A three-sided corner welding method and a rail vehicle corner weld welding method
By adopting a specific welding method at the corners of the three sides of the aluminum alloy, the weld joints are located in the straight seam section, which solves the problem of concentrated welding defects, improves welding quality and vehicle safety, and achieves a more efficient welding process.
Patent Information
- Application Number
- CN202311296917.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-08
AI Technical Summary
The existing welding methods at the three-sided corners of aluminum alloy are prone to cause welding defects such as unfused, unwelded, and cracks at the corners, resulting in concentrated welding defects and increasing safety hazards for rail vehicle operation.
A three-sided corner welding method is adopted to make the only weld joint located in the linear weld section. By fixing the components to be welded, three planes are formed perpendicular to each other, spot welding and welding at the corners, using arc starting and arc closing currents Weld separately to ensure that the welds are connected to the outside of the corners and avoid defect aggregation.
It improves welding quality, reduces the incidence of welding defects at corners, enhances the overall strength and operational safety of the vehicle, and improves welding efficiency.
Smart Images

Figure CN117161511B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of equipment corner welding, in particular to a three-sided corner welding method and a rail vehicle corner weld welding method. Background Art
[0002] At present, most of the rail train bodies such as high-speed EMUs, subway vehicles, and urban rail vehicles are welded from aluminum alloy plates and profiles. Corner welding is often involved in the welding process, and the welding quality of each weld directly affects the strength of the entire vehicle and the safety of train operation. The setting of welding parameters and welding methods will affect the welding effect. Defects in the welding process will have a direct impact on the strength of the components after welding, and then affect the strength of the rail vehicle body.
[0003] The existing welding method for three-sided corners of aluminum alloy usually welds each welding gap one by one, and often the arc ending and arc starting are placed at the corner. This easily leads to welding defects such as lack of fusion, lack of penetration, and cracks at the corner. Welding defects are concentrated at the corners, further increasing the probability of welding defects, which bury hidden dangers for vehicle operation safety. Summary of the invention
[0004] The purpose of the present invention is to provide a three-sided corner welding method and a rail vehicle corner weld welding method to solve the problems existing in the prior art, so that the only weld joint is located in a straight weld section, thereby avoiding welding defects from gathering at the corners, improving welding quality and reducing safety hazards.
[0005] To achieve the above object, the present invention provides the following solution: The present invention provides a three-sided corner welding method, comprising the following steps:
[0006] 1) Fix the components to be welded to obtain three mutually perpendicular planes, form a welding gap between two adjacent planes, and the three mutually perpendicular welding gaps intersect at a corner point;
[0007] 2) Spot weld the three welding gaps respectively to fix the components to be welded;
[0008] 3) Weld from the outer end of the first welding gap toward the corner, stop welding when the distance from the corner is 15mm to 10mm, and obtain the first weld;
[0009] 4) welding is performed from the outer end of the second welding gap toward the corner, and the welding gun is swung from the corner along the plane where the first weld and the second weld are located to connect the weld at the corner with the first weld to obtain a second weld;
[0010] 5) After the corner welding is completed, welding is continued from the corner toward the outer end of the third welding gap without stopping the machine to obtain the third weld.
[0011] Preferably, among the three planes, the first plane is arranged horizontally, the second plane and the third plane are arranged vertically on the first plane, and the second plane and the third plane intersect vertically; there is a first welding gap between the first plane and the second plane, there is a second welding gap between the first plane and the third plane, and there is a third welding gap between the second plane and the third plane.
[0012] Preferably, the first welding gap is welded using the arc starting current; the second welding gap and the corner weld are welded using the arc starting current, and the connection with the first weld is completed; the third welding gap is welded from bottom to top using the welding current, and after the welding is completed, the arc pit is filled using the arc ending current; the arc starting current is 110% to 125% of the welding current, and the arc ending current is 50% to 60% of the welding current.
[0013] Preferably, in step 3), the arc ending point of the first weld is ground into a slope shape with the slope facing the corner.
[0014] The present invention also provides a rail vehicle corner weld welding method, comprising the following steps:
[0015] 1) Fix the base frame; vertically place the side wall and the end wall on the base frame for fixing, and the end wall is perpendicular to the side wall; there is a first welding gap between the base frame and the end wall, a second welding gap between the base frame and the side wall, and a third welding gap between the side wall and the end wall;
[0016] 2) The first welding gap, the second welding gap and the third welding gap are welded using the above-mentioned three-sided corner welding method.
[0017] Preferably, when welding the third welding gap, a sawtooth swing welding process is adopted.
[0018] Preferably, before welding, the first welding gap, the second welding gap and the third welding gap are adjusted so that the first welding gap, the second welding gap and the third welding gap are all no larger than 1 mm.
[0019] Preferably, before welding, the oxide film and oil stains on the surface of the welding area are cleaned.
