Surface treatment method for hydrogen storage alloy and use thereof

By forming a Ni-rich layer through low-temperature heat treatment, the problem of corrosion and pulverization of hydrogen storage alloy powder in nickel-metal hydride batteries has been solved, improving the discharge performance and cycle life of nickel-metal hydride batteries while reducing environmental risks and production costs.

CN117185253BActive Publication Date: 2026-11-10SOUTH CHINA UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311144343.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-05
Publication Date
2026-11-10
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

Existing hydrogen storage alloy powders suffer from performance degradation in nickel-metal hydride batteries due to corrosion and pulverization. Furthermore, traditional surface treatment methods present environmental problems and excessive Ni content hinders hydrogen atom transport, leading to a decrease in hydrogen storage capacity.

Method used

The surface of the hydrogen storage alloy is treated by low-temperature heat treatment. A Ni-rich layer is formed by low-temperature heat treatment in a muffle furnace, which improves the catalytic activity and corrosion resistance of the alloy surface and reduces the Ni content.

Benefits of technology

It improves the activity and corrosion resistance of the alloy surface, enhances the hydrogen insertion and extraction performance, improves the discharge performance and cycle life of nickel-metal hydride batteries, and reduces environmental risks and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117185253B_ABST
    Figure CN117185253B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of rare earth hydrogen storage alloy electrode, and provides a method for modifying the surface of hydrogen storage alloy by low-temperature heat treatment. The method comprises the following steps: placing the hydrogen storage alloy in a muffle furnace for low-temperature short-time heat treatment, so that the surface layer of the alloy is slightly oxidized to form nanometer nickel, the saturation magnetization of the alloy is increased, and the charge-discharge rate performance of the alloy is greatly improved on the premise of ensuring the discharge capacity of the alloy. The process condition of the present application is simple, green and environmentally friendly, and low in cost, and can significantly improve the charge-discharge rate performance of the nickel-hydrogen battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nickel-metal hydride battery electrode processing technology, and in particular to a surface treatment method for hydrogen storage alloys and its application. Background Technology

[0002] Nickel-metal hydride (Ni-MH) batteries, as one of the earliest commercially available rechargeable batteries, possess advantages such as high energy density, good resistance to overcharge and over-discharge, high safety performance, and environmental friendliness, and still hold an irreplaceable position in some application areas. However, there is still significant room for improvement in Ni-MH batteries regarding output power, cycle life, and low-temperature performance. The key to improving Ni-MH battery performance lies in improving its negative electrode material. After hydrogen storage alloy powder is used to fabricate battery electrodes, repeated charge-discharge cycles in an alkaline electrolyte lead to corrosion and pulverization of the alloy powder, resulting in a gradual decline in battery performance. Therefore, surface modification techniques are needed to optimize the activity of the alloy surface, making hydrogen insertion and extraction on the surface of the hydrogen storage alloy powder easier, thereby optimizing the performance of the alloy electrode.

[0003] Current surface treatment methods for hydrogen storage alloy powders mainly include reduction, coating, alkaline solutions, and acid solutions. The Ni-rich layer formed on the alloy surface after hot alkaline treatment exhibits good catalytic activity and corrosion resistance; however, excessively high Ni content hinders hydrogen atom transport, leading to a decrease in hydrogen storage capacity. Furthermore, alkaline treatment processes require large amounts of strong alkaline solutions and water for cleaning the alloy surface, resulting in lengthy processing times and environmental concerns. Therefore, providing an environmentally friendly and efficient surface treatment method for hydrogen storage alloys is a problem that needs to be solved. Summary of the Invention

[0004] To address the aforementioned problems, the present invention aims to provide a surface treatment method for hydrogen storage alloys and its application. The treatment method involves performing low-temperature heat treatment on the hydrogen storage alloy in a muffle furnace. This method is not only simple to operate and use, but also has a high safety factor, low energy consumption, mild conditions, and a stable and easily controllable reaction process, making it suitable for large-scale industrial production and use.

[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0006] A surface treatment method for a hydrogen storage alloy includes the following steps:

[0007] The hydrogen storage alloy is obtained by low-temperature heat treatment.

