Titanium nitride ceramic and its preparation method and application

Titanium nitride ceramics prepared through inorganic powder solve the problem of limited application of block ceramics in many fields, and achieve high density and adjustable resistance ceramics. They are suitable for biomedical, high-temperature wear resistance and electrodes. They are equipped with Excellent mechanical and electrical conductivity.

CN117125986BActive Publication Date: 2024-11-12SHANDONG DONGDA NEW MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210544002.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-19
Publication Date
2024-11-12
Estimated Expiration
2042-05-19

AI Technical Summary

Technical Problem

The application of block titanium nitride ceramics in biomedical, high-temperature wear-resistant components, PTC heating, cutting tools, electrodes and electrical contacts is limited, and the prior art has failed to effectively utilize its excellent characteristics.

Method used

Titanium nitride ceramic made of inorganic powder, including titanium nitride, resistance regulator and sintering additive, can produce high bending strength, Vickers hardness and adjustable resistivity through specific mass ratios and preparation methods. Ceramic material, and high density titanium nitride ceramics are prepared by ball milling, molding and sintering steps.

Benefits of technology

It realizes effective application of titanium nitride ceramics in biomedical, high-temperature wear-resistant components, heating materials and electrodes, etc. It has excellent mechanical strength and conductivity, and can be adjusted in resistivity and resistance temperature coefficient, which is suitable for a variety of high-performance requirements. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003651370820000061
    Figure BDA0003651370820000061
  • Figure HDA0003651370830000011
    Figure HDA0003651370830000011
  • Figure HDA0003651370830000012
    Figure HDA0003651370830000012
Patent Text Reader

Abstract

The present invention discloses a titanium nitride ceramic and its preparation method and application. The titanium nitride ceramic is made of raw materials including inorganic powders, wherein the inorganic powders include titanium nitride, a resistance regulator and a sintering aid; the mass ratio of the titanium nitride, the resistance regulator and the sintering aid is 100:(1-110):(4-20). The titanium nitride ceramic in the present invention has high bending strength and Vickers hardness, and can be used in biomedicine, such as ceramic knees, bones, teeth, etc., high temperature wear-resistant parts, cutting tools, etc. In addition, the resistivity and resistance temperature coefficient of the titanium nitride ceramic in the present invention are adjustable and controllable, and can be used for the heating component of the atomization core of electronic cigarettes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials, and in particular to a titanium nitride ceramic and a preparation method and application thereof. Background Art

[0002] Titanium nitride, as a new type of multifunctional ceramic material, has excellent properties such as high melting point, high hardness, wear resistance, good chemical stability, good electrical and thermal conductivity and optical properties. Its melting point is 2930-2950℃. It is a good conductor of heat and electricity, and it has superconductivity at low temperatures. It is a material for manufacturing jet engines. With the development and breakthroughs of science and technology, titanium nitride plays different roles in many fields. Its unique golden metallic luster makes titanium nitride also used in the field of gold decoration.

[0003] Titanium nitride is often used in the form of coatings or films in practical fields. For example, titanium nitride coating on the front windshield of a car can effectively protect against the sun and provide heat insulation. Titanium nitride film has better electromagnetic signal permeability than metal film. The chemical properties of titanium nitride film are relatively stable, not easy to oxidize, and resistant to acid, alkali and organic solvent corrosion, so it can have a long service life. However, few people have studied blocky titanium nitride ceramics, which limits the application of titanium nitride ceramics in biomedicine, high temperature wear-resistant parts, PTC heating, cutting tools, electrodes and electrical contacts. Summary of the invention

[0004] In order to overcome the problems existing in the prior art, one of the objectives of the present invention is to provide a titanium nitride ceramic.

[0005] A second object of the present invention is to provide a method for preparing titanium nitride ceramics.

[0006] A third object of the present invention is to provide a conductive nail.

[0007] A fourth object of the present invention is to provide a heating plate.

[0008] A fifth object of the present invention is to provide an electrode pair.

