A high-strength steel plate for pressurized water reactor nuclear power plant support and a manufacturing method thereof
A high-strength steel plate with optimized chemical composition and manufacturing process addresses cleanliness and mechanical performance issues, ensuring high-temperature and low-temperature strength for nuclear reactor supports, enhancing structural reliability and reducing production costs.
Patent Information
- Application Number
- CN202311083389.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-08-25
AI Technical Summary
Conventional high-strength steel plates for nuclear reactor supports lack sufficient cleanliness, uniformity, and meet insufficient mechanical performance requirements under tempering and simulated post-weld heat treatment conditions, particularly in terms of low-temperature and high-temperature strength.
A high-strength steel plate with specific chemical composition (C: 0.10-0.15%, Si: 0.15-0.30%, Mn: 1.15-1.40%, Ni: 1.30-1.40%, Mo: 0.65-0.85%, Al: 0.03-0.045%, Nb: 0.03-0.05%, Cu: 0.001-0.020%, V: 0.001-0.020%, controlled impurities) and a manufacturing process involving LF refining, RH refining, continuous casting, electroslag remelting, rolling, and quenching and tempering heat treatment to ensure purity and uniformity.
The steel plate achieves yield strength ≥450 MPa, tensile strength 535 to 615 MPa, -40°C low-temperature impact toughness ≥100 J, and 200°C high-temperature tensile yield strength ≥450 MPa, meeting the stringent requirements for nuclear reactor support structures with improved reliability and reduced production costs.
Smart Images

Figure BDA0004415442330000071 
Figure BDA0004415442330000081 
Figure BDA0004415442330000082
Abstract
Description
Technical Field
[0001] The invention relates to a ferrous metal material, in particular to a high-strength steel plate for supporting a 450MPa-level pressurized water reactor nuclear power plant and a manufacturing method thereof. Background Art
[0002] The support parts of pressurized water reactor nuclear power plants are welded from low-alloy high-strength steel, which play a supporting and fixing role for the nuclear reactor pressure vessel. Its service life is not only related to the working environment, but also closely related to the quality of its structure itself. The pressure vessel support of pressurized water reactor nuclear power plants faces extremely harsh environments during use. While bearing dynamic and static loads, it is also affected by radiation, so the dimensional stability and reliability of its support structure must be ensured.
[0003] The relevant patents for steel used in nuclear reactor supports currently produced are as follows:
[0004] The patent applied for by Jigang Group Co., Ltd. is titled "A high-strength and tough steel plate for nuclear power plant mechanical module support and its manufacturing method", with patent application number 201310083274.7 and publication number CN 102766805A, C: 0.08-0.22%, Si: 0.15-0.45%, Mn: 0.60-1.10%, P≤0.020%, S≤0.015%, Ni: 0.60~1.00%, Cr: 0.40~0.70%, Mo: 0.40~0.60%, Cu: 0.15~0.55%, V: 0.020~0.080%, Ti: 0.008~0.030%, B: 0.0005~0.005%, Alt: 0.020~0.050%, and the remainder is iron and impurities. The steel plate for nuclear power plant support described in the invention has high strength and high toughness, and both the base material and the heat-affected zone have good impact toughness at low temperatures. However, the maximum thickness of the steel plate in the claims of the reference document is 65 mm, and the specification does not provide a 200°C high-temperature tensile index.
[0005] Wuyang Iron and Steel Co., Ltd. applied for a patent named "High-strength and low-hardness 15MnNi steel plate for nuclear power equipment and its production method", with patent application number 201710780614.X and publication number CN107699819A, C: 0.15~0.17%, Si: 0.23~0.26%, Mn: 1.57~1.64%, P≤0.012%, S≤0.005%, Cr: 0.04~0.06%, Mo: 0.007~0.010%, Cu≤0.010%, Ni: 0.52~0.57%, V: 0.001~0.003%, Nb: 0.001~0.002%, Ti: 0.014~0.017%, and the balance is Fe and unavoidable impurities. The steel plate manufactured by the method of the invention has a room temperature yield strength of more than 450 MPa and high temperature resistance of 200° C. However, the ingot rolling production method adopted by the invention has a low yield rate, poor head-to-tail uniformity, and unstable internal quality of the steel plate.
