0126] Among them, from the viewpoint of hot forming processability of the obtained polyimide resin powder, the content of the aliphatic diamine in the diamine component (B), preferably the total content of the diamine (B1) and the diamine (B2), more preferably the total content of 1,3-bis(aminomethyl)cyclohexane and 1,8-octamethylenediamine, is preferably 50 mol% or more, more preferably 70 mol% or more, further preferably 80 mol% or more, and further preferably 90 mol% or more, and is 100 mol% or less, relative to the total molar number of the diamines in the diamine component (B).

[0127] The tetracarboxylic acid component (A) contains tetracarboxylic dianhydride. The tetracarboxylic dianhydride is preferably a tetracarboxylic dianhydride containing at least one aromatic ring, and more preferably a tetracarboxylic dianhydride represented by formula (A-1).

[0128]

[0129] (X is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)

[0130] X is a tetravalent group having 6 to 22 carbon atoms and including at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.

[0131] X has 6 to 22 carbon atoms, preferably 6 to 18 carbon atoms.

[0132] X contains at least one aromatic ring, and preferably contains 1 to 3 aromatic rings.

[0133] X is preferably a tetravalent group represented by any one of the following formulae (X-1) to (X-4).

[0134]

[0135] (R 11 ~R 18 Each is independently an alkyl group having 1 to 4 carbon atoms. 11 ~p 13 Each independently represents an integer of 0 to 2, and is preferably 0. 14 、p15 、p 16 and p 18 Each independently represents an integer of 0 to 3, and is preferably 0. 17 is an integer of 0 to 4, preferably 0. 11 ~L 13 Each is independently a single bond, an ether group, a carbonyl group or an alkylene group having 1 to 4 carbon atoms.)

[0136] It should be noted that X is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, R in formula (X-2) 12 , R 13 、p 12 and p 13 The tetravalent group represented by the formula (X-2) is selected so that the number of carbon atoms falls within the range of 10 to 22.

[0137] Similarly, L in formula (X-3) 11 , R 14 , R 15 、p 14 and p 15 The tetravalent group represented by formula (X-3) is selected so that the number of carbon atoms falls within the range of 12 to 22. 12 , L 13 , R 16 , R 17 , R 18 、p 16 、p 17 and p 18 The tetravalent group represented by the formula (X-4) is selected so that the number of carbon atoms falls within the range of 18 to 22.

[0138] X is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).

[0139]

[0140] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride, 2,3,5,6-toluene tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, etc. These tetracarboxylic dianhydrides may be used alone or in combination of two or more. Among these, pyromellitic dianhydride is particularly preferred.

[0141] The tetracarboxylic acid component (A) may contain a derivative of tetracarboxylic dianhydride (tetracarboxylic acid and / or an alkyl ester of tetracarboxylic acid) in addition to tetracarboxylic dianhydride.

[0142] Examples of the tetracarboxylic acid include pyromellitic acid, 2,3,5,6-toluenetetracarboxylic acid, 3,3′,4,4′-benzophenonetetracarboxylic acid, 3,3′,4,4′-biphenyltetracarboxylic acid, and 1,4,5,8-naphthalenetetracarboxylic acid. Among these, pyromellitic acid is particularly preferred.

[0143] Examples of the alkyl esters of tetracarboxylic acids include dimethyl pyromellitic acid, diethyl pyromellitic acid, dipropyl pyromellitic acid, diisopropyl pyromellitic acid, dimethyl 2,3,5,6-toluenetetracarboxylate, dimethyl 3,3',4,4'-diphenylsulfonetetracarboxylate, dimethyl 3,3',4,4'-benzophenonetetracarboxylate, dimethyl 3,3',4,4'-biphenyltetracarboxylate, and dimethyl 1,4,5,8-naphthalenetetracarboxylate. In the alkyl esters of the tetracarboxylic acids, the number of carbon atoms of the alkyl group is preferably 1 to 3.

[0144] These tetracarboxylic acids and derivatives thereof may be used alone or in combination of two or more.

[0145] The ratio of the tetracarboxylic acid in the tetracarboxylic acid component (A) is preferably as small as possible, preferably 50 mol% or less, more preferably 30 mol% or less, particularly preferably 0 mol%.

[0146] When producing the polyimide resin powder, the charging amount ratio of the tetracarboxylic acid component (A) to the diamine component (B) is preferably 0.9 to 1.1 mol of the diamine component (B) per 1 mol of the tetracarboxylic acid component (A).

[0147] In the method for producing a polyimide resin powder of the present invention, in addition to mixing the aforementioned tetracarboxylic acid component (A) and the aforementioned diamine component (B), an end-capping agent may also be mixed. As the end-capping agent, at least one selected from the group consisting of monoamines and dicarboxylic acids is preferred. The amount of the end-capping agent used is an amount that can introduce a desired amount of terminal groups into the polyimide resin, preferably 0.0001 to 0.1 mole, more preferably 0.001 to 0.06 mole, and further preferably 0.002 to 0.035 mole relative to 1 mole of the tetracarboxylic acid component (A).

[0148] Examples of the monoamine blocking agent include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, n-decylamine, n-undecylamine, laurylamine, n-tridecylamine, n-tetradecylamine, isopentylamine, neopentylamine, 2-methylpentylamine, 2-methylhexylamine, 2-ethylpentylamine, 3-ethylpentylamine, isooctylamine, 2-ethylhexylamine, 3-ethylhexylamine, isononylamine, 2-ethyloctylamine, isodecylamine, isododecylamine, isotridecylamine and isotetradecylamine; and aromatic monoamines such as benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline and 4-methylaniline.

[0149] As other monoamine end-capping agents, if monoamines having halogen elements such as fluorine are used, there is a tendency to obtain low dielectric properties, so they are suitable. Specific examples include 2-trifluoromethylaniline, 3-trifluoromethylaniline, 4-trifluoromethylaniline, 2,3-bis(trifluoromethyl)aniline, 2,4-bis(trifluoromethyl)aniline, 2,5-bis(trifluoromethyl)aniline, 2,6-bis(trifluoromethyl)aniline, 3,4-bis(trifluoromethyl)aniline, 3,5-bis(trifluoromethyl)aniline, 2,3,4-tris(trifluoromethyl)aniline, 2, 3,5-Tris(trifluoromethyl)aniline, 2,3,6-Tris(trifluoromethyl)aniline, 2,4,5-Tris(trifluoromethyl)aniline, 2,4,6-Tris(trifluoromethyl)aniline, 3,4,5-Tris(trifluoromethyl)aniline, 2,3,4,5-tetrakis(trifluoromethyl)aniline, 2,4,5,6-tetrakis(trifluoromethyl)aniline, 2,4-bis(3,5-bis(trifluoromethyl)phenoxy)aniline, and the like.

[0150] In addition, when using monoamines having a bulky structure (specifically, alicyclic monoamines) as other monoamine end-capping agents, there is a tendency to obtain low dielectric properties, so they are suitable. Specific examples include amines having adamantyl groups such as cyclohexylamine, dicyclohexylamine, methylcyclohexylamine, and adamantaneamine; and amines having a fluorene skeleton.

[0151] As the dicarboxylic acid end-capping agent, dicarboxylic acids are preferred, and a part of them may be ring-closed. Examples thereof include phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenone dicarboxylic acid, 3,4-benzophenone dicarboxylic acid, cyclohexane-1,2-dicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, and 4-cyclohexene-1,2-dicarboxylic acid. Among these, phthalic acid and phthalic anhydride are preferred.

[0152] As other dicarboxylic acid-based end-capping agents, similarly to the other monoamine-based end-capping agents described above, dicarboxylic acids having a halogen element such as fluorine or dicarboxylic acids having a bulky structure are preferably used because they can contribute to lowering the dielectric constant.

[0153] These blocking agents may be used alone or in combination of two or more.

[0154] The blocking agent is particularly preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, isononylamine, n-decylamine and isodecylamine, more preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine and isononylamine, and even more preferably at least one selected from the group consisting of n-octylamine, isooctylamine and 2-ethylhexylamine.

[0155] The solution (c) containing a polyimide resin precursor containing polyamic acid includes a solution (a) and a solution (b), wherein the solution (a) contains a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride in the aforementioned solvent (C), and the solution (b) contains a diamine component (B) containing an aliphatic diamine in the aforementioned solvent (C). It should be noted that, when a capping agent is used, the solution (c) containing a polyimide resin precursor containing polyamic acid includes a solution (d) containing the capping agent in the aforementioned solvent (C).

[0156] In the method for producing a polyimide resin powder of the present invention, from the viewpoint of controlling the solid content concentration of the solution (c) containing the polyimide resin precursor containing polyamic acid prepared in the above step 1 to 15 to 25% by mass, the content of the tetracarboxylic acid component (A) in the above solution (a) is preferably 20 to 45% by mass, more preferably 25 to 45% by mass, and the content of the diamine component (B) in the above solution (b) is preferably 20 to 80% by mass, more preferably 40 to 60% by mass.

