Aqueous zinc ion electrolyte additive and its application

By using maltodextrin as an additive in zinc ion batteries, the zinc ion deposition orientation is adjusted, the problems of zinc dendrites generation and hydrogen evolution corrosion are solved, the stability and cycle life of the battery are significantly improved, and the commercialization of zinc ion batteries is promoted. application.

CN117080580BActive Publication Date: 2024-11-12NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311229676.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-22
Publication Date
2024-11-12
Estimated Expiration
2043-09-22

AI Technical Summary

Technical Problem

Zinc ion batteries are prone to forming zinc dendrites during circulation, resulting in low electrochemical stability and cycle life, and the existing additives are high or toxic, limiting their commercial applications.

Method used

Maltodextrin is used as an additive for aqueous zinc ion electrolyte, and its hydroxyl-rich long-chain structure is adsorbed on the surface of the zinc electrode, adjust the zinc ion deposition orientation, refine the grains, inhibit the formation of zinc dendrites, and reduce the hydrogen evolution reaction.

Benefits of technology

It significantly improves the electrochemical stability and cycle life of zinc ion batteries, avoids the generation and corrosion of zinc dendrites, realizes low-cost and non-toxic electrolyte optimization, and promotes the application of zinc ion batteries in the energy storage field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117080580B_ABST
    Figure CN117080580B_ABST
Patent Text Reader

Abstract

The invention discloses an aqueous zinc ion electrolyte additive and an application thereof, belonging to the technical field of aqueous batteries. The aqueous zinc ion electrolyte additive is maltodextrin. The commonly used additive in the prior art is α-cyclodextrin, which regulates Zn by its own special supramolecular macrocycle. 2+ The diffusion pathway and deposition position of zinc can be induced by maltodextrin, which can induce zinc deposition and reduce the nucleation overpotential. Maltodextrin, on the other hand, can preferentially adsorb on the surface of zinc electrode by using its long chain structure rich in hydroxyl groups, thereby adjusting the orientation of zinc deposition and increasing the nucleation overpotential, making it easier to refine zinc grains and form a dense and uniform zinc deposition layer to achieve the purpose of inhibiting zinc dendrites. In addition, in the performance comparison of symmetrical batteries, the Zn / / Zn symmetrical battery with maltodextrin has a higher Zn / / Zn ratio at 1 mA / cm 2 The cycle life can reach more than 4000h at a current density of 2.547 W, which is much longer than the cycle life of α-cyclodextrin (1600h).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous batteries, and in particular relates to an aqueous zinc ion electrolyte additive and application thereof. Background Art

[0002] The development of battery energy storage systems is one of the hot topics in the current energy field. In particular, lithium-ion batteries have dominated the consumer electronics market since their introduction due to their high energy density, excellent cycle performance, and good multi-scenario compatibility. However, serious problems such as high cost, leakage of toxic substances, and potential for combustion and explosion have gradually been exposed in the development of lithium-ion batteries and have been criticized. Therefore, the development of efficient and available alternative products is what people expect.

[0003] Compared with traditional lithium-ion batteries based on organic electrolytes, aqueous zinc-ion batteries (ZIBs) have attracted much attention due to their unique advantages, such as high theoretical capacity, low redox potential (0.76V relative to the standard hydrogen electrode), high safety, high abundance, simple preparation conditions and environmental protection. However, zinc dendrites are easily formed at the zinc negative electrode during the cycle of zinc-ion batteries. The formation of dendrites accelerates the rate of hydrogen evolution in aqueous batteries, and the accelerated hydrogen evolution will lead to changes in local pH and form byproducts. The accumulation of ZHS on the surface of the zinc negative electrode aggravates the surface unevenness and increases the polarization. The increased polarization intensifies the growth of zinc dendrites. Therefore, problems such as dendrite problems, hydrogen evolution problems and side reactions affect and intensify each other. This vicious cycle leads to extremely low efficiency of zinc negative electrode deposition / stripping, which is not conducive to its commercialization and widespread application.

