A cycloolefin dynamically cross-linked copolymer and its preparation method and use
Through random copolymerization reaction of cycloolefin intermediate compounds and primary amine crosslinking, dynamic crosslinking of cycloolefins are formed, which solves the problem of insufficient chemical resistance and structural stability of existing materials, and achieves thermal stability and ability Improve mechanical properties and support recyclable processing.
Patent Information
- Application Number
- CN202311130804.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-09-04
AI Technical Summary
There is a lack of functional polymers formed by ring-opening polymerization of cycloolefins in existing dynamic crosslinking materials, and the introduction of dynamic covalent bonds is insufficient in the chemical resistance and structural stability of the material.
Through the random copolymerization reaction of intermediate compound A and intermediate compound B, combined with Grubbs catalyst and primary amine crosslinking agent, a cycloolefin dynamic crosslinking copolymer is formed, and the vinyl amine ester dynamic bond is introduced to regulate the thermal properties of the material and Mechanical properties.
Thermal stability and chemical resistance of cycloolefin dynamic crosslinked copolymers are achieved, and the adjustable mechanical and dynamic properties are given, which extends the service life of the material and supports recyclable processing.
Smart Images

Figure CN117164453B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a cycloolefin dynamically cross-linked copolymer and a preparation method and application thereof. Background Art
[0002] Ring-opening metathesis polymerization (ROMP) is an effective method for synthesizing polymers with special structures and functions using cycloolefins. Since Ru-based catalysts have high activity in initiating ROMP reactions and the molecular weight and its distribution can be well controlled, ROMP reactions play an important role in the preparation of new functional materials with controllable properties.
[0003] Cyclic olefin dynamically cross-linked copolymer is a material obtained by introducing dynamic covalent bonds. The introduction of dynamic covalent bonds enables the cyclic olefin linear copolymer to form a dynamic cross-linked network. On the one hand, this retains the application value of the cyclic olefin copolymer in the fields of packaging, medicine and optics, and on the other hand, it gives it chemical resistance, structural stability and dynamics.
[0004] Most of the existing dynamic cross-linking materials are synthesized through small molecule condensation reactions, and there are few reports on dynamic cross-linking materials based on functional polymers formed by ring-opening polymerization of cycloolefins. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a cycloolefin copolymer and a new material with dynamic functions formed therefrom.
[0006] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.
[0007] The first aspect of the present invention provides an intermediate compound A, whose structural formula is shown in Formula I:
[0008]
[0009] The second aspect of the present invention provides a method for preparing the intermediate compound A as described above, wherein compound a and compound b are contacted to produce a ring-opening reaction, and the synthesis route is as follows:
[0010]
[0011] Preferably, the molar ratio of compound b to compound a is at least 1. More preferably, the compound b is in excess, and the molar ratio of compound b to compound a is (1.05-1.5):1, for example, 1.05:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1.
[0012] Preferably, an acid binding agent is also used in the reaction. Preferably, the acid binding agent is selected from one or more of triethylamine, triisobutylamine, and pyridine. These chemical substances have the function of binding acid and can promote the reaction.
[0013] Preferably, a reaction medium is also used in the reaction, and the reaction medium is selected from one or more of dichloromethane and tetrahydrofuran.
[0014] Preferably, when the reaction is carried out at room temperature, the reaction time is at least 10 hours. The room temperature is 20-25° C. The increase in reaction time is conducive to the improvement of conversion rate. At room temperature, when the reaction time is less than 10 hours, the efficiency of obtaining intermediate compound A is extremely low. Specifically, the applicant found that: when at room temperature, 8 hours cannot be completely converted into intermediate compound A.
[0015] Preferably, after the reaction is completed, a post-treatment step is also included, and the post-treatment includes heating and purification. More specifically, the post-treatment includes a first heating, purification and a second heating. More preferably, the first heating is rotary evaporation, and the reaction medium is removed by heating and rotary evaporation to obtain a crude intermediate compound A sample. More preferably, the purification is performed by a silica gel column, and the eluent is a mixture of n-hexane and ethyl acetate. The purpose of using the eluent is to remove excess compound b, triethylamine and other impurities. More preferably, the volume ratio of n-hexane to ethyl acetate is (4.5-5.5): 1. More preferably, the second heating is rotary evaporation, and the eluent is removed by heating and rotary evaporation to obtain a pure intermediate compound A.
[0016] The third aspect of the present invention discloses a cycloolefin linear random copolymer, wherein the cycloolefin linear random copolymer comprises a structural unit and structural units The random copolymers formed.