[0157] When a terminal blocking agent is used, the content of the terminal blocking agent in the solution (d) is preferably 1 to 100% by mass, more preferably 10 to 80% by mass.

[0158] In solution (a), the ratio of tetracarboxylic dianhydride in tetracarboxylic acid component (A) is preferably 50 mol% or more, more preferably 70 mol% or more, and further preferably 90 mol% or more. It is particularly preferred that the tetracarboxylic acid component (A) is substantially composed of tetracarboxylic dianhydride. The "substantially" mentioned here means that when only tetracarboxylic dianhydride is used as tetracarboxylic acid component (A), a part thereof (to about 10 mol%) can be accepted to react with moisture in the atmosphere and open the ring.

[0159] In the step 1, it is preferred to complete the addition of the solution (b) to the solution (a) when the total amount of the diamine component (B) added reaches 0.9 to 1.1 mol per 1 mol of the tetracarboxylic acid component (A).

[0160] When a blocking agent is used, solution (b) may be added to solution (a), and then solution (d) may be added. The type and content of the blocking agent, and preferred embodiments thereof are as described above.

[0161] The step of reacting the tetracarboxylic acid component (A) and the diamine component (B) in the presence of the solvent (C) may be performed under normal pressure or under pressure. However, it is preferably performed under normal pressure because a pressure-resistant container is not required.

[0162] By making the step of reacting the tetracarboxylic acid component (A) and the diamine component (B) in the presence of the solvent (C) include the step 1 and the step 2, a polyimide resin powder having a volume average particle size D50 in a specific range (specifically, 5 to 50 μm) and a good particle size distribution can be obtained.

[0163] <Polyimide resin powder>

[0164] The polyimide resin powder obtained by the production method of the present invention comprises a repeating structural unit represented by the following formula (I) and a repeating structural unit represented by the following formula (II), wherein the content ratio of the repeating structural unit of the formula (I) relative to the total of the repeating structural unit of the formula (I) and the repeating structural unit of the formula (II) is 20 to 70 mol%.

[0165]

[0166] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)

[0167] The polyimide resin powder of the present invention has a volume average particle size D50 of preferably 5 to 50 μm, more preferably 10 to 40 μm, and further preferably 13 to 35 μm, a volume average particle size D10 of preferably 1 to 40 μm, more preferably 2 to 30 μm, and further preferably 5 to 25 μm, and a volume average particle size D90 of preferably 5 to 60 μm, more preferably 10 to 50 μm, and further preferably 15 to 45 μm in a particle size measurement based on a laser diffraction light scattering particle size distribution measuring device.

[0168] The particle size within this range provides the following advantages: clogging of the filter cloth is less likely to occur during the production of the polyimide resin powder, the filterability for removing the solvent is good, and the residual solution (high boiling point solvent, water) retained in the particles can be reduced.

[0169] It should be noted that the volume average particle diameters D50, D10 and D90 can be specifically determined by the methods described in the Examples.

[0170] The value of D10 of the polyimide resin powder relative to the value of D50 (D10 / D50) is preferably 1 / 3 (0.33) or more, and more preferably 1 / 2 (0.5) or more.

[0171] The value of D90 of the polyimide resin powder relative to the value of D50 (D90 / D50) is preferably 3 or less, more preferably 2 or less.

[0172] More preferably, D10 / D50 is 0.45 to 0.9 and D90 / D50 is more than 1.4 and is 2.0 or less. Still more preferably, D10 / D50 is 0.7 to 0.9 and D90 / D50 is 1.1 to 1.4.

[0173] By setting the particle size distribution within this range, a single peak is obtained and a sharp shape is obtained, or even if a two-peak property is obtained, the main peak can obtain a sharp shape, and the volume frequency of the main peak becomes larger, so that the following advantages can be obtained: excellent handling properties, for example, a stable feeding state is presented during extrusion molding and productivity is improved. Similarly, classification can be suppressed during feeding, and the scattering of fine powder can be suppressed, and the fluidity of the powder itself is improved. When manufacturing resin powder, the conditions for filtering and transportation are stable. When used as an additive, the dispersibility is excellent and the physical properties are easily exhibited.

[0174] The polyimide resin powder is a thermoplastic resin. Thermoplastic polyimide resin is different from polyimide resin having no glass transition temperature (Tg) formed by closing the imide ring after molding in the state of a polyimide precursor such as polyamic acid, or polyimide resin that decomposes at a temperature lower than the glass transition temperature.

[0175] The repeating structural unit of formula (I) is described in detail below.

[0176] R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. Here, the alicyclic hydrocarbon structure refers to a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated and may be monocyclic or polycyclic.

[0177] Examples of the alicyclic hydrocarbon structure include, but are not limited to, cycloalkane rings such as cyclohexane rings, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane rings, and bicycloalkene rings such as norbornene. Among these, cycloalkane rings are preferred, cycloalkane rings having 4 to 7 carbon atoms are more preferred, and cyclohexane rings are still more preferred.

[0178] The number of carbon atoms in R1 is 6 to 22, preferably 8 to 17.

[0179] R1 contains at least one alicyclic hydrocarbon structure, and preferably contains 1 to 3 alicyclic hydrocarbon structures.

[0180] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2).

[0181]

[0182] (m 11 and m 12 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 13 ~m 15 Each independently represents an integer from 0 to 2, preferably 0 or 1.)

[0183] R1 is particularly preferably a divalent group represented by the following formula (R1-3).

[0184]

[0185] It should be noted that in the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be cis or trans, and the ratio of cis to trans may be any value.

[0186] X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.

[0187] X1 has 6 to 22 carbon atoms, preferably 6 to 18 carbon atoms.

[0188] X1 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.

[0189] X1 is preferably a tetravalent group represented by any one of the following formulae (X-1) to (X-4).

[0190]

[0191] (R 11 ~R 18 Each is independently an alkyl group having 1 to 4 carbon atoms. 11~p 13 Each independently represents an integer of 0 to 2, and is preferably 0. 14 、p 15 、p 16 and p 18 Each independently represents an integer of 0 to 3, and is preferably 0. 17 is an integer of 0 to 4, preferably 0. 11 ~L 13 Each is independently a single bond, an ether group, a carbonyl group or an alkylene group having 1 to 4 carbon atoms.)

[0192] It should be noted that X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, R in formula (X-2) 12 , R 13 、p 12 and p 13 The tetravalent group represented by the formula (X-2) is selected so that the number of carbon atoms falls within the range of 10 to 22.

[0193] Similarly, L in formula (X-3) 11 , R 14 , R 15 、p 14 and p 15 The tetravalent group represented by formula (X-3) is selected so that the number of carbon atoms falls within the range of 12 to 22. 12 , L 13 , R 16 , R 17 , R 18 、p 16 、p 17 and p 18 The tetravalent group represented by the formula (X-4) is selected so that the number of carbon atoms falls within the range of 18 to 22.

[0194] X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).

[0195]

[0196] Next, the repeating structural unit of formula (II) is described in detail below.

[0197] R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms.

[0198] R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, further preferably an alkylene group having 7 to 12 carbon atoms, and particularly preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear alkylene group or a branched alkylene group, and is preferably a linear alkylene group.

[0199] R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and is particularly preferably an octamethylene group.

[0200] In addition, other suitable embodiments of R2 include divalent chain aliphatic groups having 5 to 16 carbon atoms including an ether group. The carbon number is preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms. Among them, divalent groups represented by the following formula (R2-1) or (R2-2) are preferred.

[0201]

[0202] (m 21 and m 22 Each independently represents an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and further preferably 1 to 9. 23 ~m 25 Each independently represents an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8.)

[0203] It should be noted that R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). Therefore, m in formula (R2-1) 21 and m 22 The divalent group represented by formula (R2-1) is selected so that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). 21 +m 22 It is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10).

[0204] Similarly, m in formula (R2-2) 23 ~m 25 The divalent group represented by formula (R2-2) is selected so that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). 23 +m 24 +m 25The carbon number is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and still more preferably 8 to 10 carbon atoms).

[0205] X2 is defined similarly to X1 in formula (I), and preferred embodiments are also the same.

[0206] The repeating structural unit of formula (I) contains 20 to 70 mol% relative to the total of the repeating structural unit of formula (I) and the repeating structural unit of formula (II). When the repeating structural unit of formula (I) contains the above-mentioned range, in a general injection molding cycle, the polyimide resin powder can also be fully crystallized. If the content ratio is less than 20 mol%, the molding processability is reduced, and if it exceeds 70 mol%, the crystallinity is reduced, and therefore, the heat resistance is reduced.

