A self-initiating cationic electrophoretic polyurethane acrylate resin and its preparation method and application

By reacting the photoactive chain extender with the isocyanate group in the water-based UV-curable coating and grafting it on the middle chain segment of the macromolecule, the problem of uneven dispersion of oil-soluble photoinitiators and migration of small molecules is solved, and high performance is achieved. Self-initiating cationic electrophoretic polyurethane acrylate resin with mechanical stability and impact resistance, eliminating the need for additional photoinitiators.

CN117126364BActive Publication Date: 2024-10-18GUANGDONG SHEN ZHAN IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311072948.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-24
Publication Date
2024-10-18
Estimated Expiration
2043-08-24

AI Technical Summary

Technical Problem

Oil-soluble photoinitiators in existing water-based UV-curable coatings are difficult to disperse evenly, resulting in uneven curing of the coating, residual migration of small molecule photoinitiators, slow curing speed, low hardness and unstable resin.

Method used

Using self-initiating cationic electrophoretic polyurethane acrylate resin, the photoactive chain extender E-2959 is reacted with the isocyanate group and grafted on the middle segment of the macromolecule to fix the photoinitiator active group and avoid small molecule photoinitiators migration, and no additional photoinitiator is required during preparation.

Benefits of technology

It achieves uniform dispersion and solidification of the photoinitiator, improves the mechanical stability and impact resistance of the coating, and solves the problems of slow curing speed and low hardness without adding a photoinitiator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117126364B_ABST
    Figure CN117126364B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of synthesis of ultraviolet light-cured resin polymer materials, and specifically relates to a self-initiating cationic electrophoretic polyurethane acrylate resin and a preparation method and application thereof, wherein the resin comprises the following components in parts by weight: 41.02 to 44.54 parts of IPDI, 29.13 to 31.57 parts of polycarbonate diol, 4.29 to 4.36 parts of N-methyldiethanolamine, 3.75 to 5.34 parts of 1,4-butanediol, 2.13 to 10.46 parts of E-2959 photoactive chain extender, 9.18 to 9.95 parts of hydroxyethyl acrylate, 2.16 to 2.20 parts of acetic acid, and a polymerization inhibitor; wherein the polymerization inhibitor is 0.05% to 0.10% of the solid content. The resin provided by the present invention does not require the addition of a photoinitiator, and there is almost no photoinitiator migration. The cured film has good hardness, excellent flexibility and impact resistance, and can be widely used in the coating of iron and coiled steel substrates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthesis of ultraviolet light-curing resin polymer materials, and in particular relates to a self-initiating cationic electrophoretic polyurethane acrylate resin and a preparation method and application thereof. Background Art

[0002] Electrophoretic coating is a new type of energy-saving, environmentally friendly and corrosion-resistant coating. It has the advantages of good water and chemical resistance, and is easy to realize mechanization and automation of the coating process. Electrophoresis is one of the most effective methods for coating metal workpieces. UV curing technology is a kind of curing source with ultraviolet light, which can quickly realize the cross-linking polymerization of polymers and has the advantages of high efficiency, energy saving and environmental protection. The combination of electrophoretic process and UV curing technology can realize environmentally friendly and efficient mechanized and automated coating of metal substrates.

[0003] Electrophoretic coatings are generally water-based coatings (such as water-based polyurethane, water-based acrylic emulsion, etc.), which have the disadvantages of slow curing and drying speed and low hardness. Water-based UV-curing coatings are applied by electrophoretic process. After the moisture on the coating surface is dried, they can be rapidly cross-linked and cured by ultraviolet light irradiation to achieve higher hardness and better wear resistance. However, water-based UV-curing coatings require the addition of photoinitiators. Generally, photoinitiators are oil-soluble substances and it is difficult to evenly disperse them in water-based UV-curing resins. Even if dispersed in the resin, their mechanical stability is relatively poor, which may cause uneven curing of the coating. At the same time, photoinitiators are small molecules, and incompletely decomposed photoinitiators remain inside the coating and will eventually slowly migrate to the surface of the coating, resulting in certain limitations on its scope of application.

