Preparation method of electrolytic copper foil, electrolytic copper foil and negative electrode material of lithium ion battery
By adding specific additives and optimizing electrolysis conditions during the preparation of electrolytic copper foil, the problem of insufficient tensile strength and elongation of lithium battery copper foil with a thickness of less than 8μm in the prior art has been solved, and a 5μm thick electrolytic copper foil with excellent performance has been prepared.
Patent Information
- Application Number
- CN202311075144.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-08-24
AI Technical Summary
Existing technologies struggle to simultaneously achieve good tensile strength and elongation when the thickness of the copper foil in lithium-ion batteries is less than 8 μm.
By adding specific proportions of leveling agent, brightener, high-resistance agent and wetting agent during the preparation of electrolytic copper foil, and optimizing the electrolyte composition and electrolysis conditions, an electrolytic copper foil with a thickness of 5μm was prepared.
This technology enables electrolytic copper foil to maintain its thinness while possessing excellent tensile strength and elongation properties.
Smart Images

Figure CN117051447B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrolytic copper foil, and in particular to a method for preparing electrolytic copper foil, electrolytic copper foil and a negative electrode material for a lithium-ion battery. Background Art
[0002] Lithium battery copper foil is one of the important raw materials for lithium batteries, and serves as a carrier for the negative current collector and negative active material of lithium batteries. The methods for preparing lithium battery copper foil mainly include calendering and electrolysis. The cost of calendering is much higher than that of electrolysis. Electrolysis is currently the most commonly used method for large-scale production of lithium battery copper foil. The steps of producing lithium battery copper foil by electrolysis mainly include copper dissolution process, electrolytic deposition process, passivation process, baking process and winding process.
[0003] As electronic devices using lithium-ion batteries are becoming smaller and thinner, lithium battery copper foil needs to be thinner and lighter while maintaining existing performance. In the background art, when the thickness of lithium battery copper foil is less than 8 μm, it is difficult to obtain lithium battery copper foil products with both good tensile strength and elongation using existing preparation methods. Summary of the invention
[0004] In view of the above problems, the embodiments of the present application provide a method for preparing an electrolytic copper foil, an electrolytic copper foil and a negative electrode material for a lithium-ion battery to solve the above technical problems.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing an electrolytic copper foil, wherein the thickness of the electrolytic copper foil is 5 μm, comprising:
[0006] adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0007] Supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying voltage between the anode plate and the cathode roller, electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0008] Among them, the additives include 12 to 14 parts by mass of a leveling agent, 26 to 28 parts by mass of a brightener, 0.2 to 0.4 parts by mass of a high-resistance agent and 4 to 6 parts by mass of a wetting agent; the leveling agent includes collagen and polyethylene glycol, the brightener includes sodium polydisulfide dipropane sulfonate, the high-resistance agent includes thiourea, and the wetting agent includes polyol polyoxyethylene ether.
[0009] In a second aspect, an embodiment of the present application provides an electrolytic copper foil, which is obtained according to the above-mentioned method for preparing the electrolytic copper foil.
[0010] In a third aspect, an embodiment of the present application provides a negative electrode material for a lithium-ion battery, comprising the above-mentioned electrolytic copper foil.
[0011] The preparation method of electrolytic copper foil, electrolytic copper foil and lithium-ion battery negative electrode material provided in the embodiments of the present application, the additives in the second electrolyte include 12 to 14 parts by mass of a leveling agent, 26 to 28 parts by mass of a brightener, 0.2 to 0.4 parts by mass of a high-resistance agent and 4 to 6 parts by mass of a wetting agent; the leveling agent includes collagen and polyethylene glycol, the brightener includes sodium polydisulfide dipropane sulfonate, the high-resistance agent includes thiourea, and the wetting agent includes polyol polyoxyethylene ether; through the above method, the components of the additives and the ratio of each component are improved, and the 5μm electrolytic copper foil obtained by electrolysis with the above second electrolyte has good tensile strength and elongation at the same time.
[0012] These and other aspects of the present application will become more clearly understood in the description of the following embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 A flow chart of a method for preparing an electrolytic copper foil provided in an embodiment of the present application is shown. DETAILED DESCRIPTION
[0014] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0015] In order to enable those skilled in the art to better understand the solutions of the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application.