[0207] From the viewpoint of exhibiting high crystallinity, the content ratio of the repeating structural unit of formula (I) relative to the total of the repeating structural unit of formula (I) and the repeating structural unit of formula (II) is preferably 65 mol% or less, more preferably 60 mol% or less, and further preferably 50 mol% or less.

[0208] Wherein, the repeating structural unit of formula (II) is preferably 20 mol% or more and less than 40 mol% relative to the total of the repeating structural unit of formula (I) and the repeating structural unit of formula (II). If it is within this range, the crystallinity of the polyimide resin powder can be obtained to be higher, heat resistance is more excellent, it is suitable for manufacturing the high-frequency circuit substrate described later, and the effect of suppressing the rise of the dielectric loss tangent at high temperature is also excellent. It should be noted that it is known that the molecular motion of the resin is easily activated at high temperature, the dielectric properties such as the dielectric loss tangent deteriorate, so it can be considered that: giving crystallinity to the resin and increasing the glass transition temperature of the resin are effective for suppressing the molecular motion of the resin.

[0209] From the viewpoint of formability, the content ratio is preferably 25 mol% or more, more preferably 30 mol% or more, and further preferably 32 mol% or more. From the viewpoint of exhibiting high crystallinity, the content ratio is further preferably 35 mol% or less.

[0210] The total content of the repeating structural unit of formula (I) and the repeating structural unit of formula (II) is preferably 50 to 100 mol %, more preferably 75 to 100 mol %, further preferably 80 to 100 mol %, and further preferably 85 to 100 mol % based on the total repeating structural units constituting the polyimide resin powder.

[0211] The polyimide resin powder may further contain a repeating structural unit of the following formula (III). In this case, the repeating structural unit of formula (III) preferably contains less than 25 mol% relative to the total of the repeating structural unit of formula (I) and the repeating structural unit of formula (II). On the other hand, the lower limit is not particularly limited as long as it exceeds 0 mol%.

[0212] From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, it is preferably 20 mol % or less, more preferably 15 mol % or less.

[0213]

[0214] (R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. X3 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)

[0215] R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include, but are not limited to, a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.

[0216] The number of carbon atoms in R3 is 6-22, preferably 6-18.

[0217] R3 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.

[0218] In addition, the aromatic ring may be bonded with a monovalent or divalent electron-withdrawing group. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, a halogen group, a haloalkyl group, a phenyl group, and an acyl group. Examples of the divalent electron-withdrawing group include fluorinated alkylene groups (e.g., -C(CF3)2-, -(CF2) p- (here, p is an integer of 1 to 10))) and other halogenated alkylene groups, include -CO-, -SO2-, -SO-, -CONH-, -COO- and the like.

[0219] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2).

[0220]

[0221] (m 31 and m 32 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 33 and m 34 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 21 , R22 and R 23 Each is independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 、p 22 and p 23 is an integer of 0 to 4, preferably 0. 21 It is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.)

[0222] It should be noted that R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, m in formula (R3-1) 31 、m 32 , R 21 and p 21 The divalent group represented by the formula (R3-1) is selected so that the number of carbon atoms falls within the range of 6 to 22.

[0223] Similarly, L in formula (R3-2) 21 、m 33 、m 34 , R 22 , R 23 、p 22 and p 23 The divalent group represented by the formula (R3-2) is selected so that the number of carbon atoms falls within the range of 12 to 22.

[0224] X3 is defined similarly to X1 in formula (I), and preferred embodiments are also the same.

[0225] The polyimide resin powder may further contain a repeating structural unit represented by the following formula (IV).

[0226]

[0227] (R4 is -SO2- or -Si(R x )(R y )O-divalent group, R x and R y Each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. X4 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.

[0228] X4 is defined similarly to X1 in formula (I), and preferred embodiments are also the same.

[0229] The terminal structure of the polyimide resin powder is not particularly limited, but it is preferred that the terminal has a chain aliphatic group having 5 to 14 carbon atoms.

[0230] The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. If the polyimide resin powder has the above-mentioned specific group at the end, a resin film having excellent heat aging resistance can be obtained.

[0231] Examples of the saturated chain aliphatic group having 5 to 14 carbon atoms include n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, lauryl, n-tridecyl, n-tetradecyl, isopentyl, neopentyl, 2-methylpentyl, 2-methylhexyl, 2-ethylpentyl, 3-ethylpentyl, isooctyl, 2-ethylhexyl, 3-ethylhexyl, isononyl, 2-ethyloctyl, isodecyl, isododecyl, isotridecyl, and isotetradecyl.

[0232] Examples of the unsaturated chain aliphatic group having 5 to 14 carbon atoms include 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl, dodecenyl, tridecenyl and tetradecenyl.

[0233] Among them, the above-mentioned chain aliphatic group is preferably a saturated chain aliphatic group, and more preferably a saturated straight-chain aliphatic group. In addition, from the viewpoint of obtaining heat aging resistance, the carbon number of the above-mentioned chain aliphatic group is preferably 6 or more, more preferably 7 or more, and further preferably 8 or more, and the carbon number is preferably 12 or less, more preferably 10 or less, and further preferably 9 or less. The above-mentioned chain aliphatic group may be only one kind or two or more kinds.

[0234] The above-mentioned chain aliphatic group is particularly preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl, isononyl, n-decyl and isodecyl, further preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl and isononyl, and most preferably at least one selected from the group consisting of n-octyl, isooctyl and 2-ethylhexyl.

[0235] In addition, from the viewpoint of heat aging resistance, the polyimide resin powder preferably has, in addition to the terminal amino group and the terminal carboxyl group, only a chain aliphatic group having 5 to 14 carbon atoms at the terminal. When a group other than the above is present at the terminal, the content thereof is preferably 10 mol% or less, more preferably 5 mol% or less, relative to the chain aliphatic group having 5 to 14 carbon atoms.

[0236] From the viewpoint of exhibiting excellent heat aging resistance, the content of the above-mentioned chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin powder is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and further preferably 0.2 mol% or more, relative to 100 mol% of the total of all repeating structural units constituting the polyimide resin powder. In addition, in order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the above-mentioned chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin powder is preferably 10 mol% or less, more preferably 6 mol% or less, and further preferably 3.5 mol% or less, relative to 100 mol% of the total of all repeating structural units constituting the polyimide resin powder.

[0237] The content of the chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin powder can be determined by depolymerizing the polyimide resin powder.

[0238] The polyimide resin powder preferably has a melting point of 360°C or less and a glass transition temperature of 150°C or more. From the viewpoint of heat resistance, the melting point of the polyimide resin powder is more preferably 280°C or more, and further preferably 290°C or more. From the viewpoint of high formability, it is preferably 345°C or less, more preferably 340°C or less, and further preferably 335°C or less. In addition, from the viewpoint of heat resistance, the glass transition temperature of the polyimide resin powder is more preferably 160°C or more, and further preferably 170°C or more. From the viewpoint of high formability, it is preferably 250°C or less, more preferably 230°C or less, and further preferably 200°C or less.

[0239] The melting point and glass transition temperature of the polyimide resin powder can be measured using a differential scanning calorimeter.

[0240] In addition, with respect to the polyimide resin powder, from the viewpoint of improving crystallinity, heat resistance, mechanical strength, and chemical resistance, the heat of the crystallization exothermic peak observed when the polyimide resin powder is melted and cooled at a temperature drop rate of 20°C / minute (hereinafter also referred to as "crystallization exothermic heat") is preferably 5.0 mJ / mg or more, more preferably 10.0 mJ / mg or more, and further preferably 17.0 mJ / mg or more. The upper limit of the crystallization exothermic heat is not particularly limited, and is usually 45.0 mJ / mg or less.

[0241] Specifically, the melting point, glass transition temperature, and crystallization heat of the polyimide resin powder can be measured by the methods described in Examples.

[0242] The logarithmic viscosity of a 0.5 mass % concentrated sulfuric acid solution of the polyimide resin powder at 30°C is preferably in the range of 0.2 to 2.0 dL / g, more preferably in the range of 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or more, sufficient mechanical strength can be obtained when the obtained polyimide resin powder is made into a molded body, and if it is 2.0 dL / g or less, the molding processability and handling properties become good. The logarithmic viscosity μ is obtained as follows: Using a Cannon-Fresco viscometer, the flow time of concentrated sulfuric acid and the above-mentioned polyimide resin solution is measured at 30°C, respectively, and obtained according to the following formula.