[0017] Preferably, the structural unit and structural units The molar ratio of (1 to 15): (5 to 10) is selected in consideration of the performance of the cross-linked copolymer. and structural units A molar ratio higher than 3 will result in a hard and brittle material, and a molar ratio lower than 0.1 will result in extremely weak mechanical properties of the material. The properties of the material can be regulated by changing the molar ratio of the two. More preferably, the molar ratio is 2: (5-10), 3: (5-10), 4: (5-10), 5: (5-10); more preferably, the molar ratio is (2-5): (5-10); and further preferably, (2-5): (5-8).
[0018] The fourth aspect of the present invention provides a method for preparing the above-mentioned cycloolefin linear random copolymer, using the intermediate compound A and the intermediate compound B as described above to carry out random copolymerization, and the synthesis route is as follows:
[0019]
[0020] Preferably, the molar ratio of intermediate compound A to intermediate compound B is (1-15): (5-10). The selection of the range here takes into account the performance of the cross-linked copolymer. If the molar ratio of compound A to B is higher than 3, the material will be hard and brittle. If the molar ratio of compound A to B is lower than 0.1, the mechanical properties of the material will be extremely weak. The performance of the material can be regulated by changing the molar ratio of compound B to A. More preferably, the molar ratio of intermediate compound A to intermediate compound B is 2: (5-10), 3: (5-10), 4: (5-10), 5: (5-10); more preferably, the molar ratio of intermediate compound A to intermediate compound B is (2-5): (5-10); further preferably (2-5): (5-8).
[0021] Preferably, a catalyst is also used in the random copolymerization reaction, and the catalyst is selected from one or more of the third generation Grubbs catalyst (G3) and the second generation Grubbs catalyst (G2). The use of the catalyst can break the double bonds of the norbornene-modified monomer and form a macromolecule in a head-to-tail manner.
[0022] Preferably, the random copolymerization reaction is terminated by using a terminator or an end-capping agent. Preferably, the terminator or end-capping agent is vinyl ethyl ether. Vinyl ethyl ether will separate the G3 catalyst from the polymer backbone by reacting with the [Ru] carbene species of the G3 catalyst.
[0023] Preferably, a reaction solvent is also used in the random copolymerization reaction, and the reaction solvent is selected from one or more of tetrahydrofuran and dichloromethane.
[0024] Preferably, after the random copolymerization reaction is completed, a post-treatment step is further included, and the post-treatment includes precipitation and drying. More preferably, the precipitation process uses a precipitant. Particularly preferably, the precipitant is one or more of anhydrous cold methanol and anhydrous ice ether, which is used to remove part of the solvent, reaction monomers and catalysts. More preferably, the drying temperature is 40 to 70°C.
[0025] The fifth aspect of the present invention discloses a cycloolefin dynamically crosslinked copolymer, which is formed by crosslinking the cycloolefin linear random copolymer described above with a primary amine crosslinking agent.
[0026] Preferably, the primary amine cross-linking agent is selected from one or more of 1,2-bis(2-aminoethoxy)ethane, 1,3-phenylenediamine, and tris(2-aminoethyl)amine.
[0027] Preferably, an organic solvent is also used in the cross-linking reaction. More preferably, the organic solvent is one or more of tetrahydrofuran, dichloromethane, and acetonitrile.
[0028] Preferably, the structural units contained in the primary amine crosslinking agent and the cycloolefin linear random copolymer The molar ratio is: (0.5-1): 1. For example, it can be 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1.
[0029] Preferably, the temperature of the cross-linking reaction is 80-150°C. For example, the temperature of the cross-linking reaction can be 80-90°C, 90-100°C, 100-110°C, 110-120°C, 120-130°C, 130-140°C, 140-150°C, and in a specific embodiment, it is 120°C. This temperature range is used for curing of volatile solvents and cycloolefin dynamic cross-linked copolymer materials. Too low temperature or short time will result in no reaction completion, and high temperature or too long reaction time will result in oxidation of free primary amines and poor material dynamics.
[0030] Preferably, the reaction time of the cross-linking reaction is 6 to 8 hours, such as 6 hours, 7 hours, or 8 hours.
[0031] Preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 1050s at a relaxation temperature of 150°C; more preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 1050s and greater than 150s at a relaxation temperature of 150°C. For example, the relaxation time may be 150-180s, 160-190s, 190-300s, 300-500s, 500-600s, 600-700s, 700-800s, 800-900s, 900-1000s, 1000-1050s, and in a specific embodiment, it is 174s, 565s, 740s, 956s, or 1042s.