[0020] Compared with the prior art, the present invention has achieved the following technical effects:
[0021] In the present invention, there is a certain interval between the end of the first weld and the corner. When welding the second weld, the second weld is connected to the end of the first weld by a swinging welding gun, and the operation of the third weld is completed without stopping the machine, so that the only welding joint is located outside the corner, and the joint quality at the straight weld is easier to ensure, thereby making the overall welding quality higher, and avoiding the technical problem in the prior art that arc closing and arc starting are placed at the corner, so that welding defects are concentrated at the corner, which poses a safety hazard; and the second weld and the third weld are welded without stopping the machine, which can improve the welding efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 It is a schematic diagram of the matching structure of the base frame, end wall and side wall in the present invention;
[0024] Figure 2 It is a schematic diagram of the weld at the corner;
[0025] Among them, 1. base frame; 2. end wall; 3. side wall; 4. first weld; 5. second weld; 6. third weld. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The purpose of the present invention is to provide a three-sided corner welding method and a rail vehicle corner weld welding method to solve the problems existing in the prior art, so that the only weld joint is located in a straight weld section, thereby avoiding welding defects from gathering at the corners, improving welding quality and reducing safety hazards.
[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] Embodiment 1:
[0030] like Figure 2As shown, this embodiment provides a three-sided corner welding method, comprising the following steps:
[0031] 1) Fix the components to be welded to obtain three mutually perpendicular planes, form a welding gap between two adjacent planes, and the three mutually perpendicular welding gaps intersect at a corner point;
[0032] 2) Spot weld the three welding gaps respectively to fix the components to be welded;
[0033] 3) Welding is performed from the outer end of the first welding gap toward the corner, and welding is stopped when the distance from the corner is 15 mm to 10 mm, thereby obtaining the first weld 4;
[0034] 4) Welding is performed from the outer end of the second welding gap toward the corner, and the welding gun is swung from the corner along the plane where the first weld 4 and the second weld 5 are located to connect the weld at the corner with the first weld 4 to obtain the second weld 5;
[0035] 5) After the corner welding is completed, welding is continued from the corner toward the outer end of the third welding gap without stopping the machine to obtain the third weld 6.
[0036] In this embodiment, there is a certain interval between the end of the first weld 4 and the corner. When the second weld 5 is welded, the second weld 5 is connected to the end of the first weld 4 by a swinging welding gun, and the operation of the third weld 6 is completed without stopping the machine, so that the only welding joint is located outside the corner, and the joint quality at the straight weld is easier to ensure, thereby making the overall welding quality higher, and avoiding the technical problem in the prior art that arc closing and arc starting are placed at the corner, so that welding defects are concentrated at the corner, which poses a safety hazard; and the second weld 5 and the third weld 6 do not stop during welding, which can improve the welding efficiency.
[0037] In order to facilitate the connection between the second weld 5 and the first weld 4 and improve the welding quality at the connection position, in step 3), the arc closing point of the first weld 4 is ground into a slope shape with the slope facing the corner.
[0038] Furthermore, among the three planes in this embodiment, the first plane is horizontally arranged, the second plane and the third plane are both vertically arranged on the first plane, and the second plane and the third plane intersect vertically; there is a first welding gap between the first plane and the second plane, there is a second welding gap between the first plane and the third plane, and there is a third welding gap between the second plane and the third plane.
[0039] Furthermore, before welding, the welding is adjusted to a three-stage current form, wherein the three stages are arc starting current, welding current and arc ending current. The arc starting current is used to weld the first welding gap; the arc starting current is used to weld the second welding gap and the corner weld, and the connection with the first weld 4 is completed; the welding current is used to weld the third welding gap from bottom to top, and after welding is completed, the arc ending current is used to fill the arc ending pit; the arc starting current is 110% to 125% of the welding current, and the arc ending current is 50% to 60% of the welding current.
[0040] Embodiment 2:
[0041] Based on the three-sided corner welding method in Example 1, this embodiment provides a rail vehicle corner weld welding method, such as Figure 1-2 As shown, the following steps are included:
[0042] 1. Assembly steps:
[0043] (1) Lift the base frame 1 into the tooling, adjust the base frame 1 to the deflection state required by the drawing, and fix it with a clamp.
[0044] (2) Remove the oxide film, oil stains and other impurities on the surface of the welding area on the chassis 1, and grind the weld according to the weld form required by the drawing.
[0045] (3) Hang the side wall 3 on the side of the base frame 1, adjust the position of the side wall 3 so that the side wall 3 is perpendicular to the base frame 1 and fix it.
[0046] (4) The end wall 2 is hoisted to the end of the base frame 1 so that the end wall 2 is perpendicular to the base frame 1 and the side wall 3 at the same time, and the position of the end wall 2 is adjusted and fixed.
[0047] (5) Lift the qualified roof into the tooling, assemble the complete vehicle body, and adjust the diagonal and other related dimensions. Secure the entire vehicle.
[0048] (6) Clean the oxide film, oil stains, etc. at the joints of the base frame 1, side wall 3, end wall 2, welds, and 30 mm on both sides.
[0049] (7) Adjust the welding gap so that the gap is ≤1mm.
[0050] (8) Spot fix the workpiece and recheck the dimensions after spot fixation. Before spot fixation of the workpiece, it is necessary to measure the gap in the welding area with a steel ruler, and measure the length, height, width and symmetry inside the vehicle body with a tape measure and a laser line marker. After the position adjustment of the side wall 3 and the end wall 2 is completed, tighten the binding belt, clamps and other tools to fix them. After the tool is fixed, the weld is fixed by spot welding with a segment length of 50 mm.