[0006] Wuyang Iron and Steel Co., Ltd. applied for a patent for a heat treatment method of a steel plate for supporting a normalizing nuclear power pressure vessel equipment. The patent application number is 201910280879.2 and the publication number is CN 110117705A. The steel plate contains by weight: C: 0.16-0.19%, Si: 0.10-0.20%, Mn: 1.45-1.55%, P: 0.007-0.011%, S: 0.0010-0.0018%, N: 0.0048-0.0055%, Cu: 0.08-0.14%, V: 0.060-0.070%, and the rest is Fe and unavoidable impurity elements. The steel plate is composed of bainite + ferrite, and the normalizing holding temperature, total heating time and cooling back to red temperature are optimized and adjusted to make the strength and toughness of the steel plate match reasonably and have excellent comprehensive performance. However, the invention specification does not provide the mechanical performance indicators after die welding.
[0007] Therefore, the key indicators of the new generation of high-strength steel plates used for the support of pressurized water reactor nuclear power plants are the following three aspects: first, strict requirements are placed on the cleanliness and uniformity of the steel plates; second, the steel plates should have a sufficient margin of Charpy impact absorption energy under extreme service conditions (-40°C) after tempering treatment and simulated post-weld heat treatment; third, the steel plates need to have good room temperature and high temperature tensile properties both under tempering treatment and simulated post-weld heat treatment. Summary of the invention
[0008] The purpose of the present invention is to provide a high-strength steel plate for support of a pressurized water reactor nuclear power plant, so as to solve the problem that the cleanliness, uniformity and low-temperature, normal-temperature and high-temperature strength of conventional high-strength steel plates for support of nuclear reactors need to be improved under the conditions of tempering treatment and simulated post-weld heat treatment.
[0009] In addition, the present invention also provides a method for manufacturing the high-strength steel plate for supporting a pressurized water reactor nuclear power plant.
[0010] In the first aspect, the high-strength steel plate for supporting a pressurized water reactor nuclear power plant according to the present invention has the following chemical composition in terms of mass percentage:
[0011] C: 0.10-0.15%; Si: 0.15-0.30%; Mn: 1.15-1.40%; P≤0.015%; S≤0.005%;
[0012] Ni: 1.30-1.40%; Mo: 0.65-0.85%; Al: 0.03-0.045%; Nb: 0.03-0.05%; Cu: 0.001-0.020%; V: 0.001-0.020%; the rest is Fe and inevitable impurities.
[0013] The design reasons for the present invention using the above chemical components and contents are as follows:
[0014] (1) C: As the C content in steel increases, the hardness and strength of the steel increase, while the toughness and plasticity decrease. At the same time, too high a carbon content affects the weldability of the steel plate; C, as an interstitial element, increases the tendency of radiation embrittlement. Therefore, the present invention requires that the C content in the steel should be controlled within the range of 0.10-0.15%.
[0015] (2) Si: Si dissolved in ferrite and austenite can improve the hardness and strength of steel. However, too high Si content will damage the plasticity and toughness of the steel plate and reduce the welding performance of the steel. At the same time, high Si content has the effect of stabilizing radiation defects. Therefore, the present invention requires that the Si content in the steel be controlled at 0.15-0.30%.
[0016] (3) Mn: Mn can strengthen ferrite and has a significant solid solution strengthening effect. It can effectively improve the hardenability of steel and increase the yield point, but Mn has a tendency to increase radiation catalysis. Therefore, the Mn content in steel is required to be controlled within the range of 1.15-1.40%.
[0017] (4) Ni: Ni reduces the resistance of dislocation movement in steel, relaxes stress, and further changes the substructure of the matrix organization, thereby improving the low-temperature toughness of the steel plate. However, Ni has a tendency to increase radiation catalysis. Therefore, the present invention requires that the Ni content in the steel be controlled to 1.30-1.40%.