[0243] μ=ln(ts / t0) / C

[0244] t0: Flow time of concentrated sulfuric acid

[0245] ts: Flow time of polyimide resin solution

[0246] C: 0.5 (g / dL)

[0247] The weight average molecular weight Mw of the polyimide resin powder is preferably 10,000 to 150,000, more preferably 15,000 to 100,000, further preferably 20,000 to 80,000, further preferably 30,000 to 70,000, further preferably 35,000 to 65,000. In addition, when the weight average molecular weight Mw of the polyimide resin powder is 10,000 or more, the mechanical strength of the obtained molded body becomes good, when it is 40,000 or more, the stability of the mechanical strength becomes good, and when it is 150,000 or less, the molding processability becomes good.

[0248] The weight average molecular weight Mw of the polyimide resin powder can be measured by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.

[0249] <Resin film>

[0250] The present invention provides a film-like molded product (resin film) obtained using a molding material containing a polyimide resin powder having a specific composition obtained by the production method of the present invention.

[0251] The resin film of the present invention is obtained by using a molding material containing a polyimide resin powder of a specific composition obtained by the production method of the present invention. The mechanism of the effect of suppressing the increase in dielectric loss tangent at high temperature is not necessarily clear, but it is considered as follows.

[0252] The polyimide resin powder obtained by the production method of the present invention contains, as divalent groups derived from the diamine component (B), divalent groups having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure and divalent chain aliphatic groups having 5 to 16 carbon atoms at a specific ratio.

[0253] The alicyclic hydrocarbon structure has a fluffy structure, so it is believed that there is a tendency to increase the free volume of the resin (the difference between the volume actually occupied by the substance and the space occupied volume calculated based on the atomic radius, etc.). This is considered to be a reason for the effect of improving dielectric properties such as dielectric loss tangent. Among them, it can be considered that if it is a divalent group derived from an alicyclic diamine with low symmetry (such as 1,3-bis(aminomethyl)cyclohexane), the tendency to increase the free volume of the resin is higher, so it can be considered that the effect of improving dielectric properties such as dielectric loss tangent becomes higher.

[0254] In addition to the design concept at room temperature, there is also the following design concept: according to the polyimide resin powder having a specific composition range of the present invention, a high crystallization temperature can be exhibited by a crystallized part, and a high glass transition temperature can be exhibited by an amorphous part.

[0255] Therefore, it can be considered that the resin film obtained by using the molding material containing the polyimide resin powder of the present invention which has the design concept not only at room temperature but also at high temperature, the molecular motion of the resin is difficult to be activated even at high temperature, and the deterioration of dielectric properties such as dielectric loss tangent is suppressed.

[0256] It should be noted that it is known that crystalline resins generally tend to have a lower water absorption rate. Therefore, it is considered that the resin film according to the present invention also exhibits an effect of suppressing the deterioration of dielectric properties such as dielectric loss tangent caused by water absorption under high humidity.

[0257] Dielectric constant P of resin film at 10 GHz and 120°C 120 The dielectric constant P at 40°C 40 The ratio (P 120 / P 40 ) is preferably 0.8 to 1.2, more preferably 0.8 to 1.1.

[0258] In addition, the dielectric constant P of the resin film at 20 GHz and 120°C is 120 The dielectric constant P at 40°C 40 The ratio (P 120 / P 40 ) is preferably 0.8 to 1.2, more preferably 0.85 to 1.1.

[0259] Dielectric loss tangent Q of resin film at 10 GHz and 120°C 120 Dielectric loss tangent Q at 40°C 40 The ratio (Q 120 / Q 40 ) is preferably 1.0 to 1.5, more preferably 1.0 to 1.3.

[0260] In addition, the dielectric loss tangent Q of the resin film at 20 GHz and 120°C is 120 Dielectric loss tangent Q at 40°C 40 The ratio (Q 120 / Q 40 ) is preferably 1.0 to 1.7, more preferably 1.2 to 1.6.

[0261] Specifically, the dielectric constant and dielectric loss tangent of the resin film can be measured by the method described in the examples.

[0262] The saturated water absorption of the resin film is 1.0% or less, preferably 0.9% or less, and more preferably 0.8% or less under the conditions of 85° C. and 85% relative humidity.

[0263] Specifically, the saturated water absorption of the resin film can be measured by the method described in Examples.

[0264] As the molding material of the resin film, additives other than the polyimide resin powder may be blended as needed within a range that does not impair the properties of the polyimide resin powder.

[0265] Examples of additives include matting agents, plasticizers, antistatic agents, anti-coloring agents, anti-gelling agents, colorants, antioxidants, conductive agents, resin modifiers, flame retardants, glass fibers, carbon fibers, crystal nucleating agents, crystallization retarders, slip modifiers, fluororesin powders, calcium carbonate powders and other low dielectric agents, and the like.

[0266] As glass fiber, NE glass with low dielectric properties is suitable. As flame retardant, from the viewpoint of improving the appearance of molded products, flame retardant with melting point and glass transition temperature or powdered flame retardant with a particle size of several microns or less is suitable. As fluororesin, powdered fluororesin with a particle size of several microns or less is suitable.

[0267] The amount of the additive compounded is not particularly limited, but is generally 50% by mass or less, preferably 0.0001 to 30% by mass, more preferably 0.001 to 15% by mass, and further preferably 0.01 to 10% by mass in the molding material from the viewpoint of maintaining the physical properties derived from the polyimide resin powder and expressing the additive effect.

[0268] In addition, as a molding material of the resin film, other resins other than the polyimide resin powder may be blended within a range that does not impair the properties of the polyimide resin powder.

[0269] As other resins, highly heat-resistant thermoplastic resins are preferred, and examples thereof include polyamide resins, polyester resins, polyimide resins other than the aforementioned polyimide resin powder, polycarbonate resins, polyetherimide resins, polyamideimide resins, polyphenylene ether imide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyarylate resins, liquid crystal polymers, polyether ketone resins (polyether ether ketone resins, polyether ketone resins, polyether ketone ketone resins, polyether ether ketone ketone resins, etc.), polybenzimidazole resins, fluororesins, etc. Among these, from the viewpoints of heat resistance (heat aging resistance, short-term heat resistance, physical property retention rate at high temperature, etc.), formability, strength, excellent dielectric properties at high temperature, and solvent resistance, at least one selected from the group consisting of polyetherimide resins, polyphenylene sulfide resins, and polyether ketone resins is preferred.

[0270] When the polyimide resin powder and other resins are used in combination, the blending ratio is not particularly limited as long as it does not inhibit the properties of the polyimide resin powder. Specifically, it can be arbitrarily selected within the range of 1 / 99 to 99 / 1 according to various required properties.

[0271] Among them, from the viewpoint of obtaining the effect of suppressing the increase of the dielectric loss tangent at high temperature, the content of the polyimide resin powder in the forming material for making the resin film is preferably 20% by mass or more, more preferably 45% by mass or more, further preferably 70% by mass or more, and further preferably 80% by mass or more. In addition, the upper limit is 100% by mass.

[0272] The above-mentioned molding material may be provided in a powder state for molding of a resin film or the like, or may be provided in a pellet state for molding of a resin film or the like.

[0273] The polyimide resin powder of the present invention has thermoplasticity and therefore can be easily produced into a film-like molded product (resin film) by thermoforming.

[0274] For example, the following methods can be listed: (i) a method in which a molding material containing polyimide resin powder is fed into an extrusion molding machine, directly extruded and then subjected to various types of thermal forming to obtain a film-like molded body; (ii) a method in which a molding material containing polyimide resin powder is fed into an extrusion molding machine, temporarily formed into pellets, and then subjected to various types of thermal forming using the pellets to obtain a film-like molded body; and (iii) a method in which a molding material containing polyimide resin powder is directly compression-molded using a hot pressing device to obtain a film-like molded body.

[0275] The method for producing a resin film preferably includes a step of heat-forming a molding material containing polyimide resin powder and various optional components as required at 300 to 410° C. As a specific procedure, for example, in the case of the method (ii) above, the following method can be mentioned.

[0276] First, a polyimide resin powder and various optional components as required are dry-blended, and then charged into an extruder, preferably melted at 300 to 410° C., melt-kneaded and extruded in the extruder to produce pellets.

[0277] Alternatively, the polyimide resin powder is charged into an extruder, preferably melted at 300 to 410° C., various optional components as required are added thereto, and charged into an extruder, melt-kneaded and extruded in the extruder to produce pellets.

[0278] After the prepared pellets are dried, they are put into a single screw extruder or a twin screw extruder equipped with a T die, preferably melt kneaded at 300-410°C, and the melt kneaded molding material is continuously extruded from various dies such as the T die of the single screw extruder or the twin screw extruder, and then preferably cooled by a metal roller as a cooling roller at 100-250°C, thereby obtaining a film-like molded body (resin film). It should be noted that after obtaining the film-like molded body, it can also be supplied to various stretching processes online or offline. As the stretching conditions in the stretching process, it is preferred that the film-like molded body can be preheated in a temperature range of 100-300°C, and preferably stretched to 1.1 times or more, more preferably stretched to 1.5 times or more along the MD direction and the TD direction. By stretching the film, the mechanical strength of the film itself can be improved, and the linear expansion coefficient in the stretching direction can be greatly reduced. Therefore, it is particularly suitable for multilayering with low linear expansion coefficient materials.