[0004] Patent CN101481450A prepares a photosensitive self-initiating polyurethane acrylate oligomer by direct reaction of isocyanate groups with primary hydroxyl groups in photoinitiator 2959, which contains three oligomers with different structures: a polyurethane oligomer with acrylate double bonds at both ends (ineffective component), a polyurethane oligomer with acrylate double bonds at one end and photoinitiator 2959 at the other end (effective component), and a polyurethane oligomer with photoinitiator 2959 at both ends (non-photopolymerizable component). The mobility of the photoinitiator can be reduced to a certain extent, but the prepared oligomer contains two ineffective components, and the effective component contains only one photopolymerizable acrylate double bond. The curing speed is slow, and the hardness of the cured film is low, which cannot meet the application requirements.

[0005] Patent CN110835397A discloses a self-crosslinking water-based photocurable polyurethane and its preparation method. The self-initiated photocurable property is given by introducing benzophenone and acrylate double bonds in the side chain, and primary or secondary amine groups are introduced at both ends of the molecule. Since primary or secondary amines are easy to undergo Michael addition reaction with acrylate double bonds, it is possible that the acrylate double bonds in the resin molecules have undergone Michael addition reaction with primary or secondary amines before ultraviolet light exposure, which ultimately leads to instability of the emulsion system or even gelation. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a self-initiating cationic electrophoretic polyurethane acrylate resin and a preparation method and application thereof, which solves the problems that oil-soluble photoinitiators are difficult to evenly disperse in water-based UV-curing coatings, resulting in uneven coating curing, residual migration of small molecule photoinitiators, slow resin curing speed, low hardness of the cured film and unstable resin.

[0007] The first object of the present invention is to provide a self-initiating cationic electrophoretic polyurethane acrylate resin.

[0008] The second object of the present invention is to provide a method for preparing the self-initiating cationic electrophoretic polyurethane acrylate resin.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A self-initiating cationic electrophoretic polyurethane acrylate resin material comprises the following components in parts by weight: 41.02-44.54 parts of isophorone diisocyanate, 29.13-31.57 parts of polycarbonate diol, 4.29-4.36 parts of N-methyldiethanolamine, 3.75-5.34 parts of 1,4-butanediol, 2.13-10.46 parts of E-2959 photoactive chain extender, 9.18-9.95 parts of hydroxyethyl acrylate, 2.16-2.20 parts of acetic acid, and a polymerization inhibitor; the polymerization inhibitor is 0.05-0.10% of the solid content;

[0011] The structural formula of the photoactive chain extender E-2959 is

[0012]

[0013] Preferably, the self-initiating cationic electrophoretic polyurethane acrylate resin has a structure as shown in formula (I):

[0014]

[0015] in It is photoactive and can initiate double bond polymerization under ultraviolet light irradiation.

[0016] A method for preparing a self-initiating cationic electrophoretic polyurethane acrylate resin comprises the following steps:

[0017] S1, heating isophorone diisocyanate and polycarbonate diol to react; then dropping N-methyldiethanolamine and 1,4-butanediol thereinto, controlling the reaction temperature, and obtaining prepolymer I after the reaction;

[0018] S2, adding photoactive chain extender E-2959 to the prepolymer I obtained in step S1, reacting under heating conditions; then adding hydroxyethyl acrylate and a polymerization inhibitor, and reacting to obtain prepolymer II;

[0019] S3. Under heating and stirring conditions, acetic acid is added to the prepolymer II obtained in step S2, and the prepolymer III is obtained after heat preservation reaction. During the reaction process, a solvent is used to adjust the viscosity of the reaction system, and then the prepolymer III is added to water and stirred, and the solvent is removed to obtain the prepolymer III.

[0020] Preferably, the polycarbonate diol in step S1 has a molecular weight of 2000 g / mol and a hydroxyl value of 55-57 mg KOH / g.

[0021] Preferably, the heating temperature in step S1 is 90°C to 105°C, more preferably 95°C to 98°C; the reaction time is 0.5h-2h, more preferably 1h; the reaction temperature is controlled at 75°C to 90°C, more preferably 80°C to 85°C; the reaction time is 0.5h-2h, more preferably 1h.

[0022] Preferably, the polymerization inhibitor in step S2 is one of p-hydroxyanisole and hydroquinone, more preferably p-hydroxyanisole.

