Method for carbon sequestration using solid waste
By grinding and chemically activating the solid waste, a polymer sol is formed to reduce the carbonization reaction energy, which solves the problem of high carbon solid waste energy consumption and achieves a more efficient carbon solidification effect and cost reduction.
Patent Information
- Application Number
- CN202311019964.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-08-14
AI Technical Summary
The existing technologies that utilize solid waste to fix carbon are high in energy consumption and can achieve less carbon sequestration.
By grinding the solid waste and adding chemical activator, the slurry is formed and activated, dried and autoclaved carbonated, the crystal lattice structure in the solid waste is destroyed and a polymer sol is formed to reduce the energy required for the carbonation reaction.
Improve carbon sequestration capacity under the same energy consumption, reduce the energy consumption and cost of the carbon sequestration process, and achieve lower energy consumption and cost. The simple process has industrial promotion value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy, and in particular to a method for carbon fixation using solid waste. Background Art
[0002] As an industrial power, my country is rich in various industrial solid wastes and mineral mining tailings. Carbonation and fixation of solid wastes and minerals is an important way to reduce CO2 emissions. As mineralization raw materials, they have a wide source, large solidification capacity, stable products, and can realize the resource utilization of carbon fixation products, improving the safety and economy of CO2 storage technology.
[0003] However, the current technology for carbon fixation using solid waste has high energy consumption and can achieve a relatively small amount of carbon fixation. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a carbon fixation method using solid waste, aiming to solve the problem that the current technology of carbon fixation using solid waste can only achieve a relatively small amount of carbon fixation.
[0005] To achieve the above-mentioned purpose, the present invention proposes a carbon fixation reagent, comprising the following steps: grinding solid waste, adding a chemical activator to the ground solid waste, and then adding water to obtain a slurry; after the slurry is activated, dried, and autoclaved and carbonated, carbon fixation is completed.
[0006] Optionally, the fineness of the ground solid waste is ≥200 mesh.
[0007] Optionally, the chemical activator comprises caustic and / or a weak base that can generate caustic during the activation.
[0008] Optionally, the weight ratio of the ground solid waste to the chemical activator is (2-10):0.3.
[0009] Optionally, the activation temperature is 50°C to 80°C.
[0010] Optionally, the concentration of carbon dioxide in the autoclaved carbonation is >60%.
[0011] Optionally, the temperature of the autoclave carbonation is 140°C to 200°C.
[0012] Optionally, the pressure of the autoclaved carbonation is 8 bar to 12 bar.
[0013] Optionally, the solid waste includes industrial and mining solid waste.
[0014] Optionally, the industrial and mining solid waste includes at least one of blast furnace slag, steel slag, pyrite cinder, fly ash, coal gangue, tailings, and hot molten slag.
[0015] Beneficial effects of the present invention: The method for carbon fixation using solid waste provided by the present invention increases the specific surface area of the solid waste by grinding, and then destroys the lattice in the solid waste by a chemical activator to reorganize it, thereby weakening the stable crystal structure formed by the solid waste material after smelting and cooling. The amorphous solid waste compounds in the slurry gradually react and dissolve under the erosion of the chemical activator to form a polymer sol. The crystal structure of this polymer sol is weaker than the crystal structure before activation, so the energy required for its carbonation reaction is lower. Therefore, the present invention reduces the energy consumption required for carbon fixation using solid waste, and can improve the ability to fix carbon on solid waste materials under the premise of the same energy consumption, so as to achieve lower energy consumption and cost in the carbon fixation process. The process is simple and has great industrial promotion value. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0017] Unless defined otherwise, all technical and scientific terms used herein have the common meaning in the art to which the claimed subject matter belongs.
[0018] As an industrial power, my country is rich in various industrial solid wastes and mineral mining tailings. Carbonation and fixation of solid wastes and minerals is an important way to reduce CO2 emissions. As mineralization raw materials, they have a wide source, large solidification capacity, stable products, and can realize the resource utilization of carbon fixation products, improving the safety and economy of CO2 storage technology.
[0019] However, the current technology for carbon fixation using solid waste has high energy consumption and can achieve a relatively small amount of carbon fixation.