[0032] Preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 850s at a relaxation temperature of 160°C; more preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 850s and greater than 120s at a relaxation temperature of 160°C. For example, the relaxation time may be 120-130s, 130-140s, 140-200s, 200-300s, 300-400s, 400-600s, 600-700s, 700-800s, 800-850s, and in a specific embodiment, it is 134s, 373s, 628s, 738s, 824s.
[0033] Preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 650s at a relaxation temperature of 170°C. More preferably, the relaxation time of the cycloolefin dynamically crosslinked copolymer is less than 650s and greater than 100s at a relaxation temperature of 170°C. For example, it may be 100-110s, 110-120s, 120-200s, 200-300s, 250-350s, 350-450s, 450-550s, 500-600s, 600-650s, and in a specific embodiment, it is 113s, 297s, 558s, 506s, 630s.
[0034] The seventh aspect of the present invention discloses the use of the cycloolefin dynamically cross-linked copolymer as a recyclable processing material.
[0035] The preparation method provided by the present application can easily regulate the thermal properties, mechanical properties and dynamic properties of the cycloolefin dynamic crosslinked copolymer by changing the ratio of the two norbornene modified monomers. The cycloolefin dynamic crosslinked copolymer thus formed can not only well maintain the excellent properties of the cycloolefin copolymer, but also exhibit adjustable mechanical and thermomechanical properties, excellent thermal stability and chemical resistance, which help promote the application of cycloolefin copolymer materials in a wider field. In addition, the presence of the vinylamine ester dynamic bond allows the network topology of the cycloolefin dynamic crosslinked copolymer material to be rearranged at high temperature, has the property of being recycled and reprocessed, and prolongs the service life of the cycloolefin dynamic crosslinked copolymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Shown is the H NMR spectrum of the product 5-norbornene-2-acetoacetate methyl ester of Example 1.
[0037] Figure 2 Shown is the mass spectrum of 5-norbornene-2-acetoacetate methyl ester, the product of Example 1.
[0038] Figure 3 Shown is the H-NMR spectrum of the cycloolefin linear random copolymer obtained in Example 2.
[0039] Figure 4 The GPC elution curve of the cyclic olefin linear random copolymer obtained in Example 2 is shown.
[0040] Figure 5 Shown is the H-NMR spectrum of the cycloolefin linear random copolymer obtained in Example 4.
[0041] Figure 6 The GPC elution curve of the cyclic olefin linear random copolymer obtained in Example 4 is shown.
[0042] Figure 7 Shown is the H-NMR spectrum of the cycloolefin linear random copolymer obtained in Example 5.
[0043] Figure 8 The GPC elution curve of the cyclic olefin linear random copolymer obtained in Example 5 is shown.
[0044] Fig. 9 Shown is the H-NMR spectrum of the cycloolefin linear random homopolymer obtained in Comparative Example 2.
[0045] Fig.10 Shown is the GPC elution curve of the cycloolefin linear random homopolymer obtained in Comparative Example 2.
[0046] Fig.11 Shown are infrared spectra of the cycloolefin dynamically cross-linked copolymers obtained in Examples 3 to 7 and Comparative Examples 1 to 2.
[0047] Fig.12 Shown are scanning calorimetry diagrams of the cycloolefin dynamically cross-linked copolymers obtained in Examples 3 to 7 and Comparative Examples 1 to 2.
[0048] Fig.13 Shown are thermomechanical analysis temperature scans of the cycloolefin dynamically crosslinked copolymers obtained in Examples 3 to 7 and Comparative Examples 1 to 2.
[0049] Fig.14 Shown are stress relaxation diagrams of the cycloolefin dynamically crosslinked copolymers obtained in Examples 3 to 7.
[0050] Fig.15 Shown are the tensile performance effect diagrams of the cycloolefin dynamically cross-linked copolymers obtained in Examples 3 to 7. DETAILED DESCRIPTION
[0051] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0052] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.
[0053] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0054] In the present application, the applicant provides a novel dynamically cross-linked copolymer with commercial application value. The technical concept is: using norbornene-modified monomers, a functionalized cycloolefin copolymer is constructed through a ring-opening metathesis polymerization reaction, and a cycloolefin dynamically cross-linked copolymer is formed by introducing vinylamine ester dynamic bonds through a primary amine cross-linking agent.