[0023] Preferably, the insulation conditions in step S2 are 50°C to 85°C, more preferably 50°C to 55°C; the reaction time is 0.5h-2h, more preferably 1h; the reaction temperature is controlled at 55°C to 85°C, more preferably 60°C to 65°C; the reaction time is 1h-2.5h, more preferably 2h.

[0024] Preferably, the heating condition in step S3 is 50°C to 65°C, more preferably 60°C to 65°C; the reaction time is 0.5h-1.5h, more preferably 1h.

[0025] Preferably, the solvent in step S3 is acetone, and the amount of acetone added is 10.0-15.0% of the solid content by mass; and the amount of water added is 3 times the solid content by mass.

[0026] The present invention also provides the use of the self-initiating cationic electrophoretic polyurethane acrylate resin in the preparation of electrophoretic coatings. During use, no photoinitiator needs to be added, thereby fundamentally solving the problem of photoinitiator migration.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] (1) The present invention modifies the photoinitiator 2959 to produce a photoactive chain extender containing two active secondary amine groups, which can complete a chain extension reaction with an isocyanate group, graft the initiator active group onto the middle chain segment of the waterborne polyurethane acrylate macromolecule, and fix it in the cured macromolecular network. There is no small molecule photoinitiator, which fundamentally solves the problem of photoinitiator migration.

[0029] (2) The self-initiating cationic electrophoretic polyurethane acrylate resin prepared by the present invention has good mechanical stability and does not require the addition of a photoinitiator during the use of electrophoretic coatings.

[0030] (3) The self-initiating cationic electrophoretic polyurethane acrylate resin prepared by the present invention is used in coatings. After impact testing, the paint film does not show cracking or falling off, indicating that the self-initiating cationic electrophoretic polyurethane acrylate resin cured film prepared by the present invention has good impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a picture of the appearance of the self-initiated cationic electrophoretic polyurethane acrylate resin prepared in an embodiment of the present invention.

[0032] Figure 2 This is a picture of the impact resistance test of the self-initiated cationic electrophoretic polyurethane acrylate resin electroplating paint film prepared in an embodiment of the present invention.

[0033] Figure 3 This is a graph showing the UV-visible light absorption curve of the immersion solution for the self-initiated cationic electrophoretic polyurethane acrylate resin electroplating curing film prepared in an embodiment of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with specific embodiments, but the scope of the present invention is not limited. It should be understood that, for those of ordinary skill in the art, improvements or changes can be made according to the above description, and all these improvements and changes should belong to the protection scope of the appended claims of the present invention.

[0035] If the specific conditions are not specified in the examples, the preparation is carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased from the market.

[0036] The specific synthesis method of the photoactive chain extender E-2959 used in all embodiments of the present invention is as follows:

[0037] Dissolve the photoinitiator 2959 in acetone of 4 times its mass, then drop ethyl isocyanate acrylate and photoinitiator 2959 in a molar ratio of 1:1 into the acetone solvent of 2959, and react at 40℃~42℃ for 2h. Then add ethylenediamine of 0.5 times the molar number of ethyl isocyanate acrylate to the above reaction system (reaction system of ethyl isocyanate acrylate and photoinitiator 2959), and react at 55℃~60℃ for 2h to obtain active chain extender E-2959.

[0038] The synthetic route of photoactive chain extender E-2959 is as follows:

[0039]

[0040] Example 1

[0041] A self-initiating cationic electrophoretic polyurethane acrylate resin comprises the following components in parts by weight:

[0042]

[0043] The self-initiating cationic electrophoretic polyurethane acrylate resin is prepared by a method comprising the following steps:

[0044] (1) 43.49 parts by weight of isophorone diisocyanate and 30.96 parts by weight of polycarbonate diol (PCD-621) (Mn=2000 g / mol, hydroxyl value 55-57 mg KOH / g) were added to a four-necked flask equipped with a mechanical stirrer, and the temperature was raised to 95° C. and reacted for 1 hour; then 4.34 parts by weight of N-methyldiethanolamine and 4.94 parts by weight of 1,4-butanediol (BDO) were added dropwise thereto, and the reaction temperature was controlled at 80° C. After reacting for 1 hour, a prepolymer I was obtained;