[0279] The resin film of the present invention also includes a plate-shaped or sheet-shaped film having a thickness of 5 mm or less.

[0280] The resin film may have any thickness depending on the application, and is not particularly limited if it is 2 to 1000 μm. When the resin film is applied to a high-frequency circuit substrate, the thickness of the resin film is preferably 5 to 800 μm, more preferably 10 to 500 μm, and further preferably 12.5 to 250 μm from the viewpoint of handling and thinning.

[0281] In addition, from the viewpoint of suppressing deformation during heating and cooling when making the copper-clad laminate described later, the linear expansion coefficient of the surface direction (X direction, Y direction) of the resin film of the present invention is preferably 80 ppm or less, more preferably 50 ppm or less, and further preferably 20 ppm or less in the temperature range of 50°C to the glass transition temperature of the resin film. In addition, from the viewpoint of suppressing deformation in the stacking direction when the resin film is highly multilayered, the linear expansion coefficient of the thickness direction (Z direction) of the resin film is preferably 300 ppm or less, more preferably 200 ppm or less, and further preferably 100 ppm or less in the range of 50°C to the glass transition temperature of the resin film. The resin film of the present invention has crystallinity, so it is easy to stack in the thickness direction and has a high glass transition temperature, so it is particularly expected to reduce the linear expansion coefficient in the thickness direction.

[0282] The resin film according to the present invention can suppress the increase of the dielectric loss tangent at high temperature, and therefore can be applied to, for example, high-frequency circuit substrates, copper-clad laminates (CCL), especially copper-clad laminates obtained using low-roughness (arithmetic mean roughness Ra=1μm or less) copper foil, bonding sheets, film capacitors, printed wiring substrates, coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines and other transmission lines; microwave antennas, millimeter-wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, three-layer board antennas, microstrip antennas, patch antennas, various sensors, vehicle-mounted radars, aerospace radars, semiconductor element materials, bearing covers, insulating shafts, brackets, seamless belts and other belts; heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, low-dielectric wire covering materials, antenna covers (radar antenna covers), antenna substrates for 5G smartphones / 5G terminals, 6G smartphone / 6G terminal antenna substrate, COF flexible substrate, optical communication module (TOSA / ROSA), 77GHz vehicle-mounted millimeter wave radar antenna substrate, terahertz wave radar antenna substrate, aircraft radar antenna substrate, tracked vehicle antenna substrate, 8K-TV cable, WiGig antenna substrate, tablet terminal, notebook PC, thin TV, roll-up TV, digital camera and other mobile terminals; digital home appliances, macro cell base stations, small cell base stations, C-RAN base stations, commercial drones, long-distance mobile drones, surveillance cameras, smart glasses, smart watches, high-frequency equipment wafers, wireless communication equipment, Wi-Fi chips, contact sensors, indoor servers, outdoor servers, industrial robot substrates, household robot communication substrates, satellites, space station communication equipment, etc. Among these, according to the resin film of the present invention, the rise of dielectric loss tangent at high temperature can be suppressed, and therefore, it is suitable for high-frequency circuit substrates and copper-clad laminates.

[0283] In addition, the powder itself can be used as a raw material for dry mixing, a filler, a raw material for compression molded products such as IC inspection tools, a toughening agent for CFRP, a toughening agent for thermosetting resins or thermoplastic resins, a heat resistance improver, a coating material, a lubricant, a raw material for 3D printers, a raw material for UD tapes, etc.

[0284] <High Frequency Circuit Substrate>

[0285] The present invention provides a high-frequency circuit substrate comprising the resin film of the present invention.

[0286] The high-frequency circuit substrate of the present invention may have any layer in addition to the aforementioned resin film, and is preferably composed of only the aforementioned resin film from the viewpoint of suppressing the increase of the dielectric loss tangent at high temperature. In this case, the resin composition constituting the high-frequency circuit substrate, the manufacturing method of the high-frequency circuit substrate, the dielectric properties (dielectric constant and dielectric loss tangent) of the high-frequency circuit substrate, the saturated water absorption rate and their suitable methods are the same as those described in the aforementioned resin film.

[0287] From the viewpoint of ensuring strength and dielectric properties, the thickness of the high-frequency circuit substrate is preferably 5 to 800 μm, more preferably 10 to 500 μm, and even more preferably 12.5 to 250 μm.

[0288] <Copper Clad Laminated Board>

[0289] The present invention also provides a copper-clad laminate including a layer formed from the resin film of the present invention.

[0290] The copper-clad laminate of the present invention only needs to have a layer formed by the resin film of the present invention (hereinafter also referred to as "resin film layer") and at least one copper foil layer. For example, a laminate having a structure in which a copper foil layer is laminated on at least one side, preferably both sides, of the resin film layer can be cited. The copper-clad laminate of such a structure is obtained by laminating the resin film of the present invention and the copper foil, for example, using a known method.

[0291] The resin film used to manufacture the copper-clad laminate can be manufactured by the same method as described above. From the viewpoint of ensuring the strength of the copper-clad laminate and improving the adhesion between the resin film layer and the copper foil layer, the thickness of the resin film and the resin film layer in the copper-clad laminate is preferably 5 to 500 μm, more preferably 10 to 300 μm, and further preferably 12.5 to 200 μm.

[0292] The copper foil used to manufacture the copper-clad laminate is not particularly limited, and commercially available rolled copper foil, electrolytic copper foil, etc. can be used. From the perspective of flexibility, rolled copper foil is more suitable. From the perspective of ensuring sufficient conductivity and improving adhesion to the resin film layer, the thickness of the copper foil layer and the copper foil used to form it is preferably 2 to 50 μm, more preferably 3 to 30 μm, and further preferably 5 to 20 μm. This thickness is relative to one layer of copper foil or one piece of copper foil.

[0293] In addition, the surface roughness of the copper foil used to manufacture the copper-clad laminate is not particularly limited. The surface roughness of the copper foil is directly related to the electrical properties of the laminate itself obtained after the resin film is attached. Generally speaking, the lower the roughness, the more excellent the dielectric properties of the laminate can be formed. Therefore, the value of the maximum height Rz of the copper foil surface is preferably in the range of 0.1 to 1 μm, more preferably in the range of 0.2 to 0.8 μm. The maximum height Rz of the copper foil surface can be measured using, for example, a surface roughness meter.

[0294] From the viewpoint of improving the strength and conductivity of the copper-clad laminate, the thickness of the copper-clad laminate is preferably 15 to 600 μm, more preferably 25 to 500 μm, and further preferably 50 to 300 μm. It should be noted that the copper-clad laminate may have any layer other than the resin film layer and the copper foil layer as long as the effect of the present invention is not impaired.

[0295] The method for manufacturing the copper-clad laminate is not particularly limited, and the following method can be cited: the resin film of the present invention is overlapped with copper foil, and then laminated by a known method under heating and pressurizing conditions. The resin film of the present invention contains a thermoplastic polyimide resin, so it can be pressed and bonded to the copper foil in a state where the surface is thermally melted.

[0296] As a device for manufacturing a copper-clad laminate, any device that can paste a resin film and a copper foil under heating and pressurizing conditions can be used, and examples thereof include a roll laminator, a flat laminator, a vacuum pressurizing device, a double-belt pressurizing device, and the like. Among these, from the perspective of the productivity of the copper-clad laminate and the perspective of obtaining a copper-clad laminate with a good appearance, a double-belt pressurizing device is preferably used. The double-belt pressurizing device refers to a device that has a pair of endless belts arranged up and down, between which materials (resin film and copper foil) forming the film shape of each layer are continuously fed, and the aforementioned materials are heated and pressurized by means of the endless belt and a heating and pressing mechanism, thereby being able to manufacture a laminate.

[0297] Examples of the double-belt pressurizing device include a device described in Japanese Patent Application Laid-Open No. 2010-221694 and a double-belt pressurizing device manufactured by DYMCO.

[0298] The heating temperature when manufacturing the copper-clad laminate by the above method is not particularly limited as long as it is a temperature at which the resin film can be softened or melted. From the perspective of reducing the burden on the device and the manufacturing aspect, it is preferably in the range of 250 to 400°C, and more preferably in the range of 280 to 350°C. In addition, regarding the pressurization conditions when manufacturing the copper-clad laminate, from the perspective of improving the adhesion between the resin film and the copper foil, and reducing the burden on the device and the manufacturing aspect, the pressure is preferably 0.1 to 20 MPa, more preferably 0.15 to 15 MPa, and further preferably 0.2 to 12 MPa. In addition, from the perspective of improving production efficiency, the pressurization time is preferably in the range of 1 to 600 seconds, more preferably 5 to 400 seconds, and further preferably 10 to 300 seconds.