[0055] Specifically, the cycloolefin copolymer is a random copolymer, and the schematic diagram of the structure of the cycloolefin linear random copolymer is as follows:
[0056]
[0057] It can be obtained by polymerization reaction of intermediate compound A and intermediate compound B. And the number average molecular weight of the final cycloolefin random copolymer can be regulated by feeding raw materials. Preferably, the number average molecular weight of the cycloolefin random copolymer is 1w-20w, such as 1w-1.5w, 1.5w-2w, 1.6w-1.8w, 2w-3w, 3w-4w, 4w-5w, 5w-10w, 11w-13w, 13w-15w, 15w-18w, 18w-20w. The molecular weight distribution can be 1.1-1.5. For example, it can be 1.1-1.2, 1.2-1.3, 1.3-1.4, 1.4-1.5, 1.17-1.29, 1.1-1.3.
[0058] Specifically, the crosslinking agent is selected from one or more of 1,2-bis(2-aminoethoxy)ethane, 1,3-phenylenediamine, and tris(2-aminoethyl)amine.
[0059] Since the constructed functionalized cycloolefin copolymer has acetoacetate groups, it can react with the primary amine groups in the cross-linking agent to form a material with a vinylamine ester dynamic bond having dynamic properties.
[0060] Specifically, in the following examples and comparative examples, the synthetic route of the cycloolefin dynamically crosslinked copolymer formed by crosslinking a cycloolefin linear random copolymer with a crosslinking agent 1,2-bis(2-aminoethoxy)ethane is as follows:
[0061]
[0062] The intermediate compound B used in the present invention is obtained through commercial purchase.
[0063] Specifically, in the following examples and comparative examples, the intermediate compound B is prepared by reacting the compound a with the compound c, and the synthesis route is as follows:
[0064]
[0065] Example 1
[0066] This example is a synthesis example of intermediate compound A.
[0067] The synthetic route of intermediate compound A is as follows:
[0068]
[0069] The specific steps are as follows:
[0070] 1) 3 g (1 eq.) of compound a (97%) was dissolved in 25 ml of anhydrous dichloromethane;
[0071] 2) Slowly add 2.24 g of compound b (1.1 eq., 97%) to the above solution;
[0072] 3) The solution was magnetically stirred at room temperature, and 100 μl of triethylamine (99.0%) was added dropwise, and the solution was stirred for 12 hours at room temperature;
[0073] Post-processing steps:
[0074] a) removing the dichloromethane solvent from the reacted solution by rotary evaporation to obtain a crude 5-norbornene-2-acetoacetate methyl ester sample;
[0075] b) purifying the crude 5-norbornene-2-acetoacetate sample by passing it through a silica gel column, wherein the eluent is n-hexane:ethyl acetate in a volume ratio of 5:1;
[0076] c) removing the eluent by rotary evaporation to obtain pure 5-norbornene-2-acetoacetate methyl ester.
[0077] Figure 1 The H NMR spectrum of the product 5-norbornene-2-acetoacetate in this example is shown in FIG. Figure 1 It can be seen that the peak position and integral ratio of the H NMR spectrum are consistent with the theoretical structure of 5-norbornene-2-acetoacetate methyl ester, proving that the product is 5-norbornene-2-acetoacetate methyl ester and contains no impurities.
[0078] Figure 2 The mass spectrum of the product 5-norbornene-2-acetoacetate in this example is shown in FIG. Figure 2 It can be seen that the mass spectrum result of 208.1 is consistent with the theoretical molecular weight and is the target compound.
[0079] The calculated yield is 91.2%.
[0080] Example 2
[0081] This example is the preparation of a cycloolefin linear random copolymer in which the intermediate compound A accounts for 35%.
[0082] The specific synthetic route is as follows:
[0083]
[0084] The specific steps are as follows:
[0085] 1) In a glove box, the monomer intermediate compound A (262.4 mg, 1.26 mmol) and the intermediate compound B (585.9 mg, 2.34 mmol) prepared in Example 1 were added to a reaction bottle containing 16 ml of anhydrous tetrahydrofuran;
[0086] 2) In a glove box, take Grubbs third-generation catalyst (63.7 mg, 0.072 mmol) and add it to 4 ml of anhydrous tetrahydrofuran to completely dissolve the catalyst in the solvent;
[0087] 3) then, under magnetic stirring, the catalyst solution was quickly added to the solution containing the reaction monomer, and the solution was stirred at room temperature for 1 hour;
[0088] 4) Add 2.4 ml of vinyl ethyl ether to the above solution for capping reaction for half an hour;
[0089] Post-processing steps:
[0090] a) After the reaction is completed, the resultant solution is taken out from the glove box and dripped into a large amount of anhydrous cold methanol (20 times the volume of the resultant solution) for precipitation three times;
[0091] b) drying the obtained precipitate in a vacuum drying oven at 40° C. for 16 hours to obtain a cycloolefin linear random copolymer.