[0045] (2) adding 4.22 parts by weight of a photoactive chain extender E-2959 to prepolymer I, and reacting at 55° C. for 1 hour; then adding 9.76 parts by weight of hydroxyethyl acrylate and a polymerization inhibitor having a solid content of 0.08% by weight of p-hydroxyanisole, and reacting at 60° C. for 2 hours to obtain prepolymer II;

[0046] (3) At 60° C., under mechanical stirring conditions, 2.18 parts by weight of acetic acid was added to prepolymer II, and the mixture was kept warm for reaction for 1 hour. After the heat preservation was completed, prepolymer III was obtained. During the entire reaction process, acetone with a solid content of 10.0% was used to adjust the viscosity of the reaction system. Then, prepolymer III was added to deionized water in an amount 3 times its mass, stirred at high speed for 20 minutes, and then the acetone solvent was removed by reduced pressure distillation to obtain a self-initiating cationic electrophoretic polyurethane acrylate resin.

[0047] Example 2

[0048] A self-initiating cationic electrophoretic polyurethane acrylate resin comprises the following components in parts by weight:

[0049]

[0050] The self-initiating cationic electrophoretic polyurethane acrylate resin is prepared by a method comprising the following steps:

[0051] (1) Add 42.72 parts by weight of isophorone diisocyanate and 30.35 parts by weight of polycarbonate diol (PCD-621) into a four-necked flask equipped with a mechanical stirrer, heat to 98° C., and react for 1 hour; then dropwise add 4.32 parts by weight of N-methyldiethanolamine and 4.54 parts by weight of 1,4-butanediol (BDO), control the reaction temperature at 85° C., and react for 1 hour to obtain prepolymer I;

[0052] (2) adding 6.33 parts by weight of a photoactive chain extender E-2959 to prepolymer I, and reacting at 50° C. for 1 hour; then adding 9.56 parts by weight of hydroxyethyl acrylate and a polymerization inhibitor having a solid content of 0.10% by weight of p-hydroxyanisole, and reacting at 65° C. for 2 hours to obtain prepolymer II;

[0053] (3) At 65° C., under mechanical stirring conditions, 2.18 parts by weight of acetic acid was added to prepolymer II, and the mixture was kept warm for reaction for 1 hour. After the heat preservation was completed, prepolymer III was obtained. During the entire reaction process, acetone with a solid content of 15.0% was used to adjust the viscosity of the reaction system. Then, prepolymer III was added to deionized water in an amount 3 times its mass, stirred at high speed for 20 minutes, and then the acetone solvent was removed by reduced pressure distillation to obtain a self-initiating cationic electrophoretic polyurethane acrylate resin.

[0054] Example 3

[0055] A self-initiating cationic electrophoretic polyurethane acrylate resin comprises the following components in parts by weight:

[0056]

[0057] The self-initiating cationic electrophoretic polyurethane acrylate resin is prepared by a method comprising the following steps:

[0058] (1) Add 41.87 parts by weight of isophorone diisocyanate and 29.74 parts by weight of polycarbonate diol (PCD-621) into a four-necked flask equipped with a mechanical stirrer, heat to 96° C., and react for 1 hour; then dropwise add 4.31 parts by weight of N-methyldiethanolamine and 4.14 parts by weight of 1,4-butanediol (BDO), control the reaction temperature at 82° C., and react for 1 hour to obtain prepolymer I;

[0059] (2) adding 8.40 parts by weight of a photoactive chain extender E-2959 to prepolymer I, and reacting at 52° C. for 1 h; then adding 9.37 parts by weight of hydroxyethyl acrylate and a polymerization inhibitor having a solid content of 0.07% by weight of p-hydroxyanisole, and reacting at 63° C. for 2 h to obtain prepolymer II;

[0060] (3) At 64° C., 2.17 parts by weight of acetic acid was added to prepolymer II under mechanical stirring, and the mixture was kept warm for reaction for 1 hour. After the heat preservation was completed, prepolymer III was obtained. During the entire reaction process, acetone with a solid content of 12.0% was used to adjust the viscosity of the reaction system. Then, prepolymer III was added to deionized water in an amount 3 times its mass, stirred at high speed for 20 minutes, and then the acetone solvent was removed by reduced pressure distillation to obtain a self-initiating cationic electrophoretic polyurethane acrylate resin.