[0004] Among them, electrolyte additives have the most significant effect in inhibiting the growth of zinc dendrites, and trace amounts of additives do not require too much process cost. Therefore, it is of great significance to find a low-cost, non-toxic, and abundant additive to optimize the zinc ion battery electrolyte, thereby improving the zinc negative electrode and enhancing the electrochemical stability and cycle life of aqueous zinc ion batteries. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes an aqueous zinc ion electrolyte additive and its application. The strong affinity of the electrolyte additive to the surface of the zinc metal anode induces the zinc ions to deposit toward the (002) crystal plane, refines the grains, forms a fine-grained zinc deposition layer, and has a stronger adsorption effect on the crystal plane, isolating the direct contact between free water and the zinc anode surface, thereby reducing the hydrogen evolution reaction on the zinc anode surface, effectively avoiding the formation of zinc dendrites, and significantly reducing the corrosion and by-product formation on the zinc metal anode surface.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] Maltodextrin (MD) is used in aqueous zinc ion electrolyte as an aqueous zinc ion electrolyte additive.

[0008] The present invention also provides an aqueous zinc ion electrolyte additive, which is maltodextrin; the concentration of the maltodextrin in the aqueous zinc ion electrolyte is 0.1 mol / L to 0.8 mol / L.

[0009] Maltodextrin is used as an additive for aqueous zinc ion electrolyte. Maltodextrin, with its long chain structure rich in hydroxyl groups, preferentially adsorbs on the surface of zinc electrode, thereby adjusting the orientation of zinc deposition and increasing the nucleation overpotential, making it easier to refine zinc grains and form a dense and uniform zinc deposition layer, thereby achieving the purpose of inhibiting zinc dendrites. In addition, in the performance comparison of symmetrical batteries, the Zn / / Zn symmetrical battery with maltodextrin additive has a higher charge / discharge rate at 1 mA·cm -2 The cycle life can reach more than 4000h at a current density of 1.547 W, which is far longer than the cycle life of the battery with α-cyclodextrin as additive (1600h).

[0010] Furthermore, the concentration of maltodextrin in the aqueous zinc ion electrolyte is preferably 0.2 mol / L.

[0011] The aqueous zinc ion electrolyte additive is used in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.

[0012] An aqueous zinc ion battery electrolyte consists of a solvent, an electrolyte and the aqueous zinc ion electrolyte additive.

[0013] Further, in the aqueous zinc ion battery electrolyte, the solvent is deionized water;

[0014] The electrolyte is zinc sulfate (ZnSO4).

[0015] Furthermore, in the aqueous zinc ion battery electrolyte, the concentration of the electrolyte in the aqueous zinc ion battery electrolyte is 1.8 mol / L.

[0016] The aqueous zinc ion battery electrolyte is used in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.

[0017] An aqueous zinc ion battery consists of a positive electrode, a negative electrode, a diaphragm and the aqueous zinc ion battery electrolyte.

[0018] Furthermore, in the aqueous zinc ion battery, the positive electrode active material is MnO2, the negative electrode material is zinc sheet, zinc foil or zinc alloy, and the diaphragm material is glass fiber.

[0019] Furthermore, the positive electrode active material MnO2 is prepared by a hydrothermal synthesis method: first, 5 mmol K2MnO4 is dissolved in 70 mL H2O and stirred clockwise with a glass rod. After it is dissolved, 1.75 mL of concentrated HCl (concentration is 12 mol / L) is added. After stirring at room temperature (25±2°C) for 30 min, they are transferred to a 200 mL reactor respectively, and then the reactor is placed in a drying oven at 100°C and heated for 6 h to obtain the positive electrode active material MnO2.