[0092] Figure 3 The H NMR spectrum of the cycloolefin linear random copolymer prepared as above is shown. Figure 3 The sum of the integrated areas of the characteristic peaks at chemical shifts 3.4 and 4.9 corresponding to the methyl acetoacetate group of compound A in the mesocyclic olefin linear random copolymer is 0.35. It can be seen that compound A accounts for 35% of the copolymer, indicating that the structural unit was successfully synthesized. It accounts for 35% of cyclic olefin linear random copolymer.
[0093] Figure 4 The GPC elution curve of the cycloolefin linear random copolymer prepared as above is shown. Figure 4 It can be seen that the relative molecular mass of the cycloolefin linear random copolymer prepared above is about 16621 g / mol, and the dispersion degree is 1.235.
[0094] The product yield is 76.5%.
[0095] Example 3
[0096] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 35% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.8.
[0097] The specific steps are as follows:
[0098] a) 500 mg of the cycloolefin linear random copolymer prepared in Example 2 was dissolved in a polytetrafluoroethylene beaker containing 20 ml of anhydrous tetrahydrofuran; 101.1 mg of 1,2-bis(2-aminoethoxy)ethane (98%) was added to the above solution.
[0099] b) stirring the solution at room temperature for 30 minutes after the addition was completed;
[0100] c) The mixed solution after being stirred evenly was placed in a 120° C. oven for 6 hours to volatilize the solvent and solidify, and the sample was further placed in a 70° C. vacuum oven overnight to continue solidification and remove small molecular water, etc., to finally obtain a cycloolefin dynamically cross-linked copolymer.
[0101] The cured sample was taken out, cut into small pieces, placed on a flat-plate hot press and hot-pressed at 180°C for 30 minutes with a pressure of 18 MPa to obtain a rectangular sample with a thickness of about 1 mm for subsequent performance characterization.
[0102] Example 4
[0103] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 20% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.8.
[0104] The specific steps are as follows:
[0105] 1) Preparation of cycloolefin linear random copolymers.
[0106] The steps are exactly the same as those in Example 2, except that the amount of the monomer intermediate compound A prepared in Example 1 is 149.9 mg, 0.72 mmol; the amount of the intermediate compound B is 721.1 mg, 2.88 mmol. The other steps are exactly the same as those in Example 2.
[0107] Figure 5 The H NMR spectrum of the cycloolefin linear random copolymer prepared in this example is shown. Figure 5 The sum of the integrated areas of the characteristic peaks at chemical shifts 3.4 and 4.9 corresponding to the methyl acetoacetate group of compound A in the medium-cycloolefin linear random copolymer is 0.20. It can be seen that compound A accounts for 20% in the copolymer, indicating that the structural unit was successfully synthesized. 20% cyclic olefin linear random copolymer.
[0108] Figure 6 The GPC elution curve of the cycloolefin linear random copolymer prepared in this example is shown. Figure 6 It can be seen that the relative molecular mass of the cycloolefin linear random copolymer prepared in this example is 16742 g / mol and the dispersity is 1.175.
[0109] 2) Preparation of cycloolefin dynamically cross-linked copolymers.
[0110] The steps are exactly the same as those in Example 3, except that the cycloolefin linear random copolymer used is the cycloolefin linear random copolymer prepared in 1) of this Example, and the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added is 56.3 mg (1.8 eq.). The other steps are exactly the same as those in Example 3.
[0111] Example 5
[0112] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 50% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.8.
[0113] The specific steps are as follows:
[0114] 1) Preparation of cycloolefin linear random copolymers.
[0115] The steps are exactly the same as those in Example 2, except that the amount of the monomer intermediate compound A prepared in Example 1 is 374.9 mg, 1.8 mmol; the amount of the intermediate compound B is 450.7 mg, 1.8 mmol. The other steps are exactly the same as those in Example 2.
[0116] The product yield is 82.9%.
[0117] Figure 7 The H NMR spectrum of the cycloolefin linear random copolymer prepared as above is shown. Figure 7 The sum of the integrated areas of the characteristic peaks at chemical shifts 3.4 and 4.9 corresponding to the methyl acetoacetate group of compound A in the medium-cycloolefin linear random copolymer is 0.50. It can be seen that compound A accounts for 50% of the copolymer, indicating that the structural unit was successfully synthesized. 50% cyclic olefin linear random copolymer.
[0118] Figure 8 The GPC elution curve of the cycloolefin linear random copolymer prepared as above is shown. Figure 8 It can be seen that the relative molecular mass of the cycloolefin linear random copolymer prepared in this example is 18183 g / mol and the dispersity is 1.220.