[0020] In order to solve the above problems, the present invention provides a carbon fixation reagent, comprising the following steps:
[0021] S1: grinding the solid waste, adding a chemical activator to the ground solid waste, and then adding water to obtain a slurry;
[0022] After smelting and cooling, the compounds in the solid waste materials will form a relatively stable crystal structure. Grinding is an important way to deeply stimulate the activity of solid waste. Grinding solid waste can increase the specific surface area of solid waste materials, thereby increasing the activation reaction area. Adding chemical activators can destroy the crystal lattice in the solid waste and reorganize it, thereby achieving the purpose of weakening the crystal structure. Adding water to make pulp provides the necessary solution environment for the activation reaction.
[0023] S2: The slurry is activated, dried, and carbonated by autoclaving to complete carbon fixation.
[0024] The amorphous solid waste compounds in the slurry gradually react and dissolve under the erosion of the chemical activator to form a polymer sol. The crystal structure of the polymer sol is weaker than the crystal structure before activation, so the energy required for its carbonation reaction is lower. Therefore, the present invention reduces the energy consumption required for carbon fixation using solid waste, and can improve the carbon fixation capacity of solid waste materials under the premise of the same energy consumption, so as to achieve lower energy consumption and cost in the carbon fixation process.
[0025] Furthermore, the fineness of the ground solid waste is ≥200 mesh. In one embodiment, a steam mill is used for grinding to utilize the supersonic steam flow formed by superheated steam to drive the self-collision of the material, and the powerful kinetic energy of the supersonic steam flow is utilized to achieve efficient crushing. In another embodiment, an ultrafine ball mill is used for grinding. Steam milling and ultrafine ball milling classification are cutting-edge advanced and low-cost technologies for achieving ultrafine pulverization of solid waste. Combined with the principle of synergistic excitation of multiple solid wastes, the further utilization of solid waste can be optimized.
[0026] Further, the chemical activator includes caustic alkali and / or a weak base that can generate caustic alkali during the activation. In some embodiments, the chemical activator includes at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, and sodium sulfate. Preferably, the chemical activator is sodium hydroxide, or a mixture of sodium sulfate, calcium hydroxide and sodium hydroxide.
[0027] Furthermore, the weight ratio of the ground solid waste to the chemical activator is (2-10):0.3. Within this weight ratio range, it is beneficial to form [Si(OH)4] - Monomer and [Al(OH)4] - monomer, then [Si(OH)4] - The monomers undergo condensation reaction to form a ring-shaped polymer sol.
[0028] Furthermore, the activation temperature is 50°C to 80°C. Carrying out the activation reaction within this temperature range not only ensures that the reaction has a large activation energy, but also avoids the destruction of the reaction by excess heat during the electronic cascade between the reactant molecules when the temperature is too high, thereby preventing the reaction from being hindered. In some embodiments, the activation temperature is 55°C, 60°C, 65°C, 70°C or 75°C. In some embodiments, the activation time is 12h to 48h.
[0029] Further, the concentration of carbon dioxide in the autoclaved carbonation is >60%. Carbon dioxide concentration promotes the carbonation reaction to proceed in a positive direction. Under normal conditions, the concentration of carbon dioxide in the carbonation reaction needs to be >90%, but in this solution, only >60% can achieve a good promotion effect. In some embodiments, the carbon dioxide concentration is 65%, 70%, 75%, 80%, 85%, 90% or 95%.
[0030] Furthermore, the temperature of the autoclaved carbonation is 140°C to 200°C. Within this temperature range, carbon dioxide dissolves in water to form carbonic acid, which can quickly react with the activated calcium magnesium silicate to produce more stable calcium magnesium carbonate and achieve carbon fixation. In some embodiments, the temperature of the autoclaved carbonation is 150°C, 160°C, 170°C, 180°C or 190°C.
[0031] Furthermore, the pressure of the autoclaved carbonation is 8 bar to 12 bar. Expanding the gas-liquid two-phase contact area and increasing the carbon dioxide pressure are beneficial to the carbonation process. Within this pressure range, the reaction system can achieve excellent carbon fixation effect by synergizing with the activated solid waste.
[0032] Furthermore, the solid waste includes industrial and mining solid waste. In some embodiments, the industrial and mining solid waste includes calcium silicate solid waste. After smelting and cooling, the silicate phase in the solid waste material will form a relatively stable crystal structure, so carbon fixation is more difficult.
[0033] Furthermore, the industrial and mining solid waste includes at least one of blast furnace slag, steel slag, pyrite cinder, fly ash, coal gangue, tailings, and hot molten slag. Preferably, since the mineralization reaction of calcium silicate substances requires lower temperature and pressure, the carbon fixation method of this scheme is more advantageous in treating solid waste whose main component is calcium silicate.