[0020] Furthermore, when the positive electrode active material is MnO2, the preparation method of the positive electrode is as follows: first, MnO2 and a conductive agent (Ketjen black) are ground separately with a mortar, and then MnO2, a conductive agent (Ketjen black) and a binder (PVDF) are mixed in a mass ratio of 7:2:1, and N-methylpyrrolidone is used as a solvent. After grinding evenly in a mortar to obtain a slurry, a 200μm scraper is used on a coating infrared dryer to evenly apply the ground slurry on a PE (polyethylene) film, and then the slurry is placed in a vacuum drying oven to dry. After drying, a cutting machine is used to cut it into a positive electrode sheet with a diameter of 12mm, which is the positive electrode.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] The present invention uses maltodextrin as an additive for aqueous zinc ion battery electrolyte, preferably using 1.8M ZnSO4 as a basic electrolyte. During the zinc deposition process, maltodextrin induces zinc ions to deposit in the direction of the (002) crystal plane, which has the effect of refining grains and regulating the uniform deposition of zinc ions. In addition, since zinc atoms mainly grow horizontally on the (002) crystal plane of the zinc metal anode, the generation of dendrites can be effectively avoided. In addition, since maltodextrin is more easily adsorbed on the surface of the zinc metal anode and has a large adsorption energy on the (002) crystal plane, it can hinder the direct contact between water molecules and the zinc metal anode, reduce the water content at the interface between the zinc metal anode and the electrolyte, thereby alleviating the hydrogen evolution corrosion reaction of the zinc metal anode, and can significantly reduce the corrosion of the zinc metal anode surface and the generation of by-products.

[0023] The present invention uses maltodextrin as an additive in the aqueous zinc ion battery electrolyte, which not only has the effect of inhibiting dendrite growth and hydrogen evolution corrosion, but also can significantly improve the cycle life and stability of the aqueous zinc ion battery, which is of great significance in promoting its application in the field of large-scale energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0025] Figure 1The contact angle test diagrams of the electrolytes used in Example 1(a) and Comparative Example 1(b) are shown.

[0026] Figure 2 This is a SEM morphology image of the zinc electrode in Example 1 after 100 cycles of deposition in the electrolyte at a magnification of 2000 times.

[0027] Figure 3 This is the XRD diagram of the zinc electrode in Example 1 after being deposited in the electrolyte for 100 cycles.

[0028] Figure 4 This is a SEM morphology image of the zinc electrode in Comparative Example 1 after 100 cycles of deposition in the electrolyte at a magnification of 2000 times.

[0029] Figure 5 This is the XRD diagram of the zinc electrode in Comparative Example 1 after 100 cycles of deposition in the electrolyte.

[0030] Figure 6 In the figure, a is the cycle life test diagram of the Zn / / Zn symmetric battery of Example 1 and Examples 4 to 6 (1.8M ZnSO4 + xg MD) and Comparative Example 1 (1.8M ZnSO4), and b is the voltage curve of the Zn / / Zn symmetric battery of Example 1 and Examples 4 to 6 (1.8M ZnSO4 + xg MD) and Comparative Example 1 (1.8M ZnSO4) at 196h~201h, 1612h~1617h and 3078h~3083h, respectively, wherein x refers to the addition amount of MD, such as Example 1 is 1.8M ZnSO4+0.5g MD, Example 4 is 1.8MZnSO4+0.25g MD, Example 5 is 1.8M ZnSO4+1g MD, and Example 6 is 1.8M ZnSO4+2g MD.

[0031] Figure 7 At 10 mA cm -2 At a current density and a total time of 1 hour, the zinc deposition morphology in Example 1 was photographed once every 10 minutes using an optical microscope for in-situ observation of electron microscope images (the first to sixth images from left to right correspond to shooting times of 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, and 60 minutes, respectively).

[0032] Figure 8 At 10 mA cm -2 At a current density and a total time of 1 hour, the zinc deposition morphology in Comparative Example 1 was photographed once every 10 minutes using an optical microscope for in-situ observation of electron microscope images (the first to sixth images from left to right correspond to shooting times of 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, and 60 minutes, respectively).

[0033] Fig. 9 This is a linear voltammetric scan test graph of the aqueous zinc ion battery Zn / / MnO2 assembled by Example 2 (1.8M ZnSO4+0.5g MD) and Comparative Example 2 (1.8M ZnSO4).