[0009] A sixth object of the present invention is to provide an application of titanium nitride ceramics in conductive materials, heating materials or biomedical materials.

[0010] In order to achieve the above object, the technical solution adopted by the present invention is:

[0011] The first aspect of the present invention is to provide a titanium nitride ceramic, which is made of a raw material including an inorganic powder, wherein the inorganic powder includes titanium nitride, a resistance regulator and a sintering aid; the mass ratio of the titanium nitride, the resistance regulator and the sintering aid is 100:(1-110):(4-20).

[0012] Preferably, the titanium nitride has an average particle size of 0.4-3 μm and a purity greater than 98%.

[0013] Preferably, the mass ratio of titanium nitride to the resistance adjuster is: 100:(1-100); further preferably, the mass ratio of titanium nitride to the resistance adjuster is: 100:(5-90); even further preferably, the mass ratio of titanium nitride to the resistance adjuster is: 100:(5-70).

[0014] Preferably, the mass ratio of titanium nitride to sintering aid is 100:(4-18); further preferably, the mass ratio of titanium nitride to sintering aid is 100:(4-17); further preferably, the mass ratio of titanium nitride to sintering aid is 100:(4-15).

[0015] Preferably, the resistance adjuster is at least one of silicon oxide, aluminum oxide and zirconium oxide.

[0016] Preferably, the sintering aid is at least one of magnesium oxide, yttrium oxide, calcium oxide, cerium oxide, lanthanum oxide and copper sulfate.

[0017] Preferably, the inorganic powder further includes a titanium source.

[0018] Preferably, the mass ratio of the titanium source to titanium nitride is (0-50):100; further preferably, the mass ratio of the titanium source to titanium nitride is (1-40):100; even further preferably, the mass ratio of the titanium source to titanium nitride is (10-30):100.

[0019] Preferably, the titanium source is Ti powder, titanium sulfate, TiCl 4 、TiO 2 , at least one of butyl titanate.

[0020] Preferably, the titanium nitride ceramic further comprises the following preparation raw materials: a binder and a solvent.

[0021] Preferably, the mass ratio of the inorganic powder, binder and solvent is 1:(0.15-0.25):(1.2-1.8).

[0022] Preferably, the mass ratio of the inorganic powder to the binder is 1:(0.18-0.25); further preferably, the mass ratio of the inorganic powder to the binder is 1:(0.2-0.25).

[0023] Preferably, the mass ratio of the inorganic powder to the solvent is 1:(1.5-1.8); further preferably, the mass ratio of the inorganic powder to the solvent is 1:(1.6-1.8).

[0024] Preferably, the binder is organic glue; further preferably, the binder is at least one of phenolic resin, PVA, and PVB.

[0025] Preferably, the solvent is at least one of water, acetone and ethanol.

[0026] Preferably, the resistivity of the titanium nitride ceramic is 8.5×10 -7 ~9.8×10 -1 Ω·m; Further preferably, the resistivity of the titanium nitride ceramic is 8.5×10 -7 ~4.6×10 -4 Ω·m; Further preferably, the resistivity of the titanium nitride ceramic is 8.5×10 -7 ~9.6×10 -5 Ω·m.

[0027] Preferably, the temperature coefficient of resistance of the titanium nitride ceramic is 800-2600 ppm / °C; further preferably, the temperature coefficient of resistance of the titanium nitride ceramic is 1000-2600 ppm / °C; even further preferably, the temperature coefficient of resistance of the titanium nitride ceramic is 1630-2600 ppm / °C.

[0028] Preferably, the porosity of the titanium nitride ceramic is 0.2-1.1%; further preferably, the porosity of the titanium nitride ceramic is 0.3-0.9%; even further preferably, the porosity of the titanium nitride ceramic is 0.35-0.42%.

[0029] Preferably, the bending strength of the titanium nitride ceramic is 320 to 650 MPa; further preferably, the bending strength of the titanium nitride ceramic is 370 to 650 MPa; even further preferably, the bending strength of the titanium nitride ceramic is 450 to 650 MPa.