[0016] In the embodiments of the present application, it should be noted that, in this article, relational terms such as first and second, etc. are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.
[0017] Moreover, the terms "comprises," "comprising," or any other variation thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the process, method, article, or apparatus that includes the element.
[0018] In the description of the embodiments of the present application, words such as "example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "example" or "for example" in the embodiments of the present application is not to be interpreted as being more preferred or having more advantages than another embodiment or design. The use of words such as "example" or "for example" is intended to present relative concepts in a clear manner.
[0019] In addition, the "plurality" in the embodiments of the present application refers to two or more than two. In view of this, in the embodiments of the present application, "plurality" can also be understood as "at least two". "At least one" can be understood as one or more, for example, one, two or more. For example, including at least one means including one, two or more, and there is no limit on which ones are included. For example, including at least one of A, B and C, then A, B, C, A and B, A and C, B and C, or A, B and C can be included.
[0020] The present application provides a method for preparing an electrolytic copper foil. Figure 1 As shown, the preparation method of the electrolytic copper foil comprises the following steps:
[0021] S11, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0022] Among them, the first copper sulfate electrolyte includes copper sulfate, sulfuric acid and hydrochloric acid; copper sulfate and sulfuric acid are the main components in the first sulfuric acid electrolyte and the second copper sulfate electrolyte, both of which participate in the electrode process. A low copper sulfate concentration will cause the copper layer corresponding to the high current area to be easily burned, and a high copper sulfate concentration will cause the dispersion ability and leveling ability of the electrolyte to decrease; sulfuric acid can improve the conductivity of the electrolyte and make the copper layer formed by electrolytic deposition crystallize finer. Therefore, when the sulfuric acid concentration is low, the conductivity of the electrolyte is poor, which will lead to a decrease in the dispersion ability of the electrolyte; when the sulfuric acid concentration is high, the mobility of copper ions is reduced, which will lead to a decrease in the efficiency of copper layer formation and is not conducive to the extension and brightness of the formed copper layer. In addition, when the sulfuric acid concentration is increased, the concentration of copper sulfate needs to be appropriately reduced to avoid the precipitation of copper sulfate due to the decrease in the solubility of copper sulfate.
[0023] Hydrochloric acid can provide chloride ions, which are anode activators and can form a complex with copper ions CuCl + , so that the copper ion equilibrium potential moves negatively, and at the same time, it can eliminate the stress of the copper foil formed by electrolytic deposition, and can also help the anode dissolve. At the same time, it can produce synergistic effects with additives, for example, it can coordinate with brighteners to make copper foil bright, and coordinate with leveling agents to make copper foil flat. If the concentration of hydrochloric acid is low, the copper layer formed by electrolytic deposition will be easy to burn; if the concentration of hydrochloric acid is high, the color of the copper layer formed by electrolytic deposition will be white, which is not conducive to the improvement of brightness. In the process of electrolytic deposition, as the concentration of hydrochloric acid is appropriately increased, the elongation of copper foil increases.
[0024] Among them, the additives include leveling agent, brightener, high resistance agent and wetting agent. The function of the leveling agent is to improve the flatness of the copper foil, so that the copper foil obtained by electrolytic deposition is smoother than the surface of the cathode roller. The main function of the brightener is to make the surface of the copper foil bright. The main function of the high resistance agent is to improve the tensile strength of the copper foil. The function of the wetting agent is to reduce the surface tension of the copper foil, so that water can spread on the surface of the copper foil to wet the copper foil.
[0025] This embodiment is for a copper foil product with a thickness of 5 μm. The additives include 12 to 14 parts by mass of a leveling agent, 26 to 28 parts by mass of a brightener, 0.2 to 0.4 parts by mass of a high-resistance agent, and 4 to 6 parts by mass of a wetting agent; the leveling agent includes collagen and polyethylene glycol, the brightener includes sodium polydisulfide dipropane sulfonate, the high-resistance agent includes thiourea, and the wetting agent includes polyol polyoxyethylene ether.