[0034] Fig.10 This is the rate performance diagram of the aqueous zinc ion battery Zn / / MnO2 assembled by Example 2 (1.8M ZnSO4+0.5g MD) and Comparative Example 2 (1.8M ZnSO4).

[0035] Fig.11 It is a long cycle performance diagram of the aqueous zinc ion battery Zn / / MnO2 assembled in Example 2 (1.8M ZnSO4+0.5g MD) and Comparative Example 2 (1.8M ZnSO4), wherein ZnSO4-CE is the coulombic efficiency of the aqueous zinc ion battery Zn / / MnO2 assembled in Comparative Example 2 (1.8M ZnSO4), and ZnSO4+0.5g MD-CE is the coulombic efficiency of the aqueous zinc ion battery Zn / / MnO2 assembled in Example 2 (1.8M ZnSO4+0.5g MD). DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0041] Unless otherwise specified, the room temperature in the embodiments of the present invention refers to 25±2°C.

[0042] Example 1

[0043] This embodiment provides a method for preparing an aqueous zinc ion electrolyte: first, 51.76g of ZnSO4·7H2O is dissolved in 60mL of deionized water, and after stirring to completely dissolve, a 100mL volumetric flask is used to make a constant volume to prepare a 100mL electrolyte for standby use. Take out 5mL of the electrolyte, and add 0.5g of maltodextrin (i.e., the concentration of maltodextrin in the aqueous zinc ion electrolyte is 0.2mol / L) thereto, and stir it magnetically at room temperature until the maltodextrin is completely dissolved, and then stand it to obtain an aqueous zinc ion electrolyte containing maltodextrin (the final concentration of ZnSO4 in the system is 1.8M).

[0044] The contact angle of the aqueous zinc ion electrolyte prepared in Example 1 was tested using a contact angle measuring instrument. Figure 1 As shown in (a), the contact angle is 80°.

[0045] The aqueous zinc ion electrolyte prepared in Example 1 was used to assemble a Zn / / Zn symmetric battery and tested on a Xinwei test system. Figure 2 For a Zn / / Zn symmetric cell at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 SEM image after 100 cycles under the test conditions. Figure 3It is an XRD diagram. From the SEM diagram, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated. In addition, it can be observed from the XRD spectrum that after 100 cycles of the Zn / / Zn symmetrical battery, the position of the diffraction peak on the zinc anode surface is almost exactly the same as the diffraction peak position of bare zinc and zinc PDF#04-0831, and no other miscellaneous peaks appear, indicating that the Zn / / Zn symmetrical battery in Example 1 does not generate by-products after 100 cycles. In addition, the diffraction peak intensity of the Zn / / Zn symmetrical battery on the (002) crystal plane is significantly higher than that of bare zinc, and the diffraction peak intensity on the (101) crystal plane is significantly lower than that of bare zinc, which shows that maltodextrin can induce zinc ions to deposit in the direction of the (002) crystal plane, and has the effect of regulating the uniform deposition of zinc ions.

[0046] The aqueous zinc ion electrolyte prepared in Example 1 was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. Figure 6 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 4000h and exhibits a stable polarization voltage.

[0047] The aqueous zinc ion electrolyte prepared in Example 1 was used to assemble a Zn / / Zn symmetrical cell. The deposition time was 10 mA / cm 2 The Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in Example 1 was used for in-situ observation of zinc deposition at a current density of . Figure 7 As shown, within 1 hour, Zn 2+ The uniform deposition along the Zn interface without protrusions or bubbles is always observed, which indicates that the MD additive plays a significant positive role in regulating Zn deposition and controlling the nucleation sites.

[0048] Comparative Example 1

[0049] Prepare an electrolyte with a final concentration of 1.8 M ZnSO4 in an additive-free system: first dissolve 51.76 g ZnSO4·7H2O in 60 mL deionized water, stir it with a magnetic stirrer to completely dissolve it, and then use a 100 mL volumetric flask to make up to 100 mL of electrolyte.