[0299] It should be noted that, about resin film of the present invention, it is characterized in that, can carry out heat fusion, in the manufacture of copper clad laminated board, also can use adhesive that resin film and copper foil are pasted.As adhesive, can arbitrarily select varnish-like adhesive, sheet-like adhesive, powdery adhesive etc.On the other hand, from the viewpoint of ensuring low dielectric properties, as adhesive, also be suitable for adhesive with low dielectric properties.As adhesive with low dielectric properties, can list out for example polyimide adhesive " PIAD " series of Arakawa Chemical Industries, Ltd. system.

[0300] Example

[0301] Next, the present invention will be described in more detail with reference to Examples, but the present invention is not limited thereto. In addition, various measurements and evaluations in each of the production examples, examples, and comparative examples were performed as follows.

[0302] (1) Physical properties of polyimide resin powder

[0303] (1-1) Infrared spectroscopy (IR measurement)

[0304] The IR measurement of the polyimide resin powder produced in each example was performed using "JIR-WINSPEC50" manufactured by JEOL Ltd.

[0305] (1-2) Logarithmic viscosity μ

[0306] The polyimide resin powder produced in each example was dried at 190 to 200° C. for 2 hours, and then 0.100 g of the polyimide resin powder was dissolved in 20 mL of concentrated sulfuric acid (96%, manufactured by Kanto Chemical Co., Ltd.). The polyimide resin solution obtained was used as a measurement sample and measured using a Cannon-Fresco viscometer at 30° C. The logarithmic viscosity μ was determined using the following formula.

[0307] μ=ln(ts / t0) / C

[0308] t0: Flow time of concentrated sulfuric acid

[0309] ts: Flow time of polyimide resin solution

[0310] C: 0.5 g / dL

[0311] (1-3) Melting point, glass transition temperature, crystallization temperature, crystallization heat

[0312] The melting point Tm, glass transition temperature Tg, crystallization temperature Tc, and crystallization heat ΔHm of the polyimide resin powder produced in each example were measured using a differential scanning calorimeter (“DSC-6220” manufactured by SII NanoTechnology).

[0313] In a nitrogen atmosphere, the polyimide resin powder was subjected to a thermal history of the following conditions: first heating (heating rate of 10°C / min), followed by cooling (temperature reduction rate of 20°C / min), and then second heating (heating rate of 10°C / min).

[0314] The melting point Tm is determined by reading the peak value of the endothermic peak observed in the second temperature increase. The glass transition temperature Tg is determined by reading the value observed in the second temperature increase. The crystallization temperature Tc is determined by reading the peak value of the exothermic peak observed during cooling.

[0315] In addition, the crystallization heat generation amount ΔHm (mJ / mg) was calculated from the area of ​​the exothermic peak observed during cooling.

[0316] (1-4) Half crystallization time

[0317] The half crystallization time of the polyimide resin powder produced in each example was measured using a differential scanning calorimeter ("DSC-6220" manufactured by SII NanoTechnology Co., Ltd.).

[0318] Regarding the measurement conditions for polyimide resins with a half-crystallization time of less than 20 seconds, the polyimide resin is completely melted by maintaining it at 420°C for 10 minutes under a nitrogen atmosphere, and then a rapid cooling operation is performed at a cooling rate of 70°C / minute. The time taken from the appearance of the crystallization peak observed at this time to the peak top is calculated to determine the crystallization time.

[0319] (1-5) Weight average molecular weight

[0320] The weight average molecular weight (Mw) of the polyimide resin powder produced in each example was measured under the following conditions using a gel permeation chromatography (GPC) measuring apparatus "Shodex GPC-101" manufactured by Showa Denko K.K.

[0321] Column: Shodex HFIP-806M

[0322] Mobile phase solvent: HFIP containing 2 mM sodium trifluoroacetate

[0323] Column temperature: 40°C

[0324] Mobile phase flow rate: 1.0 mL / min

[0325] Sample concentration: about 0.1 mass%

[0326] Detector: IR detector

[0327] Injection volume: 100μm

[0328] Standard curve: Standard PMMA

[0329] (1-6) Volume average particle size (D10, D50, D90)

[0330] The D10, D50, and D90 of the polyimide resin powder produced in each example were determined based on the results of the laser diffraction particle size distribution measurement. Figures 1 to 10 .

[0331] As a measuring device, a laser diffraction light scattering particle size distribution measuring instrument "LMS-2000e" manufactured by Malvern was used. In the measurement of D10, D50, and D90 of the polyimide resin powder, water was used as a dispersion medium and the polyimide resin powder was fully dispersed under ultrasonic conditions. The measurement range was set to 0.02 to 2000 μm.

[0332] (2) Physical properties of resin films

[0333] (2-1) Saturated water absorption

[0334] The polyimide resin powder produced in Example 1 was used to prepare a resin film by the method described later, and 10 pieces of 10 mm×10 mm×50 μm thick were cut out and used as test pieces in one test.

[0335] According to JIS K7209:2000, the test piece was dried at 50°C for 24 hours, returned to room temperature in a desiccator, and the weight (W0) was measured in an environment of 23°C and 50% relative humidity. Next, the film was placed in a moisture desorption device IGASORP (manufactured by HEIDEN) and set to an environment of 85°C and 85% relative humidity, and the weight (W1) when the sample weight reached stability was measured. The saturated water absorption was calculated according to the following formula.

[0336] Saturated water absorption (%) = [(W1-W0) / W0] × 100

[0337] (2-2) Dielectric properties

[0338] Using the polyimide resin powder produced in Example 1, a resin film was prepared by the method described later, and cut into a size of 60 mm×75 mm×50 μm thick to prepare a test piece.

[0339] After drying the test piece in a dryer, it was immediately used for measurement. As the measuring equipment, a network analyzer P5007A (manufactured by Keysight Technologies), a split cylinder resonator 20GHz CR-720 (manufactured by EM LABO), a split cylinder temperature characteristic evaluation software CR-TC (manufactured by EM LABO), and an environmental tester SH-662 (manufactured by ESPEC) were used. According to IEC 62810, the cavity resonator perturbation method was used to measure the dielectric constant and dielectric loss tangent at a frequency of 10 GHz and 20 GHz in an environment of -40 to 150°C. The measured value was set as the average value of n=2.

[0340] [Example 1]

[0341] <Production of Polyimide Resin Powder>

[0342] 800 g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Emulsifier Co., Ltd.) and 191.95 g (0.88 mol) of pyromellitic dianhydride (manufactured by LONZA JAPAN Co., Ltd.) were introduced into a 2L separable flask equipped with a Dean Stark apparatus, a Liebig condenser, a thermocouple, and four paddle blades, and after nitrogen flow was set, the mixture was stirred at 150 rpm to form a uniform suspension solution. On the other hand, 43.81 g (0.308 mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 82.52 g (0.572 mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250 g of 2-(2-methoxyethoxy)ethanol using a 500 mL beaker to prepare a mixed diamine solution.

[0343] Using a plunger pump, it took 60 minutes to drop the mixed diamine solution into the suspension solution in the 2L separable flask. Heat was released due to the dropwise addition, but the internal temperature was adjusted to fall within the range of 40 to 80°C. When the mixed diamine solution was added dropwise, all nitrogen was flowed and the stirring blade speed was set to 250rpm. In addition, the maximum exothermic temperature during the dropwise addition was 65°C. After the dropwise addition was completed, 130g of 2-(2-methoxyethoxy)ethanol and 1.13g (0.0088mol) of n-octylamine (manufactured by Kanto Chemical Co., Ltd.) as an end-capping agent were added and further stirred. At this stage, a light yellow polyamic acid solution (c) with a solid content concentration of 20% by mass was obtained. Then, after the stirring speed was set to 200rpm, the polyamic acid solution (c) in the 2L separable flask was heated to 190°C. In the process of gradually heating up, the average heating rate of the liquid temperature in the range of 70 to 130°C was set to 0.91°C / minute for heating. During this period, precipitation of polyimide resin powder and dehydration associated with imidization were confirmed. The average temperature rise rate in the range of liquid temperature exceeding 130°C to 190°C was set to the same temperature rise rate as the average temperature rise rate in the range of 70 to 130°C, and then the temperature was raised, maintained at 190°C for 30 minutes, and then naturally cooled to room temperature and filtered. The obtained polyimide resin powder was washed with 300g of 2-(2-methoxyethoxy)ethanol and 300g of methanol, filtered, and dried in a dryer at 180°C for 10 hours to obtain 317g of polyimide resin powder.