[0018] (5) Mo: In quenched and tempered steel, Mo can improve hardenability, prevent temper brittleness, ensure that the steel plate is tempered at a higher temperature, and thus improve plasticity; at the same time, Mo significantly improves the bonding force between atoms in the solid solution and improves the thermal strength of the steel; more importantly, Mo effectively inhibits the segregation of harmful elements in the steel. Therefore, the present invention requires that the Mo content in the steel be controlled to be 0.65-0.85%.
[0019] (7) Al: Al is an effective element for adjusting the grain size of steel. It combines with an appropriate amount of N to form small particles with a high melting point, which has the effect of refining the grains. However, Al has little effect on the hardenability of steel. Therefore, the present invention requires that the Al content in the steel be controlled to be 0.03-0.045%.
[0020] (8) Nb: Nb can increase the yield strength of steel, reduce the brittle transition temperature, and is beneficial to the welding performance of steel. At the same time, Nb has poor sensitivity to radiation. Therefore, the present invention requires that the Nb content of steel be controlled to 0.03-0.05%.
[0021] (9) P: P is a harmful element that increases the brittleness of steel, significantly increases the yield point and yield strength ratio, deteriorates plasticity and toughness, and has an adverse effect on welding. At the same time, irradiation tests show that P is also very sensitive to irradiation embrittlement. Therefore, the lower the P content in the steel, the better. The present invention requires it to be less than 0.015%.
[0022] (10) S: S forms FeS and MnS sulfides at the austenite grain boundaries in steel, which will reduce the impact toughness and welding performance of the steel. At the same time, S also tends to accelerate radiation embrittlement. Therefore, the S content in steel should be limited to less than 0.005%.
[0023] (11) Cu: Too high a Cu content is not conducive to steel plate processing and welding. Cu is also the most harmful element to radiation embrittlement. Therefore, the Cu content in steel should be less than 0.020%.
[0024] (12) V: Although the addition of V can improve the room temperature and high temperature strength of steel by solid solution strengthening to pin dislocations and refine grains, V is sensitive to radiation. Therefore, the V added to steel should be less than 0.020%.
[0025] In a second aspect, the method for manufacturing the high-strength steel plate for pressurized water reactor nuclear power plant support described in the first aspect comprises LF refining + RH refining, continuous casting, electroslag remelting, heating, rolling and quenching and tempering heat treatment steps, characterized in that:
[0026] In the LF refining + RH refining process, the LF furnace is used for refining to produce reduced white slag, thereby reducing the contents of impurity elements P and S in the steel, and controlling P≤0.015% and S≤0.005% in the steel; the vacuum cycle time of the RH vacuum refining is ≥10min, and controlling H≤1.0ppm, O≤20ppm, and N≤40ppm in the steel.
[0027] In the present disclosure and possible embodiments, in the continuous casting process, a consumable electrode welded from a continuous casting billet is used, the size of the consumable electrode is: 200-500×1150-1380×Lmm (L is the length of the consumable electrode), the cross-sectional size of the crystallizer is 185-255×1500-2060mm, and the opening degree of the crystallizer cooling water valve is 80-100%.
[0028] In the present disclosure and possible embodiments, in the electroslag remelting smelting process, when starting the arc, the arc starting block of the same steel grade is used, and the bottom plate and the arc starting block are preheated before use to remove moisture; the argon blowing system adopted is to start passing argon 5 to 10 minutes before power production, and the argon flow rate is 15-30m 3 / h for atmosphere protection; the electrical system adopted is that the current increases gradually from 6000A to 16000A, slag formation begins within 5 to 10 minutes of arc starting, and a silicon-calcium-aluminum ternary slag system is used to control the level of inclusions in the steel below level 0.5; after the consumable electrode is remelted, it is left to stand for 4 to 6 hours before demolding to obtain an electroslag billet with a thickness of 185 to 255 mm.