[0030] Preferably, the Vickers hardness of the titanium nitride ceramic is 16.5 to 25.5 GPa; further preferably, the Vickers hardness of the titanium nitride ceramic is 19 to 25.5 GPa; even further preferably, the Vickers hardness of the titanium nitride ceramic is 22 to 25.5 GPa.

[0031] The second aspect of the present invention is to provide a method for preparing the titanium nitride ceramic provided in the first aspect of the present invention, comprising the following steps: mixing, granulating, compression molding, and sintering the raw materials in sequence to obtain the titanium nitride ceramic.

[0032] Preferably, the preparation method further comprises a ball milling step; the ball milling step is located before the granulation step and after the mixing step. The particle size of the inorganic powder is further reduced by ball milling, so that the inorganic powder is mixed more evenly when preparing the ceramic, and the prepared ceramic is denser.

[0033] Preferably, the granulation step adopts one of spray granulation and dry sieving granulation.

[0034] Preferably, the drying temperature in the dry sieving granulation is 40-100°C.

[0035] Preferably, a drying and dehydration step is provided between the compression molding step and the sintering step.

[0036] Preferably, the drying temperature of the drying and dehydrating step is 100-250°C; further preferably, the drying temperature of the drying and dehydrating step is 150-250°C; even further preferably, the drying temperature of the drying and dehydrating step is 180-250°C.

[0037] Preferably, the sintering temperature is 1700-1850°C; further preferably, the sintering temperature is 1750-1850°C; even further preferably, the sintering temperature is 1750-1800°C.

[0038] Preferably, the sintering time is 0.8 to 3 hours; further preferably, the sintering time is 1 to 2.5 hours; further preferably, the sintering time is 1 to 2 hours.

[0039] Preferably, a preheating step is provided before the sintering step.

[0040] Preferably, the temperature of the preheating step is 600-1200°C; further preferably, the temperature of the preheating step is 800-1200°C.

[0041] Preferably, the preheating step lasts for 0.5 to 1 h.

[0042] The third aspect of the present invention is to provide a conductive nail made of the titanium nitride ceramic provided by the first aspect of the present invention.

[0043] Preferably, the resistance of the conductive nail is less than 50 mΩ.

[0044] The fourth aspect of the present invention is to provide a heating plate made of the titanium nitride ceramic provided by the first aspect of the present invention.

[0045] The fifth aspect of the present invention is to provide an electrode pair made of the titanium nitride ceramic provided by the first aspect of the present invention.

[0046] A sixth aspect of the present invention is to provide an application of titanium nitride ceramics in conductive materials, heating materials or biomedical materials.

[0047] The beneficial effects of the present invention are: the titanium nitride ceramics in the present invention have high bending strength and Vickers hardness, and can be used in biomedicine (ceramic knees, bones, teeth), high temperature wear parts, cutting tools, etc. In addition, the resistivity and resistance temperature coefficient of the titanium nitride ceramics in the present invention are adjustable and controllable, and can be used for the heating components of the atomization core of electronic cigarettes. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is the microstructure diagram of the titanium nitride ceramic in Example 1.

[0049] Figure 2 This is the microstructure diagram of the titanium nitride ceramic in Example 2.

[0050] Figure 3 This is the microstructure diagram of the titanium nitride ceramic in Example 3.

[0051] Figure 4 This is a real-life picture comparing the heating plate sample in Example 5 with a coin. DETAILED DESCRIPTION

[0052] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.

[0053] Example 1

[0054] The titanium nitride ceramic in this example is prepared by the following preparation method, which specifically includes the following steps:

[0055] (1) titanium nitride powder with an average particle size of 1.5 μm and a purity of 98%, silicon oxide, and magnesium oxide are mixed in a mass ratio of 90:6:4 to obtain a mixed powder, and then the mixed powder, a PVA solution with a concentration of 10%, and deionized water are mixed in a mass ratio of 100:25:160 to form a slurry, and ball milled in a ball mill to obtain a mixed slurry;

[0056] (2) spray granulating the mixed slurry;