[0008] Preferably, as a preferred embodiment, the particle size of the hydrogen storage alloy is 200-400 mesh.

[0009] Preferably, as a preferred embodiment, the mass of the hydrogen storage alloy is 2g.

[0010] Preferably, as a preferred embodiment, the heat treatment can be carried out in a tube furnace or a muffle furnace.

[0011] Preferably, as a preferred embodiment, the low-temperature heat treatment heating rate is 5℃ / min, the heat treatment holding temperature is 80-240℃, and the heat treatment holding time is 10-60min.

[0012] Preferably, as a preferred embodiment, after treatment, an oxide layer of a certain thickness is formed on the alloy surface, and it contains a certain amount of nickel. The higher the heat treatment holding temperature, the higher the saturation magnetization degree of the hydrogen storage alloy.

[0013] Preferably, as a preferred embodiment, the hydrogen storage alloy is an A2B7 type or AB5 type hydrogen storage alloy, such as a Re-Mg-Ni based alloy or a LaNi5 based alloy, and the hydrogen storage alloy needs to contain Ni or Co elements.

[0014] Another object of the present invention is to provide a hydrogen storage alloy obtained by a surface treatment method.

[0015] Another object of the present invention is to provide an application of a hydrogen storage alloy in the negative electrode material of a nickel-metal hydride battery.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] This invention provides a surface treatment method for hydrogen storage alloys. The method involves low-temperature heat treatment of the hydrogen storage alloy in a muffle furnace, which is not only simple to operate and use, but also has a high safety factor, low energy consumption, mild conditions, and a stable and easily controllable reaction process, facilitating large-scale industrial production and use. The hydrogen storage alloy obtained by this invention achieves a highly active surface while maintaining discharge capacity. The maximum discharge capacity of the hydrogen storage alloy electrode obtained with different heat treatment times and temperatures is between 350-360 mAh / g, and the capacity retention rate S after 100 charge-discharge cycles is [missing information]. 100 Between 80-82%. Using the surface treatment method of this invention, the discharge performance (HRD) of the hydrogen storage alloy at a current density of 1200 mA / g is [value missing]. 1200 The HRD content was increased from 71.77% in the original alloy to 87.14%. 1500 The content of the alloy composition increased from 67.54% in the original alloy to 84.47%, and the saturation magnetization of the alloy increased from 0.097 emu / g in the initial alloy to a maximum.

[0018] The Ni content on the alloy surface was increased to 1.898 emu / g.

[0019] The low-temperature heat treatment method used in this invention is cost-effective and produces excellent electrochemical performance, making it widely applicable to new nickel-metal hydride battery anode materials with high capacity, long service life, and high current discharge performance. Attached Figure Description

[0020] Figure 1 The image shows a comparison of the saturation magnetization of the samples after treatment in Examples 1-6 of this invention with that of the original alloy; the results show that the saturation magnetization of the treated samples is improved.

[0021] Figure 2 The XRD patterns of the samples after treatment in Examples 1-6 of this invention are shown; the results indicate that the bulk structure of the samples did not change after treatment.

[0022] Figure 3 This is a comparison chart of the high-rate discharge performance of the samples after treatment in Examples 1-6 of this invention;

[0023] Figure 4 This is a comparison of the fine XPS multilayer etching spectra of Ni element in the hydrogen storage alloy raw material of the present invention and the sample after treatment in Example 6; the results show that the Ni content of the sample increases after surface treatment.

[0024] Figure 5 This is a comparison chart of the high-rate discharge performance of the samples after treatment in Example 7 of the present invention. Detailed Implementation

[0025] I. Example 1

[0026] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg 0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53 The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 200℃, and the heat treatment holding time was 10min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0027] The obtained hydrogen storage alloy was subjected to X-ray powder diffraction (XRD) analysis. The testing conditions were: Cu-Kα rays, power 45 kV × 40 mA, step size 0.02°, and test range 20–60°. Qualitative XRD analysis was performed on the obtained hydrogen storage alloy and its raw materials, and the results are as follows: Figure 2 As shown.