[0029] In the present disclosure and possible embodiments, in the heating process, the billet is fed into a walking beam heating furnace for heating, and the cast billet is sequentially treated in a preheating section, a heating section and a soaking section before being taken out of the furnace; the temperature range of the preheating section is 900 to 1100°C, the temperature range of the heating section is 1100 to 1270°C, the temperature range of the soaking section is 1190 to 1250°C, and the heating time is 2 to 3 hours.
[0030] In the present disclosure and possible embodiments, in the rolling process, the starting rolling temperature is controlled to be 1150-1190° C., the final rolling temperature is controlled to be 970-1100° C., and the rolling speed is controlled to be 3.1-4.0 m / s.
[0031] In the present disclosure and possible embodiments, in the tempering heat treatment process, the quenching temperature is controlled to be 890-910°C, and the holding time is 1-4 min / mm; the tempering temperature is: 675-695°C, and the holding time is 4-8 min / mm.
[0032] Beneficial effects of the present invention:
[0033] (1) The high-strength steel plate for pressurized water reactor nuclear power plant support of the present invention effectively improves the hardenability of the steel by adding a higher content of Mo (wt 0.65-0.85%), and at the same time improves the thermal strength of the steel, ensuring that the steel plate still has good room temperature and high temperature strength after a long period of simulated post-weld heat treatment; by increasing the trace element Nb (wt 0.03-0.05%), the effects of refining the grains, improving the thermal strength and improving the weldability are achieved;
[0034] (2) The two-stage pure steel smelting technology of continuous casting and electroslag remelting can ensure that the raw steel billet required for rolling steel plates is pure in quality and has a uniform and dense structure, laying the foundation for the production of high-quality medium and thick plate products from the source;
[0035] (3) The present invention adopts a production process of controlled rolling + quenching and tempering heat treatment to effectively control the uniformity and stability of the head and tail performance of the steel plate, ensuring that the performance of the steel plate meets the mechanical requirements;
[0036] (4) The steel plate produced by the manufacturing method of the present invention has a cost advantage. Compared with the products produced by die casting, the production cost is significantly reduced by improving the yield rate, the delivery period is shortened, and the steel plate has good processing performance on the basis of meeting the comprehensive mechanical property requirements;
[0037] (5) The steel plate prepared by the present invention has a thickness of 30 to 70 mm, and the quenched and tempered properties meet the following requirements: yield strength ≥ 450 MPa, tensile strength 535 to 615 MPa, low temperature impact toughness of -40°C ≥ 100 J, high temperature tensile yield strength of 200°C ≥ 450 MPa, and tensile strength of 200°C ≥ 500 MPa;
[0038] The simulated post-weld heat treatment state performance meets the yield strength ≥450MPa, tensile strength 515~605MPa, -40℃ low temperature impact toughness ≥150J, 200℃ high temperature tensile yield strength ≥450MPa, 200℃ tensile strength ≥500MPa. It fully meets the high quality requirements of the new generation of high-strength steel plates for nuclear reactor support, thus ensuring the stability and reliability of the size of the nuclear reactor support structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is a metallographic microstructure diagram of a steel plate according to Example 1 of the present invention;
[0040] Figure 2 This is a scanning electron microscope observation image of the steel plate fracture of Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The present disclosure is described below based on embodiments, but it is worth noting that the present disclosure is not limited to these embodiments. In the detailed description of the present disclosure below, some specific details are described in detail. However, for the parts that are not described in detail, those skilled in the art can also fully understand the present disclosure.
[0042] At the same time, unless the context clearly requires otherwise, the words "include", "comprises" and similar words throughout the specification and claims should be interpreted as inclusive rather than exclusive or exhaustive; that is, the meaning is "including but not limited to".