[0061] Example 4

[0062] A self-initiating cationic electrophoretic polyurethane acrylate resin comprises the following components in parts by weight:

[0063]

[0064] The self-initiating cationic electrophoretic polyurethane acrylate resin is prepared by a method comprising the following steps:

[0065] (1) Add 41.02 parts by weight of isophorone diisocyanate and 29.13 parts by weight of polycarbonate diol (PCD-621) into a four-necked flask equipped with a mechanical stirrer, heat to 97° C., and react for 1 hour; then dropwise add 4.29 parts by weight of N-methyldiethanolamine and 3.75 parts by weight of 1,4-butanediol (BDO), control the reaction temperature at 83° C., and react for 1 hour to obtain prepolymer I;

[0066] (2) adding 10.46 parts by weight of a photoactive chain extender E-2959 to prepolymer I, and reacting at 53° C. for 1 hour; then adding 9.18 parts by weight of hydroxyethyl acrylate and a polymerization inhibitor having a solid content of 0.09% by weight of p-hydroxyanisole, and reacting at 63° C. for 2 hours to obtain prepolymer II;

[0067] (3) At 64° C., under mechanical stirring, 2.16 parts by weight of acetic acid was added to prepolymer II, and the mixture was kept warm for reaction for 1 hour. After the heat preservation, prepolymer III was obtained. During the whole reaction process, acetone with a solid content of 14.0% was used to adjust the viscosity of the reaction system. Then, prepolymer III was added to deionized water in an amount 3 times its mass, stirred at high speed for 20 minutes, and then the acetone solvent was removed by reduced pressure distillation to obtain a self-initiating cationic electrophoretic polyurethane acrylate resin.

[0068] Experimental Example 1

[0069] The self-initiating cationic electrophoretic polyurethane acrylate resin prepared in Example 1, Example 2, Example 3, and Example 4 was electroplated on a tinplate sheet using an electrophoresis apparatus. After the electroplating was completed, it was then baked in an oven at 60° C. for 2 minutes to remove moisture, and finally cured using a mercury lamp.

[0070] The viscosity, solid content and hardness were tested according to the national standards GB / T15357-2014, GB / T 1725-2007 and GB / T 6739-2006. The results are shown in Table 1.

[0071] The stability of the resin is tested by centrifuging. The resin is placed in a centrifuge tube and centrifuged at 3000n / min for 30 minutes to observe whether the resin in the centrifuge tube is stratified or whether there is precipitation at the bottom. After centrifugation, if the resin in the centrifuge tube is stratified or precipitation appears at the bottom, it means that the mechanical stability of the resin is poor. Figure 1 These are appearance pictures of the self-initiating cationic electrophoretic polyurethane acrylate resins prepared in Examples 1, 2, 3, and 4.

[0072] Table 1

[0073]

[0074] It can be seen from the test results that the self-initiating cationic electrophoretic polyurethane acrylate resin prepared by the present invention has good mechanical stability and does not require the addition of a photoinitiator during use.

[0075] Experimental Example 2

[0076] The self-initiating cationic electrophoretic polyurethane acrylate resin prepared in Example 1, Example 2, Example 3, and Example 4 was electroplated onto a tinplate sheet, the moisture was removed and the photocuring was performed, and then the impact resistance test was performed. The test method was carried out according to the paint film impact resistance test GB / T 1732-2020. The paint film impact resistance test results are as follows: Figure 2 shown.

[0077] It can be seen from the test results that after the impact test, the paint film did not crack or fall off, indicating that the self-initiated cationic electrophoretic polyurethane acrylate resin cured film prepared by the present invention has good impact resistance.

[0078] Experimental Example 3

[0079] The self-initiating cationic electrophoretic polyurethane acrylate resin prepared in Example 1, Example 2, Example 3, and Example 4 was electroplated onto a tinplate sheet, and the water was removed and light-cured. The film of the cured film was scraped off with a blade, and 0.5 g of each was taken and soaked in 20 mL of ethanol. After soaking for 3 days, the ultraviolet-visible light absorption of the soaking solution was tested. The ultraviolet-visible light absorption results of the soaking solution are shown in FIG. Figure 3 shown.