[0026] Among them, the reduction of collagen in the leveling agent will lead to greater roughness of the copper foil; the reduction of sodium polydisulfide propane sulfonate will not only lead to a decrease in brightness but also a decrease in tensile strength; too high a content of thiourea will cause burnt scratches on the surface of the copper foil, and a decrease in the content of thiourea will lead to a decrease in the tensile strength of the copper foil; a decrease in polyol polyoxyethylene ether will lead to a poor wetting effect and a decrease in the elongation of the copper foil; an increase in polyol polyoxyethylene ether can improve the elongation of the copper foil, but will lead to a larger warpage. Therefore, by controlling the content of each component of the additive within the above range, a 5μm copper foil product with a roughness of 0.15μm to 0.45μm, an elongation of 5% to 9%, and a tensile strength of 400Map to 450Mpa can be obtained. In some preferred embodiments, a 5μm copper foil product with a roughness of 0.15μm to 0.30μm, an elongation of 5% to 9%, and a tensile strength of 400Map to 450Mpa can be obtained.
[0027] As an implementation mode, the mass of the additive added to 1L of electrolyte is 0.80g to 1.0g.
[0028] In some embodiments, the mass of the additive added to 1 L of electrolyte is 0.84 g.
[0029] S12, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0030] During the electrolysis process, copper ions in the second copper sulfate electrolyte are deposited on the surface of the cathode roller to form electrolytic copper foil, which is then peeled off from the cathode roller and enters a subsequent processing step.
[0031] As an embodiment, the anode plate may include a substrate and an activation layer stacked on the substrate, the activation layer makes the surface of the anode plate active and improves the conductivity, and the activation layer may include multiple metals, for example, the activation layer may include at least two of metal palladium, metal iridium, metal ruthenium, metal cobalt, metal lead and metal manganese. The substrate may be a steel plate or a titanium plate.
[0032] As an implementation method, since the copper foil formed by electrolytic deposition needs to be continuously peeled off from the cathode roller, the surface of the cathode roller is easily damaged. In order to increase the wear resistance of the cathode roller, the cathode roller can be a titanium roller or a steel rod with a chromium layer on the surface.
[0033] In this embodiment, the additives in the second electrolyte include 12 to 14 parts by mass of a leveling agent, 26 to 28 parts by mass of a brightener, 0.2 to 0.4 parts by mass of a high-resistance agent, and 4 to 6 parts by mass of a wetting agent; the leveling agent includes collagen and polyethylene glycol, the brightener includes sodium polydisulfide dipropane sulfonate, the high-resistance agent includes thiourea, and the wetting agent includes polyol polyoxyethylene ether; through the above method, the components of the additives and the ratio of each component are improved, and the 5μm electrolytic copper foil obtained by electrolysis using the above second electrolyte has good tensile strength and elongation at the same time.
[0034] As an embodiment, the leveling agent may include 5 to 50 parts by mass of collagen and 1 to 20 parts by mass of polyethylene glycol.
[0035] As an embodiment, the additive includes 12.8 to 13.2 parts by mass of a leveler, 26.8 to 27.2 parts by mass of a brightener, 0.28 to 0.32 parts by mass of a high resistance agent, and 4.8 to 5.2 parts by mass of a wetting agent.
[0036] In some embodiments, the leveling agent (A) may be a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1".
[0037] In some embodiments, the brightener (B) may be sodium polydisulfide dipropane sulfonate with the trade name of "SPS-CF" manufactured by Shenzhen Fuyida Material Technology Co., Ltd.
[0038] In some embodiments, the high resistance agent (C) can be thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3".
[0039] In some embodiments, the wetting agent (E) may be a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0040] In some embodiments, the additives in the second electrolyte include 13 parts by mass of a leveler, 27 parts by mass of a brightener, 0.3 parts by mass of a high resistance agent, and 5 parts by mass of a wetting agent.
[0041] As an embodiment, the first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0042] In this embodiment, part of the current in the electrolysis process is transferred by hydrogen ions in the second copper sulfate electrolyte, and the concentration of copper ions in the second copper sulfate electrolyte and the concentration of sulfuric acid are matched to better deposit copper ions on the cathode roller. At the same time, the concentration of chloride ions is controlled to accelerate the rate of electrolytic deposition, and the synergistic effect of chloride ions and additives can further improve the performance of electrolytic copper foil.
[0043] In some embodiments, the current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0044] In this embodiment, the concentration of copper ions in the second copper sulfate electrolyte, the concentration of sulfuric acid, and the intensity of the current applied between the anode plate and the cathode roller during electrolysis act together on the electrolytic deposition of copper ions. Therefore, controlling the concentration of copper ions in the first copper sulfate electrolyte to 84-96 g / L, controlling the concentration of sulfuric acid in the first copper sulfate electrolyte to 90-105 g / L, and controlling the current to 28-30 KA can achieve a better copper ion deposition effect. At the same time, the rotation speed of the cathode roller is controlled to 7.5-8.4 m / min to control the thickness of the electrolytic copper foil.