[0028] Weigh 0.1g of the hydrogen storage alloy treated in this embodiment and 0.1g of the hydrogen storage alloy raw material, and analyze them separately using a vibrating sample magnetometer (VSM). The results show that the saturation magnetization of the hydrogen storage alloy treated in this embodiment reaches 0.946 emu / g under a 5000 Oe magnetic field, and the magnetization of the hydrogen storage alloy raw material is 0.097 emu / g. The results are as follows: Figure 1 As shown.

[0029] The hydrogen storage alloy obtained after processing in this embodiment was mixed with Ni powder at a mass ratio of 1:4. 0.1g of the mixed powder was pressurized at 20MPa for 30s to obtain a circular hydrogen storage alloy electrode sheet with a diameter of 10cm and a thickness of approximately 1mm. Testing was conducted in a constant temperature chamber at 25℃ using a three-electrode system, with the negative electrode being the hydrogen storage electrode, the positive electrode being the Ni(OH)₂ electrode, the reference electrode being the Hg / HgO electrode, and the electrolyte being a 6mol / L potassium hydroxide solution. Before the electrochemical cycle test, the test electrode was placed in a 6mol / L KOH solution for 1h, charged at a current density of 60mA / g for 7.5h, allowed to stand for 5min, and then discharged at a current density of 60mA / g to a cutoff potential of -0.6V (vs. Hg / HgO), allowed to stand for 5min, and then the next cycle was performed. The high-rate discharge performance test was conducted by first charging the electrode with a current density of 60 mA / g for 7.5 h, and then discharging it with current densities of 300, 600, 900, 1200, and 1500 mA / g, respectively, with a discharge cutoff voltage of -0.6V (vs. Hg / HgO). The discharge capacity of the alloy electrode at different discharge current densities was recorded.

[0030] Keeping other conditions unchanged, the hydrogen storage alloy processed in this embodiment was replaced with hydrogen storage alloy raw material and low-temperature heat-treated alloy powder, respectively. The highest discharge specific capacity and charge-discharge cycle performance were tested, and the results are shown in Table 1, where C... max The highest discharge specific capacity of the alloy, S 100 This refers to the ratio of the discharge capacity after 100 cycles of the alloy to its maximum discharge specific capacity; the results obtained from testing high-rate discharge performance are as follows. Figure 3 As shown.

[0031] II. Example 2

[0032] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg 0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 180℃, and the heat treatment holding time was 10min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0033] The hydrogen storage alloy treated in Example 2 was tested using the same test method as in Example 1, and the results are shown in Table 1 and 2. Figure 1-3 Show.

[0034] III. Example 3

[0035] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg 0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53 The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 220℃, and the heat treatment holding time was 10min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0036] The hydrogen storage alloy treated in Example 3 was tested using the same test method as in Example 1, and the results are shown in Table 1 and 2. Figure 1-3 As shown.

[0037] IV. Example 4

[0038] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg 0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53 The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 240℃, and the heat treatment holding time was 10min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0039] The hydrogen storage alloy treated in Example 4 was tested using the same test method as in Example 1, and the results are shown in Table 1 and 2. Figure 1-3 As shown.

[0040] V. Example 5

[0041] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53 The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 200℃, and the heat treatment holding time was 30min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0042] The hydrogen storage alloy treated in Example 5 was tested using the same test method as in Example 1, and the results are shown in Table 1 and 2. Figure 1-3 As shown.

[0043] VI. Example 6

[0044] La with a particle size of 200-400 mesh 0.32 Sm 0.56 Mg 0.12 Zr 0.0024 (Ni 0.96 Al 0.04 ) 3.53 The hydrogen storage alloy raw material was placed in a magnetic boat, and the magnetic boat was placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, the heat treatment holding temperature was 200℃, and the heat treatment holding time was 60min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0045] The hydrogen storage alloy and hydrogen storage alloy raw material obtained after processing in Example 6 were subjected to XPS testing, and the test results are as follows: Figure 4 As shown, the left figure is the XPS spectrum of Ni element in the hydrogen storage alloy material at different etching thicknesses. With increasing etching thickness, the Ni content in the alloy increases. 2+ The amount of Ni decreases, while the amount of metallic Ni increases, resulting in a surface layer thickness of approximately 10-15 nm. The right figure shows the XPS spectra of Ni elemental composition at different etching thicknesses in the treated samples. Compared to hydrogen storage alloy raw materials, as the etching thickness increases, the amount of Ni in the alloy decreases. 2+ The amount of Ni in the surface layer of the hydrogen storage alloy increases by 10-15 nm after low-temperature heat treatment, resulting in a surface thickness of approximately 5 nm. Compared to the raw materials for hydrogen storage alloys, the Ni content in the surface layer of the hydrogen storage alloy increases by approximately 10-15 nm after low-temperature heat treatment.