[0043] The following provides 6 groups of examples and 3 groups of comparative examples to explain in detail the high-strength steel plate for pressurized water reactor nuclear power plant support and the manufacturing method thereof. The chemical composition of each case steel plate is shown in Table 1 (the balance is Fe and impurities):
[0044] 1. Each embodiment carries out steelmaking according to the chemical composition and content designed in Table 1:
[0045] Table 1 Chemical composition and content (wt%) of steel plates of various embodiments and comparative examples
[0046] serial number C Si Mn P S Ni Mo Al Nb Cu V Example 1 0.11 0.19 1.35 0.005 0.001 1.35 0.75 0.030 0.042 0.02 0.005 Example 2 0.13 0.15 1.38 0.008 0.002 1.36 0.72 0.031 0.045 0.01 0.003 Example 3 0.15 0.22 1.40 0.009 0.002 1.38 0.82 0.033 0.04 0.007 0.006 Example 4 0.10 0.25 1.17 0.006 0.001 1.39 0.68 0.039 0.033 0.017 0.005 Example 5 0.11 0.24 1.15 0.01 0.004 1.32 0.67 0.045 0.035 0.015 0.002 Example 6 0.14 0.28 1.25 0.006 0.003 1.33 0.83 0.035 0.047 0.018 0.018 Comparative Example 1 0.15 0.2 1.22 0.007 0.003 1.31 0.66 0.037 0.011 0.013 0.006 Comparative Example 2 0.13 0.25 1.3 0.008 0.002 1.34 _ 0.03 0.032 0.014 0.003 Comparative Example 3 0.12 0.19 1.28 0.006 0.003 1.35 0.68 0.032 0.036 0.02 0.004
[0047] Among them, Examples 1-6 and Comparative Example 3 are all designed according to the alloy composition of the present invention, and Comparative Examples 1 and 2 do not add Nb and Mo according to the requirements of the present invention.
[0048] 2. Examples 1-6 and Comparative Examples 1-3 adopt the following manufacturing scheme:
[0049] Examples 1-6 and Comparative Examples 1-2 adopt the process flow of molten iron pretreatment - converter smelting - LF+RH refining - continuous casting - electroslag remelting - billet inspection - billet pile cooling - heating - dephosphorization - controlled rolling - quenching - tempering; Comparative Example 3 only adopts continuous casting billet smelting technology. Among them:
[0050] 1. LF+RH refining: LF furnace refining produces reduced white slag to reduce the content of impurity elements P and S in steel, controlling P≤0.015% and S≤0.005% in steel; the vacuum cycle time of RH vacuum refining is ≥10min, controlling H≤1.0ppm, O≤20ppm, and N≤40ppm in steel.
[0051] 2. Electroslag remelting smelting includes:
[0052] The consumable electrode welded from continuous casting billets is used. The size of the consumable electrode is 200-500×1150-1380×Lmm (L is the length of the consumable electrode). The cross-sectional size of the crystallizer is 185-255×1500-2060mm. The opening of the crystallizer cooling water valve is 80-100%. When starting the arc, the arc-starting block of the same steel grade is used. The bottom pad and the arc-starting block are fully preheated before use to remove moisture. Argon blowing system: argon gas is started 5-10 minutes before power production, and the argon gas flow rate is 15-30m 3 / h, for atmosphere protection. Electrical system: the current is gradually increased from 6000A to 16000A, slag formation begins within 5 to 10 minutes of arcing, and the silicon-calcium-aluminum ternary slag system is used to control the level of inclusions in the steel below 0.5. After the consumable electrode is remelted, it is left to stand for 4 to 6 hours before demoulding to obtain an electroslag billet with a thickness of 185 to 255 mm.
[0053] 3. Heating: The billet is sent into a walking beam heating furnace for heating. The billet is sequentially treated in the preheating section, heating section and soaking section before being taken out of the furnace. The temperature range of the preheating section is 900-1100°C, the temperature range of the heating section is 1100-1270°C, the temperature range of the soaking section is 1190-1250°C, and the heating time is 2-3 hours.