[0057] (3) placing the granulated powder obtained in step (2) into a mold, and pressing the granulated powder into a ceramic green body at a pressure of 150 MPa using a press machine;

[0058] (4) placing the pressed ceramic green body in a drying oven at 150° C. to dry out the moisture in the ceramic green body;

[0059] (5) The ceramic green body is placed in a sintering furnace, and under vacuum, the temperature is raised to 1200° C. and kept at this temperature for 30 minutes. Then, argon gas is filled in, and when the sintering temperature reaches 1850° C., the temperature is kept at this temperature for 60 minutes to obtain the titanium nitride ceramic in this example, which has a relatively high density.

[0060] The titanium nitride ceramic in this example is processed into long strips, and the polished surface is dark gold in color. Figure 1 shown.

[0061] Example 2

[0062] The titanium nitride ceramic in this example is prepared by the following preparation method, which specifically includes the following steps:

[0063] (1) titanium nitride powder with an average particle size of 1.0 μm and a purity of 99%, aluminum oxide, and yttrium oxide are mixed in a mass ratio of 65:30:8 to obtain a mixed powder; the mixed powder, a PVB solution with a concentration of 35%, and anhydrous ethanol are mixed in a mass ratio of 100:15:120 to form a slurry, and ball-milled in a ball mill to obtain a mixed slurry;

[0064] (2) drying the mixed slurry and artificially granulating it to obtain granulated powder;

[0065] (3) placing the granulated powder into a mold and pressing it with a press machine at a pressure of 200 MPa to obtain a ceramic green body;

[0066] (4) placing the pressed ceramic green body in a drying oven at 100° C. to dry out the moisture in the ceramic green body;

[0067] (5) The ceramic green body is placed in a sintering furnace, and under vacuum, the temperature is raised to 600° C. and kept at this temperature for 30 minutes. Then, nitrogen is filled in, and when the sintering temperature reaches 1700° C., the temperature is kept at this temperature for 90 minutes to obtain the titanium nitride ceramic in this example, which has a relatively high density.

[0068] The titanium nitride ceramic in this example is processed into a long strip, and the polished surface of the long strip of titanium nitride ceramic is bright rose gold. The microstructure of the titanium nitride ceramic in this example is shown in Figure 2 shown.

[0069] Example 3

[0070] The titanium nitride ceramic in this example is prepared by the following preparation method, which specifically includes the following steps:

[0071] (1) titanium nitride powder with an average particle size of 0.5 μm and a purity of 98.5%, zirconium oxide, yttrium oxide, and titanium oxide are mixed in a mass ratio of 70:45:10:12 to obtain a mixed powder; the mixed powder, a 55% phenolic resin aqueous solution, and anhydrous ethanol are mixed in a mass ratio of 100:25:180 to form a slurry, and the slurry is ball-milled in a ball mill;

[0072] (2) spray granulating the mixed slurry to obtain granulated powder;

[0073] (3) placing the granulated powder into a mold and pressing it with a press at a pressure of 250 MPa to obtain a ceramic green body;

[0074] (4) placing the pressed ceramic green body in a drying oven at 80° C. to dry out the moisture in the ceramic green body;

[0075] (5) The ceramic green body is placed in a sintering furnace, and under vacuum, the temperature is raised to 800° C. and kept at this temperature for 60 minutes. Ammonia gas is then added, and when the sintering temperature reaches 1750° C., the temperature is kept at this temperature for 120 minutes to obtain the titanium nitride ceramic in this example, which has a relatively high density.

[0076] The titanium nitride ceramic in this example is processed into a crescent shape, and its polished surface is bright golden yellow. The microstructure of the titanium nitride ceramic in this example is shown in Figure 3 shown.

[0077] The porosity, resistivity, temperature coefficient of resistance, bending strength and Vickers hardness of the titanium nitride ceramics in Examples 1 to 3 were tested respectively according to the following test methods. The specific test methods are as follows:

[0078] The porosity test methods are: density drainage method;

[0079] The test method of resistivity is: test according to the method described in GB 5594.5-1985 standard;

[0080] The test method for bending strength is: refer to the method described in GB / T 6569-2006 standard;

[0081] The test method of Vickers hardness is: refer to the method described in GB / T 4340.1-2009 standard;

[0082] The test results of the above performance are shown in Table 1 below.