[0344] The IR spectrum of the polyimide resin powder was measured. The IR spectrum of v(C=O) was 1768, 1697 (cm -1 ) The characteristic absorption of the imide ring was confirmed.

[0345] The physical properties of the polyimide resin powder were measured to have a logarithmic viscosity of 1.60 dL / g, a Tm of 323°C, a Tg of 184°C, a Tc of 266°C, a crystallization heat of 21.0 mJ / mg, a semi-crystallization time of less than 20 seconds, and a Mw of 55,000.

[0346] The composition and evaluation results of the polyimide resin powder in Example 1 are shown in Table 1. In addition, the mol% of the tetracarboxylic acid component and the diamine component in Table 1 are values ​​calculated from the charging amount of each component when producing the polyimide resin.

[0347] The polyimide resin powders obtained in Examples 2 to 4 and Comparative Examples 1 to 6 described below all had the same composition and evaluation results as those of the polyimide resin powder of Example 1 shown in Table 1.

[0348] [Table 1]

[0349] Table 1

[0350]

[0351] *1: Content ratio (mol %) of the repeating structural unit of formula (1) relative to the sum of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) in the polyimide resin

[0352] The abbreviations in Table 1 are as follows.

[0353] PMDA; Pyromellitic Dianhydride

[0354] 1,3-BAC; 1,3-bis(aminomethyl)cyclohexane

[0355] OMDA; 1,8-octamethylenediamine

[0356] [Example 2]

[0357] In the process of gradually heating the polyamic acid solution (c) to 190°C, the average heating rate was changed to a range of 70 to 130°C as shown in Table 2, and a polyimide resin powder was obtained in the same manner as in Example 1.

[0358] [Example 3]

[0359] A polyimide resin powder was obtained in the same manner as in Example 1 except that the amount of 2-(2-methoxyethoxy)ethanol added to pyromellitic dianhydride was 665 g, the amount of 2-(2-methoxyethoxy)ethanol added to the mixed diamine was 208 g, and the amount of 2-(2-methoxyethoxy)ethanol added after the completion of the dropwise addition was 84 g.

[0360] [Example 4]

[0361] A polyimide resin powder was obtained in the same manner as in Example 3 except that the average temperature increase rate was changed within the range of 70 to 130° C. as shown in Table 2 while gradually increasing the temperature of the polyamic acid solution (c) to 190° C.

[0362] [Comparative Example 1]

[0363] A polyimide resin powder was obtained in the same manner as in Example 1 except that the amount of pyromellitic dianhydride was 76.69 g (0.353 mol), the amount of 1,3-bis(aminomethyl)cyclohexane was 17.57 g (0.123 mol), the amount of 1,8-octamethylenediamine was 33.09 g (0.229 mol), and the amount of n-octylamine was 0.453 g (0.00352 mol).

[0364] [Comparative Example 2]

[0365] A polyimide resin powder was obtained in the same manner as in Example 1 except that the amount of pyromellitic dianhydride was 295.3 g (1.359 mol), the amount of 1,3-bis(aminomethyl)cyclohexane was 67.64 g (0.474 mol), the amount of 1,8-octamethylenediamine was 127.4 g (0.882 mol), and the amount of n-octylamine was 1.74 g (0.0136 mol).

[0366] [Comparative Examples 3 to 6]

[0367] A polyimide resin powder was obtained in the same manner as in Comparative Example 2 except that the average temperature increase rate was changed within the range of 70 to 130° C. as shown in Table 2 while gradually increasing the temperature of the polyamic acid solution (c) to 190° C.

[0368] The results of volume average particle diameter D10, D50, and D90 of the polyimide resin powders obtained in Examples 1 to 4 and Comparative Examples 1 to 6 are shown in Table 2, and the results of particle size distribution are shown in Table 2. Figures 1 to 10 It should be noted that according to Figures 1 to 10 The results were evaluated on the shape of the particle size distribution according to the following criteria and are shown in Table 2.

[0369] A: Unimodal distribution and very sharp

[0370] (D10 / D50 is 0.7 to 0.9 and D90 / D50 is 1.1 to 1.4)

[0371] B: Unimodal distribution and sharp

[0372] (D10 / D50 is 0.45 to 0.9, and D90 / D50 is more than 1.4 and less than 2.0)

[0373] C: Bimodal distribution with sharp main peak

[0374] (Bimodal, but D10 / D50 is 0.45 to 0.9, and D90 / D50 is more than 1.4 and less than 2.0)

[0375] D: Bimodal distribution and very broad

[0376] (D10 / D50 is 0.45 to 0.9 and D90 / D50 exceeds 2.0)

[0377] E: Multimodal distribution with more than three peaks

[0378] [Table 2]

[0379] Table 2 Production conditions and evaluation results of polyimide resin powder

[0380]

[0381] The following conclusions can be drawn from the results listed in Table 2.

[0382] In Examples 1 to 4, the solid content concentration of the solution (c) containing the polyimide resin precursor containing polyamic acid is set to a specific range (15 to 25% by mass), and the average heating rate within the temperature range (70 to 130° C.) when the polyimide resin precursor containing polyamic acid is imidized is set to a specific range (0.5 to 8° C. / min) to produce a polyimide resin powder having a volume average particle size D50 in a specific range (specifically 5 to 50 μm) and having a good particle size distribution. In particular, in Examples 1 to 2, a polyimide resin powder having a unimodal and very sharp particle size distribution is obtained.

[0383] On the other hand, in Comparative Examples 1 to 6, the solid content concentration of the solution (c) containing the polyimide resin precursor containing polyamic acid deviates from the specific range, so that the volume average particle diameter D50 falling within the specific range (specifically, 5 to 50 μm) and the polyimide resin powder having a good particle size distribution cannot be obtained. In particular, in Comparative Example 1, only a polyimide resin powder having a multimodal particle size distribution with three or more peaks can be obtained.

[0384] [Example 5]

[0385] <Manufacturing of resin film>

[0386] The polyimide resin powder obtained in Example 1 was extruded using a twin-screw kneading extruder "TEM58SX" (manufactured by Shibaura Machine Co., Ltd.) at a barrel temperature of 250 to 330°C and a screw speed of 100 rpm. The strands extruded from the extruder were air-cooled and pelletized using a pelletizer ("Fan-Cutter fcwn30-12" manufactured by Star Plastics Co., Ltd.). The pellets of the obtained polyimide resin powder (hereinafter sometimes referred to as "pellets") were dried at 150°C for 12 hours. It should be noted that the size of the obtained pellets is: 3 to 4 mm in length and 2 to 3 mm in diameter.

[0387] The dried pellets were put into a single screw extruder with a 900 mm wide T die and a diameter of 40 mm, and melt-kneaded at a resin temperature of 340 to 360° C. The melt-kneaded polyimide resin was continuously extruded from the T die of the single screw extruder, and then cooled using a metal roll as a cooling roll at 150° C., thereby obtaining a resin film with a thickness of 50 μm. The saturated water absorption of the obtained resin film was 0.75%.

[0388] Here, the temperature of the φ40 mm single screw extruder was adjusted to 340-355°C, the temperature of the T die was adjusted to 355°C, and the temperature of the connecting pipe connecting the single screw extruder and the T die was adjusted to 355°C.

[0389] The results of the dielectric properties of the resin film of Example 5 obtained using the polyimide resin powder obtained in Example 1 are shown in Table 3. In addition, as a reference, the results of the dielectric properties of the resin film of Example 1 obtained using the thermoplastic liquid crystal polymer of Japanese Patent Application Laid-Open No. 2018-109090 are shown in Table 4.

[0390] [Table 3]

[0391] Table 3 Dielectric properties of resin films containing polyimide resin

[0392]

[0393] [Table 4]

[0394] Table 4 Dielectric properties of resin films containing liquid crystal polymers

[0395]

[0396] It can be seen that the dielectric loss tangent of the resin film (containing polyimide resin) shown in Table 3 at 10 GHz and 120°C is 20 Dielectric loss tangent Q at 40°C 40 The ratio (Q 120 / Q 40 ) is 1.29, and the dielectric loss tangent at 20 GHz and 120 ° C 20 Dielectric loss tangent Q at 40°C 40 The ratio (Q 120 / Q 40 ) is 1.5. Therefore, it is shown that the resin film of Example 5 obtained by using the polyimide resin powder of Example 1 can suppress the increase of the dielectric loss tangent at high temperature. It should be noted that the measurement results of the dielectric constant P and the dielectric loss tangent Q of the resin film of Example 5 at various temperatures when the measurement frequency is 10 GHz shown in Table 3 are shown in Fig.11The results of the dielectric constant P and dielectric loss tangent Q at various temperatures when the measurement frequency is 20 GHz are shown in Fig.12 .