[0054] 4. Rolling: Control the starting rolling temperature to 1150-1190°C, the final rolling temperature to 970-1100°C, and the rolling speed to 3.1-4.0 m / s. The rolling processes of the relevant embodiments and comparative examples are shown in Table 2:
[0055] Table 2 Rolling process
[0056]
[0057] 5. Quenching and tempering heat treatment: After rolling, the steel plate is subjected to a quenching and tempering heat treatment process to obtain a delicate and uniform bainite tempering structure, and to give the steel plate good comprehensive mechanical properties. In order to give full play to the role of alloying elements such as Ni, Mo, Nb in the steel, and at the same time combine other chemical components and rolling process characteristics to make the structure after rolling completely austenitized and fully tempered; the present invention adopts the following quenching and tempering heat treatment system according to different thickness characteristics: the quenching temperature is 890-910°C, and the holding time is 1 to 4 min / mm; the tempering temperature is: 675-695°C, and the holding time is 4 to 8 min / mm. The heat treatment system of Examples 1-6 and Comparative Examples 1-3 is shown in Table 3:
[0058] Table 3 Heat treatment system
[0059] serial number Quenching temperature / ℃ Insulation time / min Tempering temperature / ℃ Insulation time / min Example 1 896 1.5 682 4.6 Example 2 910 2 689 5.0 Example 3 891 1.8 695 4.1 Example 4 904 2.2 677 5.5 Example 5 903 3.5 679 6.5 Example 6 906 3.8 676 7.8 Comparative Example 1 899 1.2 692 7.3 Comparative Example 2 904 2.5 683 4.6 Comparative Example 3 905 3.3 695 4.2
[0060] 3. Mechanical properties of steel plates of Examples 1-6 and Comparative Examples 1-3:
[0061] Table 4 Mechanical properties of steel plates
[0062]
[0063] Note: Simulated post-weld heat treatment process: temperature: 610℃, heating and cooling rate: above 400℃, heating and cooling rate ≤70℃ / h, holding time: 16h.
[0064] IV. The tissue purity data of each embodiment is shown in Table 5:
[0065] Table 5 Steel structure purity data
[0066]
[0067]
[0068] As can be seen from Table 4 above, the steel plates of Examples 1-6 have excellent matching of strength and toughness, and a large margin of low-temperature impact toughness. In Comparative Example 1, since the Nb content does not meet the requirements, it has a great impact on the yield strength, and the low-temperature toughness is also seriously reduced. Comparative Example 2 does not contain the Mo element, resulting in poor hardenability and tempering stability, and a significant decrease in strength and impact toughness. In Comparative Example 3, the electroslag remelting technology is not used, the homogeneity of the billet is reduced, the purity of the steel plate is not high, and the low-temperature toughness is poor.
[0069] In addition, the steel plate of Example 1 was inspected and observed. Figure 1 As shown in the figure, the matrix structure of the steel plate is a tempered bainite structure, and the bainite structure is in the form of laths or needles. Figure 2 The scanning electron microscope observation of the impact fracture shown in the figure found that the entire fracture was composed of dimples of varying sizes, which is a ductile fracture, indicating that the steel plate has good impact toughness.
[0070] Therefore, the present invention adopts the production process of controlled rolling + tempering heat treatment to effectively control the uniformity and stability of the head and tail performance of the steel plate, ensuring that the performance of the steel plate meets the mechanical requirements.
[0071] The steel plate produced by the manufacturing method of the present invention has a thickness of 30 to 70 mm and has excellent low-temperature toughness index through chemical composition optimization and reasonable design of process parameters. The steel plate quenched and tempered state performance meets the yield strength ≥450MPa, tensile strength 535 to 615MPa, -40°C low-temperature impact toughness ≥100J, 200°C high-temperature tensile yield strength ≥450MPa, 200°C tensile strength ≥500MPa. The simulated post-weld heat treatment state performance meets the yield strength ≥450MPa, tensile strength 515 to 605MPa, -40°C low-temperature impact toughness ≥150J, 200°C high-temperature tensile yield strength ≥450MPa, 200°C tensile strength ≥500MPa. It fully meets the high quality requirements of the new generation of high-strength steel plates for nuclear reactor supports, thereby ensuring the stability and reliability of the size of the nuclear reactor support structure.
[0072] The steel plate produced by the manufacturing method of the present invention has cost advantages. Compared with the products produced by die casting, the production cost is significantly reduced and the delivery time is shortened mainly by improving the yield rate. On the basis of meeting the comprehensive mechanical property requirements, the steel plate has good processing performance.