[0083] Table 1 Properties of titanium nitride ceramics in Examples 1 to 3

[0084]

[0085]

[0086] It can be seen from Table 1 that the porosity of the titanium nitride ceramics in Examples 1 to 3 of the present invention is 0.35 to 0.85%, which is relatively low, indicating that the titanium nitride ceramics in the present invention have a relatively high density. The resistivity of the titanium nitride ceramics in Examples 1 to 3 is 8.5×10 -7 ~4.6×10 -4 Ω·m, indicating that the titanium nitride ceramics of the present invention have excellent electrical conductivity. The bending strength of the titanium nitride ceramics in Examples 1 to 3 is 375 to 572 MPa, and the Vickers hardness is 19.5 to 24.6 GPa, indicating that the titanium nitride ceramics of the present invention have excellent mechanical strength. The temperature coefficient of resistance of the titanium nitride ceramics in Examples 1 to 3 is 820 to 2050 ppm / °C.

[0087] Example 4

[0088] The titanium nitride ceramic in Example 1 was processed into a nail-shaped electrode (referred to as a conductive nail, the color of the conductive nail was golden yellow), and a total of 6 conductive nails were processed, which were respectively recorded as conductive nail 1, conductive nail 2, conductive nail 3, conductive nail 4, conductive nail 5 and conductive nail 6. The diameter of the top of the conductive nail (i.e., the maximum diameter) was about 5.5 mm, and the length was about 6.3 mm. The top and the tail of the conductive nail were clamped with a milliohmmeter, and the resistance of a single conductive nail could be measured. The test results are shown in Table 2. Then, the top surfaces of the two conductive nails were bonded together (the bonding force did not exceed 80 g), and the tails of the two conductive nails were clamped with a milliohmmeter, and the contact resistance of the two conductive nails could be measured. The test results are shown in Table 2.

[0089] Table 2 Resistance test results of conductive nails in Example 4

[0090] Test samples Conductive nail 1 Conductive nail 2 Conductive nail 1 and conductive nail 2 are in contact Resistance (mΩ) 1.426 1.336 34 Test samples Conductive nail 3 Conductive nail 4 Conductive nail 3 and conductive nail 4 are in contact Resistance (mΩ) 1.613 1.493 29 Test samples Conductive nail 5 Conductive nail 6 Conductive nail 5 and conductive nail 6 are in contact Resistance (mΩ) 1.617 1.561 37

[0091] It can be seen from the measured data in Table 2 that the contact resistance of the conductive nail is very small. The resistance of a single conductive nail is 1.3-1.7 mΩ, while the resistance of the contact test of two conductive nails is 29-37, all of which are less than 50 mΩ. It can be used for charging electrodes of electronic devices such as Bluetooth headsets, smart watches and e-cigarettes.

[0092] Example 5

[0093] The titanium nitride ceramic in Example 2 is processed into a heating plate, the color of the heating plate is golden yellow, and the actual picture is as shown in FIG. Figure 4As shown, the number of prepared heating sheets is three, and the thicknesses of the three heating sheets are 0.5 mm (recorded as heating sheet 1), 0.8 mm (recorded as heating sheet 2), and 1.0 mm (recorded as heating sheet 3), respectively. The resistance value of the heating sheet can be measured by clamping the two sides of the heating sheet with a milliohm meter, and the test results are shown in Table 3. Then the heating sheet is inserted into the electronic cigarette simulation tester to carry out the heating physical and chemical test experiment, and the experimental test results are shown in Table 3.