[0050] The contact angle of the aqueous zinc ion electrolyte without additives prepared in Comparative Example 1 was tested using a contact angle measuring instrument. The contact angle was as follows: Figure 1As shown in (b), the contact angle is 95°, which is greater than the contact angle of 80° measured in Example 1. The results show that the aqueous zinc ion electrolyte containing maltodextrin has greater adsorption energy on the zinc foil. In the battery, maltodextrin molecules are more easily adsorbed on the surface of the zinc foil than water molecules, which can hinder the direct contact between water molecules and the zinc metal anode, reduce the water content at the interface between the zinc metal anode and the electrolyte, and thus alleviate the hydrogen evolution corrosion reaction of the zinc metal anode.

[0051] The additive-free aqueous zinc ion electrolyte prepared in Comparative Example 1 was used to assemble a Zn / / Zn symmetric battery and tested on the Xinwei test system. Figure 4 For a Zn / / Zn symmetric cell at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 SEM image after 100 cycles under the test conditions. Figure 5 The XRD diagram is shown in Figure 2. From the SEM diagram, it can be observed that after 100 cycles of the Zn / / Zn symmetric battery, the surface of the zinc anode is very rough, the direction of zinc deposition is very disordered, and there are obvious cellular zinc sulfate salts and dendritic zinc dendrites. In addition, from the XRD spectrum, it can be observed that after 100 cycles of the Zn / / Zn symmetric battery, the position and intensity of the diffraction peaks on the zinc anode surface are compared with the diffraction peaks of bare zinc and zinc PDF#04-0831. The battery has a diffraction peak of zinc sulfate salt near the diffraction angle of 15° to 30°, which also indicates the generation of by-products, and its zinc ions are deposited in the direction of the (101) crystal plane, and its zinc atoms grow vertically in this direction, which is easy to form zinc dendrites.

[0052] The additive-free aqueous zinc ion electrolyte prepared in Comparative Example 1 was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. Figure 6 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the Zn / / Zn symmetrical battery short-circuited at about 120 hours, and the voltage polarization was very unstable. It may be that zinc dendrites were generated inside the battery, which pierced the diaphragm and caused the battery to short-circuit.

[0053] The additive-free aqueous zinc ion electrolyte prepared in Comparative Example 1 was used to assemble a Zn / / Zn symmetric battery. The Zn / / Zn symmetric battery was assembled using an optical microscope at different deposition times at 10 mA cm -2 The in-situ observation of zinc deposition was performed on the Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in Comparative Example 1 at a current density of . Figure 8As shown, obvious Zn protrusions appeared on the surface of the Zn electrode after 30 minutes and the protrusions continued to grow into moss-like Zn protrusions and Zn dendrites over time, indicating that uneven Zn deposition led to the continuous growth of Zn dendrites.

[0054] Example 2

[0055] The difference between this embodiment and embodiment 1 is that 0.2 mol of MnSO4 is added to the electrolyte (to supplement the active Mn consumed in the operation of the full battery). 2+ ).

[0056] Comparative Example 2

[0057] The only difference between this comparative example and comparative example 1 is that 0.2 mol of MnSO4 is added to the electrolyte.

[0058] The aqueous zinc ion electrolyte prepared in Example 2 and Comparative Example 2 was used to assemble a Zn / / MnO2 full battery, and a linear voltammetric sweep test was performed on a Chenhua electrochemical workstation. Fig. 9 As shown, at a scan rate of 0.2 mV / s, the Zn / / MnO2 full batteries assembled using Example 2 and Comparative Example 2 have two oxidation peaks and two reduction peaks, and the positions of the oxidation peaks and the reduction peaks almost completely overlap, indicating that the maltodextrin additive in Example 2 did not change the chemical reaction of the positive electrode active material.

[0059] The aqueous zinc ion electrolyte prepared in Example 2 and Comparative Example 2 was assembled into a Zn / / MnO2 full battery and tested on a blue-power test system. Fig.10 As shown, at current densities of 0.2 A / g, 0.5 A / g, 1.0 A / g, 2.0 A / g, and 4.0 A / g, the deposition capacity is 1 mAh / cm 2 Under the test conditions, the aqueous zinc ion batteries using the electrolyte of Example 2 all obtained higher specific capacity, and were able to maintain stable circulation after the current was restored to 0.2 A / g, indicating that the full battery reversibility and capacity retention rate of Example 2 were good. Compared with the aqueous zinc ion batteries using the electrolyte of Comparative Example 2, it was difficult to maintain stable circulation when the current was restored to 2 A / g, and the full battery reversibility and capacity retention rate of Comparative Example 2 were poor.