[0045] As an implementation mode, the roughness of the cathode roller is 0.12 to 0.17 Ra.
[0046] In this embodiment, during electrolytic deposition, the formation of the crystal phase structure of the electrolytic copper foil deposited on the cathode roller at a thickness of 0 to 1.5 μm depends on the grain roughness of the cathode roller surface, and the crystal phase structure at a thickness greater than 1.5 μm depends on the additive. Controlling the roughness of the cathode roller within the above range is conducive to improving the performance of the electrolytic copper foil, so that the tensile strength and elongation of the electrolytic copper foil can achieve better results at the same time.
[0047] In some embodiments, the roughness of the cathode roller is 0.14-0.15 Ra.
[0048] In some embodiments, the cathode roller can be polished according to the following steps:
[0049] The cathode roller is ground using a first grinding wheel, wherein the first grinding wheel is 80 mesh, the rotation speed of the first grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the first grinding wheel is 14-16 mm / min, and the grinding pressure of the first grinding wheel is 0.12-0.14 Mpa;
[0050] The cathode roller is ground using a second grinding wheel, wherein the second grinding wheel is 180 mesh, the rotation speed of the second grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the second grinding wheel is 11-13 mm / min, and the grinding pressure of the second grinding wheel is 0.14-0.16 Mpa;
[0051] The cathode roller is polished with a third grinding wheel, wherein the third grinding wheel has a mesh size of 320, a rotation speed of the third grinding wheel of 550-650 rpm, a rotation speed of the cathode roller of 40-50 m / min, a moving speed of the third grinding wheel of 11-13 mm / min, and a polishing pressure of the third grinding wheel of 0.14-0.16 MPa.
[0052] The grinding step of this embodiment is suitable for cathode rollers with less surface damage. Before electrolytic deposition, the cathode roller is ground to control the roughness of the cathode roller surface.
[0053] In other embodiments, the cathode roller can be polished according to the following steps:
[0054] The cathode roller is ground using a first grinding wheel, wherein the first grinding wheel is 80 mesh, the rotation speed of the first grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the first grinding wheel is 14-16 mm / min, and the grinding pressure of the first grinding wheel is 0.14-0.16 Mpa;
[0055] The cathode roller is ground using a second grinding wheel, wherein the second grinding wheel is 180 mesh, the rotation speed of the second grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the second grinding wheel is 14-16 mm / min, and the grinding pressure of the second grinding wheel is 0.14-0.16 Mpa;
[0056] The cathode roller is ground using a third grinding wheel, wherein the third grinding wheel has a mesh size of 320, a rotation speed of the third grinding wheel of 550-650 rpm, a rotation speed of the cathode roller of 40-50 m / min, a moving speed of the third grinding wheel of 11-13 mm / min, and a grinding pressure of the third grinding wheel of 0.14-0.16 Mpa;
[0057] The cathode roller is polished with a fourth grinding wheel, wherein the fourth grinding wheel is 600 mesh, the rotation speed of the third grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the third grinding wheel is 11-13 mm / min, and the polishing pressure of the third grinding wheel is 0.14-0.16 Mpa.
[0058] The grinding step of this embodiment is suitable for cathode rollers with relatively large surface damage. Before electrolytic deposition, the cathode roller is ground to control the roughness of the cathode roller surface.
[0059] As an implementation manner, the thickness of two ends of the anode plate is greater than the thickness of other regions of the anode plate.
[0060] In this embodiment, the thickness of the two ends of the anode plate is increased so that the thickness of the two sides of the electrolytic copper foil is greater than the thickness in the middle, thereby preventing the two sides of the electrolytic copper foil from curling.
[0061] As an implementation method, the method for preparing the electrolytic copper foil of this embodiment further includes the following steps:
[0062] Passivating the electrolytic copper foil peeled off from the surface of the cathode roller;
[0063] The electrolytic copper foil after the passivation treatment is cut into pieces.
[0064] In this embodiment, the peeled electrolytic copper foil is passivated and slit in sequence, and the slit copper foil may be further wound up.