[0094] Table 3 Performance test results of the heating plate in Example 5

[0095] Test samples Heating sheet 1 Heating sheet 2 Heating sheet 3 Thickness(mm) 0.5 0.8 1.0 Resistance(Ω) 0.85 0.53 0.43 Heating power(W) 15 10 7 Maximum temperature(℃) 285 320 350 Time(s) 1.9 2.2 2.8

[0096] It can be seen from Table 3 that the three heating plates of different thicknesses in this example have different corresponding resistances, but the three heating plates can all be quickly heated to 280-350°C within 3 seconds at a heating power of 7-15W. Compared with metal wire heating atomization, the titanium nitride ceramic heating plate in this example has a series of advantages such as simple structure, high heating cycle stability, adjustable resistivity, large resistance temperature coefficient control range, no metal volatile components, corrosion resistance, etc.; it can be seen that the heating plate made of titanium nitride ceramic material in the present invention has the characteristics of fast heating speed, high heat utilization rate, energy saving, uniform heating atomization, safety, environmental protection, health and long service life.

[0097] Example 6

[0098] The titanium nitride ceramic in Example 3 was processed into a crescent-shaped sample to obtain 6 crescent-shaped samples (i.e., electrode pairs). The color of the electrode pairs was golden yellow and they were respectively recorded as Sample 1, Sample 2, Sample 3, Sample 4, Sample 5 and Sample 6. Then, the electrode performance of the crescent-shaped titanium nitride ceramic in this example was tested, and specifically, voltage offset and noise tests were performed. The specific testing method was as follows: an ECG electrode electrical performance tester was used to test the offset voltage and noise of the electrode pair formed by Sample 1 + Sample 2, the electrode pair formed by Sample 3 + Sample 4, and the electrode pair formed by Sample 5 + Sample 6, respectively. The test results are shown in Table 4.

[0099] Table 4 Offset voltage and noise test results of crescent-shaped titanium nitride ceramics in Example 6

[0100] project Offset voltage(mV) Noise(μV) Sample 1 + Sample 2 0.0 14.5 Sample 3 + Sample 4 0.0 20.1 Sample 5 + Sample 6 0.0 33.7 Standard value ≤100 ≤150

[0101] It can be seen from Table 4 that the crescent-shaped titanium nitride ceramic electrode pair in this example shows excellent microcurrent sensitivity and excellent anti-interference ability, and can replace the traditional light wave components in smart watches to measure the microcurrent signals generated by the human heart beat; the titanium nitride ceramic electrode sheet in the present invention can continuously detect changes in pulse beats in a passive signal receiving mode, and transmit the data to the big data processing and analysis center through the 5G Internet of Things, which can monitor the health status of a person in real time online, and thus be applied to the medical industry.

[0102] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. Application of titanium nitride ceramics in biomedical materials, characterized in that: The titanium nitride ceramic is made of raw materials including inorganic powders, wherein the inorganic powders are composed of titanium nitride powder, zirconium oxide, yttrium oxide, and titanium oxide in a mass ratio of 70:45:10:12; the titanium nitride ceramic also includes the following preparation raw materials: a binder and a solvent; the mass ratio of the inorganic powder, the binder, and the solvent is 1: (0.15-0.25): (1.2-1.8); The titanium nitride ceramic is prepared by a preparation method comprising the following steps: The raw materials are sequentially mixed, ball-milled, spray-granulated, and molded to obtain a ceramic green body, dried to remove water, preheated, and sintered to obtain the titanium nitride ceramic; the temperature of the preheating step is 600-1200°C; the insulation time of the preheating step is 0.5-1h; the sintering temperature is 1700-1850°C, and the sintering insulation time is 0.8-3h; the preheating and sintering steps are specifically as follows: the ceramic green body is placed in a sintering furnace, and under a vacuum state, the temperature is raised to the temperature of the preheating step, and the temperature is kept, and then ammonia is filled to reach the sintering temperature, and the temperature is kept; The titanium nitride ceramic is processed into a crescent shape to form an electrode pair; the color of the electrode pair is golden yellow; The electrode pair continuously detects changes in pulse beats in a passive signal receiving mode, and transmits the data to a big data processing and analysis center via the 5G Internet of Things, thereby monitoring a person's health status in real time online, thereby being applied in biomedical materials.