[0060] The aqueous zinc ion electrolyte prepared in Example 2 and Comparative Example 2 was used to assemble a Zn / / MnO2 full battery, and a long cycle performance test was performed on the Xinwei test system. Fig.11 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2Under the test conditions, compared with the full battery of Comparative Example 2, the capacity decay of the aqueous zinc ion battery using the electrolyte of Example 2 is slower, and it has higher coulombic efficiency and cycle stability.

[0061] Example 3

[0062] The present embodiment provides a method for preparing an aqueous zinc ion electrolyte: first, 1.8M zinc sulfate is dissolved in 60mL deionized water, and after stirring to completely dissolve, a 100mL volumetric flask is used to make a constant volume to prepare a 100mL electrolyte for standby use. 5mL of the electrolyte is taken out, and 0.5g of maltodextrin (i.e., the concentration of maltodextrin in the aqueous zinc ion electrolyte is 0.2mol / L) is added thereto, and magnetic stirring is performed at room temperature until the maltodextrin is completely dissolved, and then the aqueous zinc ion electrolyte containing maltodextrin is obtained by standing.

[0063] The contact angle of the aqueous zinc ion electrolyte prepared in Example 1 was tested using a contact angle meter, and the contact angle was 80°.

[0064] The aqueous zinc ion electrolyte prepared in this embodiment is assembled into a Zn / / Zn symmetrical battery and tested on a Xinwei test system. From the SEM image, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated. In addition, from the XRD spectrum, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the position of the diffraction peak on the surface of the zinc anode is almost exactly the same as the position of the diffraction peak of bare zinc and zinc PDF#04-0831, and no other miscellaneous peaks appear, indicating that the Zn / / Zn symmetrical battery in this embodiment does not generate by-products after 100 cycles. In addition, the diffraction peak intensity of the Zn / / Zn symmetric battery on the (002) crystal plane is significantly higher than that of bare zinc, and the diffraction peak intensity on the (101) crystal plane is significantly lower than that of bare zinc, which indicates that maltodextrin can induce zinc ions to deposit toward the (002) crystal plane and has the effect of regulating the uniform deposition of zinc ions.

[0065] The aqueous zinc ion electrolyte prepared in this example was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 4000h and exhibits a stable polarization voltage.

[0066] The aqueous zinc ion electrolyte prepared in this embodiment was used to assemble a Zn / / Zn symmetric battery. An optical microscope was used to observe the zinc deposition in situ on the Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in this embodiment. It can be observed that the zinc deposition process maintains a flat, uniform and dense deposition morphology, and no dendrites appear.

[0067] Example 4

[0068] The present embodiment provides a method for preparing an aqueous zinc ion electrolyte: first, 1.8M zinc sulfate is dissolved in 60mL deionized water, and after stirring to completely dissolve, a 100mL volumetric flask is used to make a constant volume to prepare a 100mL electrolyte for standby use. 5mL of the electrolyte is taken out, and 0.25g of maltodextrin (i.e., the concentration of maltodextrin in the aqueous zinc ion electrolyte is 0.1mol / L) is added thereto, and magnetic stirring is performed at room temperature until the maltodextrin is completely dissolved, and then the aqueous zinc ion electrolyte containing maltodextrin is obtained by standing.