[0046] The hydrogen storage alloy treated in Example 6 was tested using the same test method as in Example 1, and the results are shown in Table 1 and 2. Figure 1-3 As shown.

[0047] Table 1. Performance results of alloy samples obtained in Examples 1-6

[0048]

[0049] As shown in Table 1, with the increase of the low-temperature heat treatment holding temperature, the magnetization of the alloy sample gradually increases, the maximum discharge specific capacity of the alloy changes little, and the charge-discharge cycle performance is relatively stable. With the extension of the low-temperature heat treatment holding time, the magnetization of the alloy sample gradually increases, the maximum discharge specific capacity of the alloy changes little, and the charge-discharge cycle performance is relatively stable. A Ni-rich layer forms on the surface of the treated hydrogen storage alloy, enhancing the saturation magnetization, improving the electrocatalytic properties and surface conductivity of the alloy powder, and inhibiting oxidation and pulverization.

[0050] from Figure 1 It can be seen that the phase structure of the sample did not change after treatment.

[0051] from Figure 4 It can be seen that as the holding temperature of the low-temperature heat treatment increases, the high-rate discharge performance of the alloy sample gradually increases; as the holding time of the low-temperature heat treatment increases, the high-rate discharge performance of the alloy sample gradually decreases.

[0052] VII. Example 7

[0053] To verify the universality of the method of this invention, an AB5 type hydrogen storage alloy was selected for testing the La gold sample. 0.658 Ce o.213 Sm 0.104 Zr 0.026 Ni 4.32 Co 0.166 Mn 0.25 Al 0.35 The test involved placing the AB5 hydrogen storage alloy raw material in a magnetic boat, which was then placed in a muffle furnace for low-temperature heat treatment. The heating rate was 5℃ / min, and the heat treatment holding temperatures were 200℃ and 240℃. The holding times at 200℃ were 10 min and 30 min, and the holding time at 240℃ was 10 min. After the holding time was completed, the sample was cooled to room temperature with the furnace to obtain the treated hydrogen storage alloy.

[0054] The high-rate discharge performance of the sample obtained in Example 7 was tested, and the results are as follows: Figure 5 As shown, from Figure 5 It can be seen that the high-rate discharge performance of the alloy changes with Figure 3 The same means that the method described in this invention is also applicable to other hydrogen storage alloys.

Claims

1. A surface treatment method for a hydrogen storage alloy, characterized in that, The A2B7 type hydrogen storage alloy powder is subjected to low-temperature heat treatment at 180-240℃; the heating rate of the low-temperature heat treatment is 5℃ / min, the holding time is 10-60min, and the cooling method is furnace cooling; the particle size of the A2B7 type hydrogen storage alloy powder is 200-400 mesh; the hydrogen storage alloy must contain Ni element, and a Ni-rich layer is formed on the surface of the heat-treated hydrogen storage alloy.

2. The surface treatment method according to claim 1, characterized in that, The mass of the hydrogen storage alloy is 2g.

3. The hydrogen storage alloy prepared by the surface treatment method according to claim 1.

4. The application of the hydrogen storage alloy treated by the surface treatment method according to claim 1 in the negative electrode material of nickel-metal hydride batteries.

5. A method for preparing a hydrogen storage alloy electrode, characterized in that, Includes the following steps: The hydrogen storage alloy treated by the surface treatment method described in claim 1 is mixed with Ni powder at a mass ratio of 1:4, cold-pressed into an electrode sheet under a pressure of 20 MPa, coated in a nickel foam substrate, and spot-welded with nickel strips to form a hydrogen storage alloy electrode.

Citation Information

Patent Citations

  • Hydrogen storage alloy electrode

    JP1995320729A