A DOPO-added flame retardant and its preparation method and application
By combining DOPO with dihydroxydiphenylsulfone, DOPO-BPS flame retardant containing phosphorus sulfur was prepared, which solved the problem of poor compatibility of flame retardant in epoxy resin, and achieved efficient flame retardant and high transparency. At the same time, the synthesis process is simplified.
Patent Information
- Application Number
- CN202311286271.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-10-07
AI Technical Summary
The existing flame retardant in epoxy resins has reduced flame retardant efficiency and mechanical properties, and has complex light transmittance and synthesis process.
By reacting DOPO with dihydroxydiphenylsulfone, a DOPO-BPS containing phosphorus sulfur is prepared. The flame retardant can maintain the high flame retardant ability of the epoxy resin under low additive amounts and Mechanical properties and maintain high transparency.
It has achieved the improvement of the flame retardant properties and mechanical properties of epoxy resin at low addition amounts, while maintaining high transparency, solving the problems of poor compatibility, reduced light transmittance and complex synthesis processes in the existing flame retardant.
Smart Images

Figure CN117186153B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardants, and specifically relates to a DOPO-added flame retardant and a preparation method and application thereof. Background Art
[0002] As a kind of thermosetting plastic, epoxy resin has many advantages and is widely used, but it is flammable, so flame retardants must be used to retard epoxy resin.
[0003] Phosphorus-containing flame retardants have been widely studied due to their good flame retardant effect and non-toxic characteristics. Although inorganic phosphorus flame retardants can provide flame retardant ability in epoxy resin, due to poor compatibility with epoxy resin, the flame retardant efficiency is reduced and the mechanical properties are greatly reduced, which is unacceptable in actual life and production. Therefore, the organic phosphorus flame retardant DOPO has attracted people's attention. Although DOPO flame retardant can provide flame retardant ability in epoxy resin, the reaction between DOPO and epoxy resin will destroy the crosslinking degree of epoxy resin, resulting in poor mechanical properties. Although reactive DOPO can solve the problem of mechanical properties to a certain extent, the production process of reactive DOPO flame retardant is usually complicated and not conducive to large-scale production. At present, it is only used in laboratory experiments, and the transmittance is also significantly reduced. Additive DOPO flame retardant can be well applied to production and has broad application prospects, but the existing additive DOPO flame retardant often requires a higher addition amount, and high addition amount will lead to poor mechanical properties and poor compatibility.
[0004] Therefore, it is necessary to design a new additive flame retardant that can maintain the high flame retardancy and mechanical properties of epoxy resin at a lower addition amount, and has the characteristics of high transparency, so that it can be used in other ways. Summary of the invention
[0005] The object of the present invention is to provide a DOPO-added flame retardant and a preparation method and application thereof, so as to solve the problems mentioned in the background technology that although the existing flame retardants can provide flame retardancy in epoxy resin, the flame retardant efficiency is reduced due to the poor compatibility between the existing flame retardants and the epoxy resin, and the mechanical properties of the epoxy resin containing the flame retardant are greatly reduced, and the transmittance is also reduced, and the existing flame retardants have high phosphorus content and complex synthesis process.
[0006] To achieve the above object, the present invention provides a DOPO additive flame retardant, the structural formula of which is
[0007] Abbreviated as DOPO-BPS.
[0008] The preparation method of a DOPO-added flame retardant according to the present invention comprises the following specific steps:
[0009] S1. Weigh DOPO into a container, add solvent, and stir to mix evenly;
[0010] S2, adding 4,4'-dihydroxydiphenyl sulfone and triethylamine into a container, and stirring evenly under a stirrer;
[0011] S3, adding carbon tetrachloride dropwise into the container under stirring, and controlling the temperature within 10°C during the adding process;
[0012] S4, react at room temperature for 8 to 12 hours;
[0013] S5, extracting and washing the reaction solution with hydrochloric acid, sodium bicarbonate, and deionized water in sequence to obtain a lower layer of viscous liquid;
[0014] S6. The separated lower layer of viscous liquid is subjected to reduced pressure distillation to remove the solvent in the reaction, thereby obtaining the product DOPO-BPS which is precipitated and then dried in vacuum.