[0397] On the other hand, Table 4 shows the dielectric properties of the resin film of Example 1 obtained using the thermoplastic liquid crystal polymer of Japanese Patent Application Laid-Open No. 2018-109090.

[0398] It can be seen that the dielectric loss tangent Q of the resin film (containing thermoplastic liquid crystal polymer) shown in Table 4 at 20 GHz and 120°C is 120 Dielectric loss tangent Q at 40°C 40 The ratio (Q 120 / Q 40 ) is 3.

[0399] The above also shows that the resin films (containing polyimide resin) shown in Table 3 are more excellent in suppressing the increase of dielectric loss tangent at high temperature than the resin films (containing thermoplastic liquid crystal polymer) shown in Table 4.

[0400] [Example 6]

[0401] <Manufacturing of Copper Clad Laminate>

[0402] The 50 μm thick resin film obtained in Example 5 was cut into an A4 size and used to produce a copper-clad laminate.

[0403] The above-mentioned resin film and a rolled copper foil with a thickness of 12 μm ("BHM-102F-HA-V2" manufactured by JX Metal Co., Ltd., A4 size, Rz of the welded surface with the resin film: 0.67 μm) were overlapped in the order of copper foil, resin film, and copper foil. Using a test double-belt pressurizing device manufactured by DYMCO, the layers were retained for 10 seconds under the conditions of a heating temperature of 300°C and a pressure of 0.22 MPa to produce a copper-clad laminate having a three-layer structure of a copper foil layer, a resin film layer, and a copper foil layer in sequence. For the obtained copper-clad laminate, the adhesion between the resin film and the copper foil was measured by a 90° peel test (JIS K6854-1:1999). In addition, for the appearance of the copper-clad laminate, the presence or absence of wrinkles was evaluated by visual observation.

[0404] The adhesion between the resin film and the copper foil and the appearance were evaluated in four stages of AA, A, B, and C, using the evaluation results of Example 6 as "A" as the standard.

[0405] [Examples 7 to 10]

[0406] A copper-clad laminate was produced and evaluated in the same manner as in Example 6 except that the copper foil used, the apparatus used, and the lamination conditions of the resin film and the copper foil were changed as shown in Table 5. The results are shown in Table 5.

[0407] The copper foils and the devices used in Table 5 are as follows.

[0408] (Copper foil)

[0409] Rolled copper foil (BHM-102F-HA-V2), manufactured by JX Metals, A4 size, Rz of the welded surface with the resin film: 0.67 μm, thickness: 12 μm

[0410] Electrolytic copper foil (TQ-M5-VSP), manufactured by Mitsui Mining & Smelting Co., Ltd., A4 size, Rz of the welded surface with the resin film: 0.70 μm, thickness: 12 μm

[0411] (Device used)

[0412] ·Double belt pressurizing device for testing, manufactured by DYMCO

[0413] ·Vacuum pressurizing device made by Kodaira Manufacturing Co., Ltd.

[0414] [Table 5]

[0415] Table 5

[0416]

[0417] Industrial Applicability

[0418] According to the manufacturing method of the present invention, a polyimide resin powder having a volume average particle size D50 in a specific range (specifically 5 to 50 μm) and having a good particle size distribution can be obtained. In addition, a resin film obtained by using a polyimide resin powder of a specific composition obtained by the manufacturing method of the present invention can suppress the increase of the dielectric loss tangent at high temperature.

[0419] The above-mentioned resin film can be applied to, for example, high-frequency circuit substrates, copper-clad laminates (CCL), especially copper-clad laminates obtained using low-roughness (arithmetic mean roughness Ra = 1 μm or less, maximum height Rz = 1 μm or less) copper foil, printed wiring substrates, coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines and other transmission lines; microwave antennas, millimeter wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, three-layer board antennas, microstrip antennas, patch antennas, various sensors, vehicle-mounted radars, aerospace radars, semiconductor component materials, bearing covers, insulating shafts, brackets, seamless belts and other various belts; heat-resistant low-dielectric tapes, heat-resistant low-dielectric tubes, low-dielectric wire covering materials, antenna covers (radar antenna covers), antenna substrates for 5G smartphones / 5G terminals, 6G smartphones / 6G terminals Antenna substrates for , chip on film (COF) flexible substrates, optical communication modules (TOSA / ROSA), antenna substrates for 77GHz automotive millimeter wave radars, antenna substrates for terahertz wave radars, antenna substrates for aircraft radars, antenna substrates for tracked vehicles, cables for 8K-TV, antenna substrates for WiGig, tablet terminals, notebook PCs, thin TVs, roll-up TVs, digital cameras and other mobile terminals; digital home appliances, macro cell base stations, small cell base stations, C-RAN base stations, commercial drones, long-distance mobile drones, surveillance cameras, smart glasses, smart watches, wafers for high-frequency devices, wireless communication equipment, Wi-Fi chips, contact sensors, indoor servers, outdoor servers, industrial robot substrates, communication substrates for household robots, artificial satellites, communication equipment for space stations, etc.

[0420] In addition, the powder itself can be used as a raw material for dry mixing, a filler, a raw material for compression molded products such as IC inspection tools, a toughening agent for CFRP, a toughening agent for thermosetting resins or thermoplastic resins, a heat resistance improver, a coating material, a lubricant, a raw material for 3D printers, a raw material for UD tapes, etc.

Claims

1. A method for producing a polyimide resin powder, wherein: The production method includes the step of reacting a tetracarboxylic acid component (A) containing tetracarboxylic dianhydride and a diamine component (B) containing an aliphatic diamine in the presence of a solvent (C) containing an alkylene glycol solvent represented by formula (1). The process comprises the steps of: preparing a solution (a) containing the tetracarboxylic acid component (A) in the solvent (C) and a solution (b) containing the diamine component (B) in the solvent (C), respectively, and then adding the solution (b) to the solution (a) or adding the solution (a) to the solution (b) to prepare a solution (c) containing a polyimide resin precursor containing a polyamic acid, Next, the solution (c) is heated to imidize the polyimide resin precursor containing polyamic acid, so that polyimide resin powder is precipitated in the solution. The solid content concentration of the solution (c) is 15 to 25% by mass, and the average temperature increase rate of the solution (c) during the heating in the temperature range of 70 to 130° C. is 0.5 to 8° C. / min. Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a straight-chain alkylene group having 2 to 6 carbon atoms, and n is an integer of 1 to 3.

2. The manufacturing method according to claim 1, wherein: The alkylene glycol-based solvent is at least one selected from the group consisting of 2-(2-methoxyethoxy)ethanol and 2-(2-ethoxyethoxy)ethanol.

3. The manufacturing method according to claim 1 or 2, wherein: The diamine component (B) comprises a diamine (B1) represented by the formula (B1-1) and a diamine (B2) represented by the formula (B2-1) as the aliphatic diamine, H2N-R1-NH2(UI-I) H2N-R2-NH2(B2-I) R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure, and R2 is a divalent chain aliphatic group having 5 to 20 carbon atoms.

4. The manufacturing method according to claim 1 or 2, wherein: The tetracarboxylic dianhydride is represented by formula (A-1), X is a tetravalent group having 6 to 22 carbon atoms and including at least one aromatic ring.

5. The manufacturing method according to claim 1 or 2, wherein: The tetracarboxylic dianhydride is pyromellitic dianhydride.

6. The manufacturing method according to claim 1 or 2, wherein: The solvent (C) further comprises 2-ethylhexanol. 7 . A method for producing a resin film, comprising: a step of producing a polyimide resin powder by the production method according to claim 1 ; and a step of thermally forming a molding material containing the polyimide resin powder.

8. The method for producing a resin film according to claim 7, wherein the resin film has a dielectric constant P of 10 GHz at 120°C. 120 The dielectric constant P at 40°C 40 Ratio P 120 / P 40 It is 0.8~1.

2.

9. The method for producing a resin film according to claim 7 or 8, wherein the dielectric loss tangent Q of the resin film at 10 GHz and 120°C is 120 Dielectric loss tangent Q at 40°C 40 Ratio Q 120 / Q 40 It is 1.0~1.

5.

10. The method for producing a resin film according to claim 7 or 8, wherein the resin film has a dielectric constant P at 20 GHz and at 120°C. 120The dielectric constant P at 40°C 40 Ratio P 120 / P 40 It is 0.8~1.

2.

11. The method for producing a resin film according to claim 7 or 8, wherein the dielectric loss tangent Q of the resin film at 20 GHz and 120°C is 120 Dielectric loss tangent Q at 40°C 40 Ratio Q 120 / Q 40 It is 1.0~1.

7. 12 . A method for producing a high-frequency circuit substrate, comprising the method for producing a resin film according to claim 7 . 13 . A method for producing a copper-clad laminate, comprising the method for producing a resin film according to claim 7 .