[0034] Embodiment 1:
[0035] In parts by weight, 97 parts of steel slag solid waste were ground to a fineness of 300 meshes, 3 parts of sodium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0036] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0037] Embodiment 2:
[0038] In parts by weight, 96 parts of steel slag solid waste were ground to a fineness of 300 meshes, 4 parts of potassium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0039] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0040] Embodiment 3:
[0041] In parts by weight, 91 parts of steel slag solid waste were ground to a fineness of 300 meshes, 6 parts of sodium sulfate and 3 parts of calcium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0042] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0043] Embodiment 4:
[0044] In parts by weight, 94 parts of steel slag solid waste were ground to a fineness of 300 meshes, 5 parts of sodium sulfate and 1 part of sodium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0045] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0046] Embodiment 5:
[0047] In parts by weight, 91 parts of steel slag solid waste were ground to a fineness of 300 meshes, 6 parts of sodium sulfate, 3 parts of calcium hydroxide and 1 part of sodium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0048] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0049] Embodiment 6:
[0050] In parts by weight, 97 parts of steel slag solid waste were ground to a fineness of 200 meshes, 3 parts of sodium hydroxide were added to the ground solid waste, and then water was added to obtain a slurry;
[0051] The slurry is activated at 60° C. for 24 hours and then dried. It is then subjected to autoclave carbonation at 10 bar and 150° C., with the concentration of carbon dioxide during autoclave carbonation being 85%, thereby completing carbon fixation.
[0052] Comparative Example 1:
[0053] The same as Example 1, except that the steel slag solid waste is not activated.
[0054] Furthermore, the carbon fixation amount of Examples 1-6 and Comparative Example 1 was measured, and the test results were summarized in Table 1.
[0055] Table 1. Carbon fixation amount of Examples 1-6 and Comparative Example 1
[0056]
[0057] Through the above carbon fixation measurement experiment, the results of Examples 1-6 are compared with Comparative Example 1. It can be seen that the activation process and the use of activators can significantly increase the final carbon fixation of the same type of solid waste under the same mineralization conditions. Further comparing the carbon fixation results of Examples 1-5, the types of activators have different effects on the degree of improvement in the final carbon fixation within the same activation time. Therefore, the type and dosage of the activator can be optimized according to the raw material prices and related solid waste conditions in different regions. The only difference between Example 6 and Example 1 is the fineness of the solid waste grinding. It can be intuitively seen that the fineness of solid waste treatment has a certain influence on the carbon fixation effect. The finer the fineness, the higher the degree of mineralization reaction.
[0058] The method for carbon fixation using solid waste provided by the present invention increases the specific surface area of the solid waste by grinding, and then destroys the lattice in the solid waste by a chemical activator to reorganize it, thereby weakening the stable crystal structure formed by the solid waste material after smelting and cooling. The amorphous solid waste compounds in the slurry gradually react and dissolve under the erosion of the chemical activator to form a polymer sol. The crystal structure of this polymer sol is weaker than the crystal structure before activation, so the energy required for its carbonation reaction is lower. Therefore, the present invention reduces the energy consumption required for carbon fixation using solid waste, and can improve the ability to fix carbon on solid waste materials under the premise of the same energy consumption, so as to achieve lower energy consumption and cost in the carbon fixation process. The process is simple and has great industrial promotion value.
[0059] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for carbon fixation using solid waste, characterized in that: The following steps are involved: grinding the solid waste, adding a chemical activator to the ground solid waste, and then adding water to obtain a slurry; The slurry is activated, dried, and autoclaved to achieve carbon fixation; The fineness of the ground solid waste is ≥ 200 mesh; The weight ratio of the ground solid waste to the chemical activator is (2-10):0.3; The concentration of carbon dioxide in the autoclaved carbonation is >60%; The temperature of the autoclaved carbonation is 140°C to 200°C; The pressure of the autoclaved carbonation is 8 bar to 12 bar.
2. The method for carbon fixation using solid waste according to claim 1, characterized in that: The chemical activator includes caustic and / or a weak base that can generate caustic during the activation.
3. The method for carbon fixation using solid waste according to claim 1, characterized in that: The activation temperature is 50°C to 80°C.
4. The method for carbon fixation using solid waste according to claim 1, characterized in that: The solid waste includes industrial and mining solid waste.
5. The method for carbon fixation using solid waste according to claim 4, characterized in that: The industrial and mining solid waste includes at least one of blast furnace slag, steel slag, pyrite cinder, fly ash, coal gangue, tailings, and hot molten slag.