[0015] In a specific embodiment, in S2, the molar ratio of 4,4'-dihydroxydiphenyl sulfone to DOPO is 1:1.8-2.2, and the molar ratio of triethylamine to DOPO is 1:0.8-1.2; in S3, the molar ratio of carbon tetrachloride to DOPO is 1:0.8-1.2.
[0016] In a specific embodiment, the molar ratio of 4,4'-dihydroxydiphenyl sulfone, DOPO, carbon tetrachloride and triethylamine is 1:2:2:2.
[0017] In a specific embodiment, the solvent is one or more of dichloromethane, ethyl acetate, acetonitrile, tetrahydrofuran, and chloroform.
[0018] In a specific embodiment, the amount of the solvent is 3 to 8 times the mass of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0019] In a specific embodiment, in S5, the concentration of hydrochloric acid used for extraction and washing is 0.05-0.15 mol / L, and the concentration of sodium bicarbonate used for extraction and washing is 0.05-0.15 mol / L; hydrochloric acid, sodium bicarbonate, and deionized water are used for extraction and washing 2-3 times each.
[0020] In a specific embodiment, the stirrer is a heat-collecting magnetic stirrer; in S3, a constant pressure dropping funnel is used for dropping.
[0021] The invention discloses an application of a DOPO-added flame retardant in the preparation of epoxy resin.
[0022] In a specific embodiment, the epoxy resin and DOPO-BPS are stirred at 80-110° C. to obtain a uniform solution, cooled to 80-90° C., 4,4'-diaminodiphenylmethane is added and stirred until transparent, poured into a mold, first vacuum dried at 110-130° C. for 2-3 hours, and then vacuum dried at 140-160° C. for 3-5 hours.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention uses the core structure of dihydroxydiphenyl sulfone and DOPO to synthesize and prepare a phosphorus-sulfur DOPO-added flame retardant, which solves the technical problems of poor flame retardancy, high phosphorus content and complex synthesis process of existing flame retardants. The flame retardant of the present invention has good flame retardant effect, low smoke, non-toxicity, high thermal stability and maintains a small change in the light transmittance of the resin matrix.
[0025] The flame retardant of the invention has good compatibility with epoxy resin, can keep the light transmittance of epoxy resin small while maintaining high chemical and thermal stability.
[0026] The present invention combines DOPO with dihydroxydiphenyl sulfone for reaction. The molecular structure contains phosphorus and sulfur elements for synergistic flame retardancy. The phosphorus and sulfur elements can promote the formation of a carbon layer. PO and P=O of DOPO have a gas phase flame retardant effect. The synergistic effect overcomes the shortcomings of a single flame retardant element, improves heat resistance and high-temperature carbonization rate, and can make the epoxy resin reach LOI32.1% and UL94V-0 level when the phosphorus content is only 0.63%.
[0027] Due to the color fixing effect of dihydroxydiphenyl sulfone, the flame retardant of the present invention does not change the light transmittance of the epoxy resin itself after being added to the epoxy resin, and still maintains high transparency, which provides more options for the application of the epoxy resin.
[0028] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0030] Figure 1 This is the FTIR spectrum of a DOPO-added flame retardant of the present invention;
[0031] Figure 2It is a DOPO added flame retardant of the present invention. 31 P NMR spectrum;
[0032] Figure 3 It is a DOPO added flame retardant of the present invention. 1 H NMR spectrum;
[0033] Figure 4 is a comparison chart of ultraviolet spectrophotometry of epoxy resins containing different DOPO-BPS contents of the present invention;
[0034] Figure 5 is a comparison chart of the total smoke generation of epoxy resins containing different DOPO-BPS contents of the present invention;
[0035] Figure 6 is a comparison chart of the total heat release of epoxy resins containing different DOPO-BPS contents of the present invention;
[0036] Figure 7 is a comparison chart of heat release rates of epoxy resins containing different DOPO-BPS contents of the present invention;
[0037] Figure 8 It is a comparison chart of the carbon residue rates of epoxy resins containing different DOPO-BPS contents of the present invention. DETAILED DESCRIPTION
[0038] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0039] Example 1
[0040] Take 8.64g of DOPO and dissolve it in a 250ml three-necked flask filled with dichloromethane, add a magnet to the three-necked flask, place the three-necked flask in a heat-collecting magnetic stirrer, add ice cubes, control the temperature within 10°C, and stir for 10 minutes; weigh 6g of 4,4'-dihydroxydiphenyl sulfone and 7.38g of triethylamine, dissolve them in the above three-necked flask, weigh 4.85g of carbon tetrachloride and add it dropwise to the three-necked flask through a constant pressure dropping funnel, and control the temperature within 10°C. After the addition was completed, the temperature of the heat-collecting magnetic stirrer was raised to room temperature, and the reaction time was 12 hours; the product solution after the reaction was loaded into a separatory funnel, and extracted and washed with 0.1 mol / L dilute hydrochloric acid, 0.1 mol / L sodium bicarbonate, and deionized water, respectively. After extraction and washing, the lower layer of viscous liquid obtained by separation was distilled under reduced pressure to recover the dichloromethane in the reaction, the reaction was stopped, and the reaction solution was vacuum dried to obtain the target compound DOPO-BPS as a milky white solid with a yield of 83.2%.