[0065] An embodiment of the present application further provides an electrolytic copper foil, which is obtained according to the above-mentioned method for preparing the electrolytic copper foil.
[0066] An embodiment of the present application further provides a negative electrode material for a lithium-ion battery, comprising the above-mentioned electrolytic copper foil.
[0067] Example 1
[0068] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0069] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0070] Among them, the additives include 12 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5.5 parts by mass of a wetting agent (E); the mass ratio of collagen to polyethylene glycol in the leveling agent (A) is 3:1, the brightener (B) includes sodium polydisulfide dipropane sulfonate, the high-resistance agent (C) includes thiourea, and the wetting agent (E) includes polyol polyoxyethylene ether.
[0071] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0072] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0073] Wherein, the roughness of the cathode roller is 0.14-0.15Ra.
[0074] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0075] Example 2
[0076] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0077] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0078] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightening agent (B), 0.3 parts by mass of a high-resistance agent (C) and 6 parts by mass of a wetting agent (E); the mass ratio of collagen to polyethylene glycol in the leveling agent (A) is 4:1, the brightening agent (B) includes sodium polydisulfide dipropane sulfonate, the high-resistance agent (C) includes thiourea, and the wetting agent (E) includes polyol polyoxyethylene ether.
[0079] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0080] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0081] Wherein, the roughness of the cathode roller is 0.14-0.15Ra.
[0082] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0083] Example 3
[0084] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0085] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0086] Among them, the additives include 14 parts by mass of a leveling agent (A), 28 parts by mass of a brightening agent (B), 0.3 parts by mass of a high-resistance agent (C) and 4 parts by mass of a wetting agent (E); the mass ratio of collagen to polyethylene glycol in the leveling agent (A) is 92:1, the brightening agent (B) includes sodium polydisulfide dipropane sulfonate, the high-resistance agent (C) includes thiourea, and the wetting agent (E) includes polyol polyoxyethylene ether.
[0087] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0088] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0089] Wherein, the roughness of the cathode roller is 0.14-0.15Ra.
[0090] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0091] Example 4
[0092] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0093] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0094] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (Agent A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B Agent) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C Agent) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E Agent) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0095] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0096] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0097] Wherein, the roughness of the cathode roller is 0.14-0.15Ra.
[0098] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0099] Example 5
[0100] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0101] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0102] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 4 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0103] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0104] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0105] Wherein, the roughness of the cathode roller is 0.14-0.15Ra.
[0106] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0107] Example 6
[0108] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0109] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0110] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0111] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0112] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0113] Wherein, the roughness of the cathode roller is 0.12Ra.
[0114] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0115] Example 7
[0116] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0117] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0118] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0119] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0120] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0121] Wherein, the roughness of the cathode roller is 0.17Ra.
[0122] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0123] Comparative Example 1
[0124] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0125] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0126] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0127] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0128] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0129] Wherein, the roughness of the cathode roller is 0.10Ra.
[0130] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0131] Comparative Example 2
[0132] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0133] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0134] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.3 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0135] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0136] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0137] Wherein, the roughness of the cathode roller is 0.20Ra.
[0138] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0139] Comparative Example 3
[0140] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0141] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0142] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.1 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0143] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0144] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0145] Wherein, the roughness of the cathode roller is 0.12Ra.
[0146] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0147] Comparative Example 4
[0148] This embodiment provides a method for preparing an electrolytic copper foil, comprising the following steps:
[0149] Step 1, adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte;
[0150] Among them, the additives include 13 parts by mass of a leveling agent (A), 27 parts by mass of a brightener (B), 0.5 parts by mass of a high-resistance agent (C) and 5 parts by mass of a wetting agent (E); the leveling agent (A) is a leveling agent manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-1", the brightener (B) is a sodium polydisulfide dipropane sulfonate manufactured by Shenzhen Fuyida Material Technology Co., Ltd. under the trade name of "SPS-CF"; the high-resistance agent (C) is a thiourea manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-3"; the wetting agent (E) is a polyol polyoxyethylene ether manufactured by Meizhou Caibao Technology Co., Ltd. under the trade name of "TB-4".
[0151] The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
[0152] Step 2, supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying a voltage between the anode plate and the cathode roller, and electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller;
[0153] Wherein, the roughness of the cathode roller is 0.17Ra.