[0069] The aqueous zinc ion electrolyte prepared in this embodiment is assembled into a Zn / / Zn symmetrical battery and tested on a Xinwei test system. From the SEM image, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated. In addition, from the XRD spectrum, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the position of the diffraction peak on the surface of the zinc anode is almost exactly the same as the position of the diffraction peak of bare zinc and zinc PDF#04-0831, and no other miscellaneous peaks appear, indicating that the Zn / / Zn symmetrical battery in this embodiment does not generate by-products after 100 cycles. In addition, the diffraction peak intensity of the Zn / / Zn symmetric battery on the (002) crystal plane is significantly higher than that of bare zinc, and the diffraction peak intensity on the (101) crystal plane is significantly lower than that of bare zinc, which indicates that maltodextrin can induce zinc ions to deposit toward the (002) crystal plane and has the effect of regulating the uniform deposition of zinc ions.

[0070] The aqueous zinc ion electrolyte prepared in this example was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 4000h and exhibits a stable polarization voltage.

[0071] The aqueous zinc ion electrolyte prepared in this example was used to assemble a Zn / / Zn symmetric battery. The Zn / / Zn symmetric battery was assembled using an optical microscope at different deposition times at 10 mA cm -2The Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in this example was subjected to in-situ observation of zinc deposition at a current density of 1.5 %. 2+ The uniform deposition along the Zn interface without protrusions or bubbles is always observed, which indicates that the MD additive plays a significant positive role in regulating Zn deposition and controlling the nucleation sites.

[0072] Example 5

[0073] The present embodiment provides a method for preparing an aqueous zinc ion electrolyte: first, dissolve 1.8M zinc sulfate in 60mL deionized water, stir until completely dissolved, and then use a 100mL volumetric flask to make a constant volume to prepare a 100mL electrolyte for standby use. Take out 5mL of the electrolyte, add 1g of maltodextrin (i.e., the concentration of maltodextrin in the aqueous zinc ion electrolyte is 0.4mol / L), stir it magnetically at room temperature until the maltodextrin is completely dissolved, and then let it stand to obtain an aqueous zinc ion electrolyte containing maltodextrin.

[0074] The aqueous zinc ion electrolyte prepared in this embodiment is assembled into a Zn / / Zn symmetrical battery and tested on a Xinwei test system. From the SEM image, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated. In addition, from the XRD spectrum, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the position of the diffraction peak on the surface of the zinc anode is almost exactly the same as the position of the diffraction peak of bare zinc and zinc PDF#04-0831, and no other miscellaneous peaks appear, indicating that the Zn / / Zn symmetrical battery in this embodiment does not generate by-products after 100 cycles. In addition, the diffraction peak intensity of the Zn / / Zn symmetric battery on the (002) crystal plane is significantly higher than that of bare zinc, and the diffraction peak intensity on the (101) crystal plane is significantly lower than that of bare zinc, which indicates that maltodextrin can induce zinc ions to deposit toward the (002) crystal plane and has the effect of regulating the uniform deposition of zinc ions.

[0075] The aqueous zinc ion electrolyte prepared in this example was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 4000h and exhibits a stable polarization voltage.

[0076] The aqueous zinc ion electrolyte prepared in this embodiment was used to assemble a Zn / / Zn symmetric battery. An optical microscope was used to observe the zinc deposition in situ on the Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in this embodiment. It can be observed that the zinc deposition process maintains a flat, uniform and dense deposition morphology, and no dendrites appear.

[0077] Example 6

[0078] The present embodiment provides a method for preparing an aqueous zinc ion electrolyte: first, 1.8M zinc sulfate is dissolved in 60mL deionized water, and after stirring to completely dissolve, a 100mL volumetric flask is used to make a constant volume to prepare a 100mL electrolyte for standby use. 5mL of the electrolyte is taken out, and 2g of maltodextrin (i.e., the concentration of maltodextrin in the aqueous zinc ion electrolyte is 0.8mol / L) is added thereto, and magnetic stirring is performed at room temperature until the maltodextrin is completely dissolved, and then the aqueous zinc ion electrolyte containing maltodextrin is obtained by standing.