[0051] 2. Welding conditions and preparation before welding:
[0052] (1) Room temperature 15℃-30℃, humidity less than 50%.
[0053] (2) Clean the oxide film, oil stains and other impurities in the welding area.
[0054] (3) Prepare the metal-metal gas shielded welding machine.
[0055] (4) The protective gas is 99.99% or 99.999% argon; the gas flow rate is adjusted to 15L / min-18L / min.
[0056] (5) Welding materials Aluminum-magnesium alloy welding wire.
[0057] (6) The dry extension length is 12mm to 15mm.
[0058] 3. Welding steps:
[0059] (1) Adjustment parameters:
[0060] ① Adjust the welding machine to three current levels, namely arc starting current, welding current and arc ending current.
[0061] ② Adjust the welding current to 130A-165A, the arc starting current to 110%-125% of the welding current, and the arc ending current to 50%-60% of the welding current.
[0062] (2) Welding of the first weld 4 between the base frame 1 and the end wall 2: Weld the first welding gap with the arc starting current and stop the arc at a distance of 10 mm from the corner.
[0063] (3) Use a straight grinder to grind the end of the first weld 4 close to the corner to form a slope shape with the broken surface facing the corner, and use a stainless steel wire brush to clean the weld to prepare for the subsequent connection of the second weld 5.
[0064] (4) The second weld 5 between the base frame 1 and the side wall 3 and the third weld 6 between the side wall 3 and the end wall 2 are welded without stopping the machine. The specific operation is as follows:
[0065] ① Use the arc starting current to weld the second weld 5 (press and hold the switch on the welding gun during welding, and the welding current is the arc starting current);
[0066] ② When welding to the corner, do not stop the machine, swing the welding gun from bottom to top and left to right to continue to form the second weld 5 layer by layer, and smoothly connect it with the first weld 4;
[0067] ③ When the corner welding is completed, start welding the third weld 6 with welding current (release the switch on the welding gun to switch to welding current); use a sawtooth swing welding technique during welding;
[0068] ⑤After welding is completed, press the switch again to switch to the arc-ending current to fill the arc-ending pit; release the switch again to extinguish the arc.
[0069] The above method can smoothly complete the welding of the welds at the corners of the vehicle body underframe 1 and the side walls 3 and the end walls 2.
[0070] Adaptive changes made according to actual needs are all within the protection scope of the present invention.
[0071] It should be noted that it is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any reference numerals in the claims should not be regarded as limiting the claims involved.
Claims
1. A three-sided corner welding method, characterized in that: The following steps are involved: 1) Fix the components to be welded to obtain three mutually perpendicular planes, and form a welding gap between two adjacent planes. The three mutually perpendicular welding gaps intersect at a corner point; 2) Spot weld the three welding gaps respectively to fix the components to be welded; 3) Weld from the outer end of the first welding gap toward the corner, stop welding when it is 15mm~10mm away from the corner, and obtain the first weld; 4) Welding is performed from the outer end of the second welding gap toward the corner, and the welding gun is swung from the corner along the plane where the first weld and the second weld are located to connect the weld at the corner with the first weld to obtain a second weld; 5) After the corner welding is completed, welding is continued from the corner toward the outer end of the third welding gap without stopping the machine to obtain the third weld; Among the three planes, the first plane is horizontally arranged, the second plane and the third plane are both vertically arranged on the first plane, and the second plane and the third plane intersect vertically; There is a first welding gap between the first plane and the second plane, there is a second welding gap between the first plane and the third plane, and there is a third welding gap between the second plane and the third plane.
2. The three-sided corner welding method according to claim 1, characterized in that: Use the starting arc current to weld the first welding gap; use the starting arc current to weld the second welding gap and the corner weld, and complete the connection with the first weld; use the welding current to weld the third welding gap from bottom to top, and after welding is completed, use the ending arc current to fill the ending arc pit; the starting arc current is 110%~125% of the welding current, and the ending arc current is 50%~60% of the welding current.
3. The three-sided corner welding method according to claim 1, characterized in that: In step 3), the arc ending point of the first weld is ground into a slope shape with the slope facing the corner.
4. A rail vehicle corner weld welding method, characterized in that: The following steps are involved: 1) Fix the base frame; vertically place the side wall and the end wall on the base frame for fixation, and the end wall is perpendicular to the side wall; there is a first welding gap between the base frame and the end wall, a second welding gap between the base frame and the side wall, and a third welding gap between the side wall and the end wall; 2) The first welding gap, the second welding gap, and the third welding gap are welded using the three-sided corner welding method according to any one of claims 1 to 3.
5. The rail vehicle corner weld welding method according to claim 4, characterized in that: When welding the third welding gap, a sawtooth swing welding process is adopted.
6. The rail vehicle corner weld welding method according to claim 4, characterized in that: Before welding, the first welding gap, the second welding gap and the third welding gap are adjusted so that the first welding gap, the second welding gap and the third welding gap are all no greater than 1 mm.