[0119] 2) Preparation of cycloolefin dynamically cross-linked copolymers.
[0120] The steps are exactly the same as those in Example 3, except that the cycloolefin linear random copolymer used is the cycloolefin linear random copolymer prepared in 1) of this Example, and the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added is 148.4 mg (1.8 eq.). The other steps are exactly the same as those in Example 3.
[0121] Example 6
[0122] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 35% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.6.
[0123] The specific steps are as follows:
[0124] The steps are exactly the same as those in Example 3, except that the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added in step a) is 89.9 mg. The other steps are exactly the same as those in Example 3.
[0125] Example 7
[0126] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 35% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 2.0.
[0127] The specific steps are as follows:
[0128] The steps are exactly the same as those in Example 3, except that the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added in step a) is 112.3 mg. The other steps are exactly the same as those in Example 3.
[0129] Comparative Example 1
[0130] This embodiment is the preparation of a cycloolefin dynamically cross-linked copolymer in which the intermediate compound A accounts for 35% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.4.
[0131] The specific steps are as follows:
[0132] The steps are exactly the same as those in Example 3, except that the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added in step a) is 78.6 mg. The other steps are exactly the same as those in Example 3.
[0133] Comparative Example 2
[0134] This example is the preparation of a cycloolefin dynamically cross-linked homopolymer in which the intermediate compound A accounts for 100% and the molar ratio of the primary amine group in the cross-linking agent to the acetoacetic acid group in the intermediate compound A is 1.8.
[0135] The specific steps are as follows:
[0136] 1) Preparation of cycloolefin linear random homopolymers.
[0137] The steps are exactly the same as those in Example 2, except that the amount of the monomer intermediate compound A prepared in Example 1 is 749.7 mg, 3.6 mmol; and the intermediate compound B is not added. The other steps are exactly the same as those in Example 2.
[0138] Fig. 9 The NMR hydrogen spectrum of the cycloolefin linear random homopolymer prepared in this example is shown. Fig. 9 The sum of the integrated areas of the characteristic peaks at chemical shifts 3.4 and 4.9 corresponding to the methyl acetoacetate group of compound A in the linear random homopolymer of medium-cycloolefin is 1.00. It can be seen that compound A accounts for 100% in the homopolymer, indicating that the structural unit was successfully synthesized. 100% cyclic olefin linear random homopolymer.
[0139] Fig.10The GPC elution curve of the cycloolefin linear random homopolymer prepared in this example is shown in FIG. Fig.10 It can be seen that the relative molecular mass of the cycloolefin linear random homopolymer prepared in this example is 16765 g / mol and the dispersity is 1.282.
[0140] 2) Preparation of cycloolefin dynamically cross-linked homopolymers.
[0141] The steps are exactly the same as those in Example 3, except that the cycloolefin linear random homopolymer used is the cycloolefin linear random homopolymer prepared in 1) of this comparative example, and the amount of 1,2-bis(2-aminoethoxy)ethane (98%) added is 326.8 mg. The other steps are exactly the same as those in Example 3.
[0142] The performance test results of the cycloolefin dynamically cross-linked copolymers obtained in Examples 3 to 7 and Comparative Examples 1 to 2 are as follows:
[0143] Infrared spectrum: Infrared spectrum was measured using FTIR (Spectrum 100) at room temperature with a wave number range of 650 to 4000 cm -1 .
[0144] Specific test results such as Fig.11 As shown. Fig.11 It can be seen from the infrared test effect diagrams of Examples 3-5 and Comparative Example 2 in the left figure that when the molar ratio of the primary amine group in the crosslinking agent to the acetoacetate group in the intermediate compound A is constant, both 1.8, the cycloolefin dynamically crosslinked copolymer has a wave number of 1730 cm -1 1600~1646cm -1 The integrated area of the regional absorption peak changes with the change of the molar ratio of compound A and B. The more the content of the structural unit formed by compound A, the higher the absorption peak area at 1730 cm -1 The smaller the integral area of the absorption peak at 1600-1646cm -1 The larger the integrated area of the regional absorption peak.
[0145] Depend on Fig.11 The infrared test effect diagrams corresponding to Example 3, Examples 6-7 and Comparative Example 1 in the right figure show that when the intermediate compound A accounts for 35%, the cycloolefin dynamically cross-linked copolymer has a wave number of 3200-3500cm -1 The area of the interval absorption peak increases with the increase of the molar ratio of the primary amine group in the cross-linking agent to the acetoacetate group in the intermediate compound A.