[0154] The current applied between the anode plate and the cathode roller during electrolysis is 28-30 KA, and the rotation speed of the cathode roller during electrolysis is 7.5-8.4 m / min.
[0155] The performance tests were performed on the electrolytic copper foils prepared in Examples 1 to 7 and Comparative Examples 1 to 4, and the results were as follows:
[0156] Table 1 Test results
[0157]
[0158] The above is only an implementation method of the present application. It should be pointed out that a person skilled in the art can make improvements without departing from the inventive concept of the present application, but these improvements are within the scope of protection of the present application.
Claims
1. A method for preparing an electrolytic copper foil, wherein the thickness of the electrolytic copper foil is 5 μm, characterized in that: include: adding an additive to the first copper sulfate electrolyte to obtain a second copper sulfate electrolyte; Supplying the second copper sulfate electrolyte between the anode plate and the cathode roller, applying voltage between the anode plate and the cathode roller, electrolyzing the second copper sulfate solution to form the electrolytic copper foil on the surface of the cathode roller; Among them, the additives include 12 to 14 parts by mass of a leveling agent, 26 to 28 parts by mass of a brightener, 0.2 to 0.4 parts by mass of a high-resistance agent and 4 to 6 parts by mass of a wetting agent; the leveling agent includes 5 to 50 parts by mass of collagen and 1 to 20 parts by mass of polyethylene glycol, the brightener includes sodium polydisulfide dipropane sulfonate, the high-resistance agent includes thiourea, and the wetting agent is a polyol polyoxyethylene ether with the trade name of "TB-4" manufactured by Meizhou Caibao Technology Co., Ltd.; the roughness of the cathode roller is 0.14 to 0.15Ra.
2. The method for preparing the electrolytic copper foil according to claim 1, characterized in that: The additives include 12.8 to 13.2 parts by mass of a leveling agent, 26.8 to 27.2 parts by mass of a brightening agent, 0.28 to 0.32 parts by mass of a high resistance agent, and 4.8 to 5.2 parts by mass of a wetting agent.
3. The method for preparing the electrolytic copper foil according to claim 1, characterized in that: The first copper sulfate electrolyte includes 84-96 g / L of copper ions, 90-105 g / L of sulfuric acid, and 20-30 mg / L of chloride ions.
4. The method for preparing an electrolytic copper foil according to claim 1, characterized in that: During electrolysis, the current applied between the anode plate and the cathode roller is 28-30 KA, and the rotation speed of the cathode roller is 7.5-8.4 m / min.
5. The method for preparing an electrolytic copper foil according to claim 1, characterized in that: The cathode roller is polished according to the following steps: The cathode roller is ground using a first grinding wheel, wherein the first grinding wheel is 80 mesh, the rotation speed of the first grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the first grinding wheel is 14-16 mm / min, and the grinding pressure of the first grinding wheel is 0.12-0.14 Mpa; The cathode roller is ground using a second grinding wheel, wherein the second grinding wheel is 180 mesh, the rotation speed of the second grinding wheel is 550-650 rpm, the rotation speed of the cathode roller is 40-50 m / min, the moving speed of the second grinding wheel is 11-13 mm / min, and the grinding pressure of the second grinding wheel is 0.14-0.16 Mpa; The cathode roller is polished with a third grinding wheel, wherein the third grinding wheel has a mesh size of 320, a rotation speed of the third grinding wheel of 550-650 rpm, a rotation speed of the cathode roller of 40-50 m / min, a moving speed of the third grinding wheel of 11-13 mm / min, and a polishing pressure of the third grinding wheel of 0.14-0.16 MPa.
6. The method for preparing an electrolytic copper foil according to claim 1, characterized in that: The thickness of the two ends of the anode plate is greater than the thickness of other regions of the anode plate.
7. The method for preparing an electrolytic copper foil according to claim 1, characterized in that: The method for preparing the electrolytic copper foil further comprises the following steps: Passivating the electrolytic copper foil peeled off from the surface of the cathode roller; The electrolytic copper foil after the passivation treatment is cut into pieces.
8. An electrolytic copper foil, characterized in that: The electrolytic copper foil is obtained according to the method for preparing the electrolytic copper foil according to any one of claims 1 to 7.
9. A negative electrode material for a lithium ion battery, characterized in that: Comprising the electrolytic copper foil as claimed in claim 8.