[0079] The aqueous zinc ion electrolyte prepared in this embodiment is assembled into a Zn / / Zn symmetrical battery and tested on a Xinwei test system. From the SEM image, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated. In addition, from the XRD spectrum, it can be observed that after 100 cycles of the Zn / / Zn symmetrical battery, the position of the diffraction peak on the surface of the zinc anode is almost exactly the same as the position of the diffraction peak of bare zinc and zinc PDF#04-0831, and no other miscellaneous peaks appear, indicating that the Zn / / Zn symmetrical battery in this embodiment does not generate by-products after 100 cycles. In addition, the diffraction peak intensity of the Zn / / Zn symmetric battery on the (002) crystal plane is significantly higher than that of bare zinc, and the diffraction peak intensity on the (101) crystal plane is significantly lower than that of bare zinc, which indicates that maltodextrin can induce zinc ions to deposit toward the (002) crystal plane and has the effect of regulating the uniform deposition of zinc ions.

[0080] The aqueous zinc ion electrolyte prepared in this example was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 4000h and exhibits a stable polarization voltage.

[0081] The aqueous zinc ion electrolyte prepared in this embodiment was used to assemble a Zn / / Zn symmetric battery. An optical microscope was used to observe the zinc deposition in situ on the Zn / / Zn symmetric battery assembled with the aqueous zinc ion electrolyte prepared in this embodiment. It can be observed that the zinc deposition process maintains a flat, uniform and dense deposition morphology, and no dendrites appear.

[0082] Comparative Example 3

[0083] The same as Example 1, except that the added additive is α-cyclodextrin, and the concentration of α-cyclodextrin in the aqueous zinc ion electrolyte is 0.2 mol / L.

[0084] The aqueous zinc ion electrolyte prepared in this comparative example was assembled into a Zn / / Zn symmetric battery and tested on a Xinwei test system. From the SEM image, it can be observed that there are small flakes and no discernible large flakes. In addition, from the XRD spectrum, it can be observed that the peak of the byproduct Zn4SO4(OH)6·xH2O is weaker than that in the blank electrolyte, which indicates that α-cyclodextrin regulates Zn through its own special supramolecular macrocycle. 2+ The diffusion pathway and deposition location of Zn are induced, and the nucleation overpotential is reduced, which is different from the role played by maltodextrin.

[0085] The aqueous zinc ion electrolyte prepared in this comparative example was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on the Xinwei test system. 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery is 1600h.

[0086] From the above content, it can be seen that the Zn / / Zn symmetrical battery with maltodextrin additive in the present invention has a high 2 The current density (deposition capacity is 1 mAh / cm 2 ) can achieve a cycle life of more than 4000h, far exceeding the cycle life of α-cyclodextrin (1600h).

[0087] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. The application of maltodextrin in aqueous zinc ion electrolyte is characterized in that: It is used as an additive for aqueous zinc ion electrolyte; The concentration of the maltodextrin in the aqueous zinc ion electrolyte is 0.1 mol / L to 0.8 mol / L.

2. An aqueous zinc ion electrolyte additive, characterized in that: The invention relates to maltodextrin, wherein the concentration of the maltodextrin in the aqueous zinc ion electrolyte is 0.1 mol / L to 0.8 mol / L.

3. Use of the aqueous zinc ion electrolyte additive according to claim 2 in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.

4. An aqueous zinc ion battery electrolyte, characterized in that: The aqueous zinc ion battery electrolyte consists of a solvent, an electrolyte and the aqueous zinc ion electrolyte additive according to claim 2.

5. The aqueous zinc ion battery electrolyte according to claim 4, characterized in that The solvent is deionized water; The electrolyte is zinc sulfate.

6. The aqueous zinc ion battery electrolyte according to claim 1, characterized in that The concentration of the electrolyte in the aqueous zinc ion battery electrolyte is 1.8 mol / L.

7. Use of the aqueous zinc ion battery electrolyte according to any one of claims 4 to 6 in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.

8. An aqueous zinc ion battery, characterized in that: The aqueous zinc ion battery consists of a positive electrode, a negative electrode, a separator and the aqueous zinc ion battery electrolyte according to any one of claims 4 to 6.

9. The aqueous zinc ion battery according to claim 8, characterized in that: The positive electrode active material is MnO2, the negative electrode material is zinc foil, and the separator material is glass fiber.