[0146] Scanning calorimetry: Scanning calorimetry experiments were performed on a DSC (TA Q2000) with three cycles of heating / cooling / heating from -60°C to 120°C at a heating / cooling rate of 10°C / min under a nitrogen atmosphere. The glass transition temperature was obtained using the third heating cycle curve.
[0147] Test results such as Fig.12 As shown by Fig.12 The DSC curves of Example 3 (Compound A content 35%), Example 4 (Compound A content 20%), Example 5 (Compound A content 50%) and Comparative Example 2 (Compound A content 100%) in the left figure show that when the molar ratio of the primary amine group in the crosslinking agent to the acetoacetic acid group in the intermediate compound A is constant, both 1.8, the glass transition temperature of the cycloolefin dynamically crosslinked copolymer increases with the increase of the molar ratio of compound A to compound B. Fig.12 From the DSC curves of Example 3, Examples 6-7 and Comparative Example 1 corresponding to the right figure, it can be seen that when the proportion of intermediate compound A is a certain 35%, the glass transition temperature of the cycloolefin dynamically cross-linked copolymer decreases with the increase of the molar ratio of primary amine groups in the cross-linking agent to acetoacetate groups in the intermediate compound A.
[0148] Temperature scanning: The temperature scanning experiment was tested on DMA (TA Q850), and rectangular splines with dimensions of 1.0 mm (T) × 5.5 mm (W) × 15 mm (L) were cut. The temperature scanning range was from -60°C to 120°C, the heating rate was 5°C / min, and the oscillation strain was 1%.
[0149] Test results such as Fig.13 As shown by Fig.13 It can be seen from the corresponding DMA curve in the left figure that the platform moduli of the cycloolefin dynamically crosslinked copolymers obtained in Example 3 (Compound A content 35%), Example 4 (Compound A content 20%), Example 5 (Compound A content 50%) and Comparative Example 2 (Compound A content 100%) are 0.48 times, 1.41 times and 2.92 times the platform modulus of the cycloolefin dynamically crosslinked copolymer obtained in Example 3, respectively; Fig.13 From the DMA curves of the cycloolefin dynamically crosslinked copolymers obtained in the corresponding examples 6, 7, and 1 in the right figure, it can be seen that the platform moduli are 1.09 times, 0.82 times, and 1.12 times the platform modulus of the cycloolefin dynamically crosslinked copolymer obtained in example 3. This indicates that the platform modulus of the cycloolefin dynamically crosslinked copolymer decreases with the increase of the molar ratio of the primary amine group in the crosslinking agent to the acetoacetate group in the intermediate compound A.
[0150] Stress relaxation: The stress relaxation experiment was conducted on a rotational rheometer (TA ARES-G2) using 8 mm parallel plates at 150°C to 170°C with a 10°C interval. The relaxation modulus G(t) obtained was normalized with the initial relaxation modulus G0 and plotted as a function of time.
[0151] Specific results such as Fig.14 As shown, Fig.14 It is a normalized stress relaxation diagram. It can be seen from the figure that the dynamic exchange rate of the cycloolefin dynamic crosslinked copolymer obtained in Example 3 at the same temperature is much greater than that of the cycloolefin dynamic crosslinked copolymer in Example 4 and Example 5, which shows that when the molar ratio of the primary amine group in the crosslinking agent to the acetoacetate group in the intermediate compound A is constant, when the intermediate compound A accounts for 35%, the dynamic exchange rate of the obtained cycloolefin dynamic crosslinked copolymer is the fastest and the dynamic property is the best. It can be seen from Example 3, Example 6 and Example 7 that when the intermediate compound A accounts for 35%, the dynamic exchange rate of the cycloolefin dynamic crosslinked copolymer increases with the increase of the molar ratio of the primary amine group in the crosslinking agent to the acetoacetate group in the intermediate compound A. The relaxation time corresponding to the specific temperature is shown in Table 1.
[0152] Table 1
[0153]
[0154] Tensile properties: The tensile stress-strain curve test of a dumbbell-shaped specimen of 1.0 mm (T) × 2 mm (W) × 35 mm (L) was carried out on a universal testing machine (Instron 3343) at room temperature (25°C) with a uniaxial tensile rate of 5 mm / min.