[0041] Infrared spectrum analysis results of compound DOPO-BPS: FT-IR (KBr), v / cm -1 : 1583, 1476 and 1425cm -1 The absorption peak is attributed to the bending vibration of the benzene ring, and its intensity is enhanced due to the conjugation with the S=O structure. -1 With 1149cm -1 The corresponding S=O bond stretching vibration is at 909cm -1 A new characteristic absorption peak attributed to the PO bond also appears at Figure 1 The change of characteristic absorption peaks in the FTIR spectrum shown preliminarily confirmed the successful synthesis of the target product.
[0042] like Figure 2 As shown in the figure, in DOPO-BPS 31 In the P NMR spectrum, a chemical shift peak at 6.92ppm can be observed, indicating that a new chemical environment of P element appears in the synthesized DOPO-BPS. The NMR spectrum further confirms that the product synthesized in this experiment is consistent with the target product. Among them, 14.03ppm and 17.83ppm are the P element peaks of DOPO.
[0043] like Figure 3 As shown in the figure, in DOPO-BPS 1 In the H NMR spectrum, it can be observed that there are 24 H atoms in the region of the H peak, which is the same as the number of hydrogen atoms contained in the DOPO-BPS compound, proving that the synthesized product is consistent with the target product.
[0044] The invention discloses an application of a DOPO-added flame retardant in the preparation of epoxy resin.
[0045] The epoxy resin and DOPO-BPS are stirred at 80-110°C to obtain a uniform solution, then cooled to 80-90°C, 4,4'-diaminodiphenylmethane is added and stirred until transparent, poured into a mold, first vacuum dried at 110-130°C for 2-3 hours, and then vacuum dried at 140-160°C for 3-5 hours to obtain an epoxy resin containing DOPO-BPS.
[0046] Comparison of epoxy resins with different DOPO-BPS contents:
[0047] 1) Epoxy resin without DOPO-BPS:
[0048] In terms of flame retardancy, the UL94 fireproof grade is not passed (NR); the LOI value is only 24.9%; the peak heat release rate (PHRR) is 899.3kW / m 2 ; Total heat release (THR) is 68.7MJ / m2 ; Total smoke production (TSP) is 38.9m 2 ; The residual carbon rate is 6.58%.
[0049] In terms of mechanical properties, the glass transition temperature is 131.9°C.
[0050] In terms of light transmission effect, the transmittance is 94.1%.
[0051] 2) Epoxy resin containing 3 wt% DOPO-BPS:
[0052] In terms of flame retardancy, the UL94 fire rating is not passed (NR); the LOI value is 29.7%; the peak heat release rate (PHRR) is 826kW / m 2 ; Total heat release (THR) is 53.3MJ / m 2 ; Total smoke production (TSP) is 27.1m 2 ; The residual carbon rate is 16.96%.
[0053] In terms of mechanical properties, the glass transition temperature is 135.5°C, which is 3.6°C higher than that of epoxy resin without addition.
[0054] In terms of light transmission effect, the transmittance is 90.4%.
[0055] 3) Epoxy resin containing 5 wt% DOPO-BPS:
[0056] In terms of flame retardancy, the UL94 fire rating is V-1; the LOI value is 30.9%; the peak heat release rate (PHRR) is 705.4kW / m 2 ; Total heat release (THR) is 50.9MJ / m 2 ; Total smoke production (TSP) is 28.2m 2 ; The residual carbon rate is 17.01%.
[0057] In terms of mechanical properties, the glass transition temperature is 142.2°C, which is 10.3°C higher than that of epoxy resin without addition.