[0073] The above-described embodiments are only embodiments of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the present disclosure. It should be noted that, for a person of ordinary skill in the art, without departing from the concept of the present disclosure, several variations, equivalent substitutions, improvements, etc. may be made, all of which fall within the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure shall be subject to the attached claims.
Claims
1. A high-strength steel plate for support of a pressurized water reactor nuclear power plant, characterized in that: Its chemical composition by mass percentage is: C: 0.10-0.15%; Si: 0.15-0.30%; Mn: 1.15-1.40%; P≤0.015%; S≤0.005%; Ni: 1.30-1.40%; Mo: 0.65-0.85%; Al: 0.03-0.045%; Nb: 0.03-0.05%; Cu: 0.001-0.020%; V: 0.001-0.020%; the rest is Fe and unavoidable impurities; The method for manufacturing the high-strength steel plate comprises continuous casting, electroslag remelting, rolling and quenching and tempering heat treatment processes; In the continuous casting process, a consumable electrode welded by continuous casting billets is used, the size of the consumable electrode is 200-500×1150-1380×Lmm, L is the length of the consumable electrode, the cross-sectional size of the crystallizer is 185-255×1500-2060mm, and the opening degree of the crystallizer cooling water valve is 80-100%; In the electroslag remelting smelting process, when starting the arc, the arc starting block of the same steel grade is used, and the bottom plate and the arc starting block are preheated before use to remove moisture; the argon blowing system adopted is to start passing argon 5 to 10 minutes before power production, and the argon flow rate is 15-30m 3 / h for atmosphere protection; the electrical system adopted is that the current is gradually increased from 6000A to 16000A, slag formation begins within 5 to 10 minutes of arcing, and a silicon-calcium-aluminum ternary slag system is used to control the level of inclusions in the steel below level 0.5; after the consumable electrode is remelted, it is left to stand for 4 to 6 hours before demoulding treatment to obtain an electroslag billet with a thickness of 185 to 255 mm; In the rolling process, the starting rolling temperature is controlled to be 1150-1190°C, the final rolling temperature is controlled to be 970-1100°C, and the rolling speed is controlled to be 3.1-4.0 m / s; In the tempering heat treatment process, the quenching temperature is controlled to be 890-910°C, and the holding time is 1-4 min / mm; the tempering temperature is: 675-695°C, and the holding time is 4-8 min / mm.
2. The method for producing a high-strength steel sheet according to claim 1, comprising LF refining + RH refining and heating steps, characterized in that: In the LF refining + RH refining process, the LF furnace is used for refining to produce reduced white slag, thereby reducing the contents of impurity elements P and S in the steel, and controlling P≤0.015% and S≤0.005% in the steel; the vacuum cycle time of the RH vacuum refining is ≥10min, and controlling H≤1.0ppm, O≤20ppm, and N≤40ppm in the steel.
3. The method for manufacturing a high-strength steel plate according to claim 2, characterized in that: In the heating process, the billet is sent to a walking beam heating furnace for heating, and the cast billet is sequentially treated in a preheating section, a heating section and a soaking section before being taken out of the furnace; the temperature range of the preheating section is 900 to 1100°C, the temperature range of the heating section is 1100 to 1270°C, the temperature range of the soaking section is 1190 to 1250°C, and the heating time is 2 to 3 hours.
Citation Information
Patent Citations
Thick steel plate for nuclear power plant containment and manufacture method thereof
CN102766805A
High-toughness steel plate for mechanical module supporting member of nuclear power plant and manufacturing method of steel plate
CN103114254A
High-strength and low-hardness 15MnNi steel plate for nuclear power equipment and production method of high-strength and low-hardness 15MnNi steel plate
CN107699819A
Heat treatment method for normalizing type nuclear power pressure vessel equipment bearing steel plate
CN110117705A
Manufacture method for manufacturing cantilever steel pipe with high strength and high toughness by using hot-rolling coiled plate
CN101603156A