[0155] Test results such as Fig.15 As shown, the curve results show that the ductility of the cycloolefin dynamically crosslinked copolymer obtained in Example 3 (Compound A content 35%) is higher than that of the cycloolefin dynamically crosslinked copolymers in Example 4 (Compound A content 20%) and Example 5 (Compound A content 50%), and the ductility of the cycloolefin dynamically crosslinked copolymers obtained in Example 3 (molar ratio 1.8), Example 6 (molar ratio 1.6) and Example 7 (molar ratio 2.0) increases with the increase of the molar ratio of the primary amine group in the crosslinking agent to the acetoacetic acid group in the intermediate compound A. Since the final product obtained in Comparative Example 1 has poor dynamics and unsatisfactory healing effect after hot pressing, and the final product obtained in Comparative Example 2 is hard and brittle, the mechanical properties of the cycloolefin dynamically crosslinked copolymers obtained in the two comparative examples are extremely poor and difficult to characterize.
[0156] In the present application, the applicant uses norbornene-modified monomers of formula I and formula II as described in the present application to construct functionalized cycloolefin copolymers through ring-opening metathesis polymerization, and introduces vinylamine ester dynamic bonds through primary amine crosslinking agents to form cycloolefin dynamic crosslinked copolymers. By changing the ratio of the two norbornene-modified monomers, the thermal properties, mechanical properties and dynamic properties of the cycloolefin dynamic crosslinked copolymer can be easily regulated, and its thermal stability and chemical resistance are greatly improved compared with traditional cycloolefin copolymers. In addition, the presence of vinylamine ester dynamic bonds allows the cycloolefin dynamic crosslinked copolymer to be recycled and reprocessed, extending the service life of the cycloolefin dynamic crosslinked copolymer.
[0157] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A cycloolefin linear random copolymer, characterized in that: The cycloolefin linear random copolymer comprises structural units and structural units The random copolymer formed; In the cycloolefin linear random copolymer, the structural unit and structural units The molar ratio is (1~15):(5~10).
2. A method for preparing a cycloolefin linear random copolymer as claimed in claim 1, wherein the intermediate compound A and the intermediate compound B are subjected to random copolymerization, and the synthetic route is as follows:
3. The preparation method according to claim 2, characterized in that: The random copolymerization reaction further uses a catalyst, the catalyst is selected from one or more of the third generation of Grubbs catalyst and the second generation of Grubbs catalyst; and / or, a terminator or end-capping agent is used to terminate the random copolymerization reaction; the terminator or end-capping agent is vinyl ethyl ether; And / or, a reaction solvent is also used in the random copolymerization reaction; the reaction solvent is selected from one or more of tetrahydrofuran and dichloromethane; And / or, after the reaction is completed, post-treatment is further included, and the post-treatment includes precipitation and drying.
4. The preparation method according to claim 3, characterized in that: The precipitation process uses a precipitant, and the precipitant is one or more of anhydrous cold methanol and anhydrous ice ether.
5. A cycloolefin dynamically crosslinked copolymer, characterized in that: The cycloolefin dynamically cross-linked copolymer is formed by cross-linking the cycloolefin linear random copolymer as claimed in claim 1 with a primary amine cross-linking agent.
6. The cycloolefin dynamically cross-linked copolymer according to claim 5, characterized in that: The primary amine crosslinking agent is selected from one or more of 1,2-bis(2-aminoethoxy)ethane, 1,3-phenylenediamine, and tris(2-aminoethyl)amine; And / or, the structural units contained in the primary amine crosslinking agent and the cycloolefin linear random copolymer The molar ratio is (0.5-1):1; And / or, an organic solvent is also used in the cross-linking reaction; the organic solvent is one or more of tetrahydrofuran, dichloromethane, and acetonitrile; And / or, the temperature of the cross-linking reaction is 80-150°C.
7. The cycloolefin dynamically cross-linked copolymer according to claim 6, characterized in that: At a relaxation temperature of 150°C, the relaxation time is less than 1050s.
8. The cycloolefin dynamically cross-linked copolymer according to claim 6, characterized in that: At a relaxation temperature of 160°C, the relaxation time is less than 850s.
9. The cycloolefin dynamically cross-linked copolymer according to claim 6, characterized in that: At a relaxation temperature of 170°C, the relaxation time is less than 650s.
10. Use of the cycloolefin dynamically cross-linked copolymer according to any one of claims 5 to 9 as a recyclable processing material.
Citation Information
Patent Citations
Cycloolefin copolymer as well as preparation method and application thereof
CN110669207A
Cycloolefin copolymer, and preparation method and application thereof
CN110776618A
Process for forming solidified composition and produced solidified composition
CN1258697A
Cellulose ester film, polarizing plate and image display device
JP2017179273A
Hardenable compositions of copolymers containing the acetoacetate of 2-hydroxymethyl-5-norbornene
US3520843A