[0080] From the test results, we can see that after the cured film is immersed for 3 days, it has only weak ultraviolet visible light absorption, indicating that the macromolecules containing photosensitive groups in the cured film have low mobility.

[0081] The above embodiments of the present invention are merely examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A self-initiating cationic electrophoretic polyurethane acrylate resin material, characterized in that: The invention comprises the following components in parts by weight: 41.02 to 44.54 parts of isophorone diisocyanate, 29.13 to 31.57 parts of polycarbonate diol, 4.29 to 4.36 parts of N-methyldiethanolamine, 3.75 to 5.34 parts of 1,4-butanediol, 2.13 to 10.46 parts of E-2959 photoactive chain extender, 9.18 to 9.95 parts of hydroxyethyl acrylate, 2.16 to 2.20 parts of acetic acid, and a polymerization inhibitor; wherein the polymerization inhibitor is 0.05% to 0.10% of the solid content; The structural formula of the photoactive chain extender E-2959 is 2. The self-initiating cationic electrophoretic polyurethane acrylate resin material according to claim 1, characterized in that: The self-initiating cationic electrophoretic polyurethane acrylate resin has a structure as shown in formula (I): in 3. The method for preparing a self-initiating cationic electrophoretic polyurethane acrylate resin material according to claim 1 or 2, characterized in that: The steps include: S1, heating isophorone diisocyanate and polycarbonate diol to react; then dropping N-methyldiethanolamine and 1,4-butanediol thereinto, controlling the reaction temperature, and obtaining prepolymer I after the reaction; S2, adding photoactive chain extender E-2959 to the prepolymer I obtained in step S1, and reacting under heat preservation conditions; then adding hydroxyethyl acrylate and a polymerization inhibitor, controlling the reaction temperature, and reacting to obtain prepolymer II; S3. Under heating and stirring conditions, acetic acid is added to the prepolymer II obtained in step S2, and the prepolymer III is obtained after heat preservation reaction. During the reaction process, a solvent is used to adjust the viscosity of the reaction system, and then the prepolymer III is added to water and stirred, and the solvent is removed to obtain the prepolymer III.

4. The preparation method according to claim 3, characterized in that: The polycarbonate diol in step S1 has a molecular weight Mn of 2000 g / mol and a hydroxyl value of 55-57 mg KOH / g.

5. The preparation method according to claim 3, characterized in that: In step S1, the heating reaction temperature is 90°C to 105°C, and the reaction time is 0.5h to 2h; the reaction temperature is controlled at 75°C to 90°C, and the reaction time is 0.5h to 2h.

6. The preparation method according to claim 3, characterized in that: The inhibitor in step S2 is one of p-hydroxyanisole and hydroquinone.

7. The preparation method according to claim 3, characterized in that: The insulation condition in step S2 is 50°C to 85°C, and the reaction time is 0.5h to 2h; the reaction temperature is controlled at 55°C to 85°C, and the reaction time is 1h to 2.5h.

8. The preparation method according to claim 3, characterized in that: The heating and stirring conditions in step S3 refer to a temperature of 50° C. to 65° C. and a reaction time of 0.5 h to 1.5 h.

9. The preparation method according to claim 3, characterized in that: In step S3, the solvent is acetone, and the amount of acetone added is 10.0-15.0% of the solid content; the amount of water added to the water for stirring the prepolymer III is 3 times the solid content.

10. Use of the self-initiating cationic electrophoretic polyurethane acrylate resin material according to claim 1 in the preparation of electrophoretic coatings.

Citation Information

Patent Citations

  • Light-sensitive self-initiated polyurethane acrylic ester oligomer and method for synthesizing the same

    CN101481450A

  • Self-cross-linking waterborne light-curing polyurethane, preparation method and applications thereof

    CN110835397A

  • Waterborne cationic-type urethane acrylate vacuum film-plating metallic paint

    CN106978066A

  • Double-curing urethane acrylate resin and preparation method thereof

    CN108456290A

  • Self-photoinitiating water-dispersible acrylate ionomers and synthetic methods

    US20050245711A1