[0058] In terms of light transmission effect, the transmittance is 89.1%.
[0059] 4) Epoxy resin containing 7 wt% of DOPO-BPS:
[0060] In terms of flame retardancy, the UL94 fire rating is V-0; the LOI value is 32.1%; the peak heat release rate (PHRR) is 592.3kW / m 2 ; Total heat release (THR) is 47MJ / m 2 ; Total smoke production (TSP) is 28.2m 2; The residual carbon rate is 18.89%.
[0061] In terms of mechanical properties, the glass transition temperature is 158.2°C, which is 26.3°C higher than that of epoxy resin without addition.
[0062] In terms of light transmission effect, the transmittance is 88.5%.
[0063] By comparison, the flame retardant performance is significantly improved, the mechanical properties are also improved, and the light transmittance effect is not greatly reduced.
[0064] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. Application of a DOPO additive flame retardant in the preparation of epoxy resin, characterized in that: The structural formula of the DOPO added flame retardant is Abbreviated as DOPO-BPS; The epoxy resin is an epoxy resin containing 5 wt% of DOPO-BPS or an epoxy resin containing 7 wt% of DOPO-BPS.
2. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 1, characterized in that: Stir the epoxy resin and DOPO-BPS at 80-110°C to obtain a uniform solution, cool to 80-90°C, add 4,4'-diaminodiphenylmethane and stir until transparent, pour into a mold, first vacuum dry at 110-130°C for 2-3 hours, and then vacuum dry at 140-160°C for 3-5 hours.
3. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 1, characterized in that: The specific steps of the preparation method of the DOPO added flame retardant are as follows: S1. Weigh DOPO into a container, add solvent, and stir to mix evenly; S2, adding 4,4'-dihydroxydiphenyl sulfone and triethylamine into a container, and stirring evenly under a stirrer; S3, adding carbon tetrachloride dropwise into the container under stirring, and controlling the temperature within 10°C during the adding process; S4, react at room temperature for 8 to 12 hours; S5, extracting and washing the reaction solution with hydrochloric acid, sodium bicarbonate, and deionized water in sequence to obtain a lower layer of viscous liquid; S6. The separated lower layer of viscous liquid is subjected to reduced pressure distillation to remove the solvent in the reaction, thereby obtaining the product DOPO-BPS which is precipitated and then dried in vacuum.
4. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 3, characterized in that: In the S2, the molar ratio of 4,4'-dihydroxydiphenyl sulfone to DOPO is 1:1.8-2.2, and the molar ratio of triethylamine to DOPO is 1:0.8-1.2; in the S3, the molar ratio of carbon tetrachloride to DOPO is 1:0.8-1.
2.
5. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 4, characterized in that: The molar ratio of the 4,4'-dihydroxydiphenyl sulfone, DOPO, carbon tetrachloride and triethylamine is 1:2:2:
2.
6. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 3, characterized in that: The solvent is one or more of dichloromethane, ethyl acetate, acetonitrile, tetrahydrofuran and chloroform.
7. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 3, characterized in that: The mass of the solvent used is 3 to 8 times the mass of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
8. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 3, characterized in that: In S5, the concentration of hydrochloric acid used for extraction and washing is 0.05-0.15 mol / L, and the concentration of sodium bicarbonate used for extraction and washing is 0.05-0.15 mol / L; the extraction and washing are performed 2-3 times with hydrochloric acid, sodium bicarbonate and deionized water respectively.
9. The use of a DOPO added flame retardant in the preparation of epoxy resin according to claim 3, characterized in that: The stirrer is a heat-collecting magnetic stirrer; in S3, a constant pressure dropping funnel is used for dropwise addition.
Citation Information
Patent Citations
Phosphorus / nitrogen / sulfur-containing flame retardant and preparation method thereof
CN105733024A
Sulfur-nitrogen-phosphorus synergistic flame-retardant resin composition, thermosetting resin composition, presoaked plate and composite metal substrate
CN107641291A
Benzene sulfone compound nitrogen phosphorus sulfur ternary synergistic flame retardants containing double DOPOs and preparation method and application thereof
CN110128702A
Novel organic phosphorus flame retardant and preparation method thereof
CN110669074A
Resin composition, and prepreg and copper-clad laminate using same
CN114634708A