A battery positive electrode lead paste and preparation method thereof and storage battery

By generating PbO2(cn)-Pb-MOF precursor in a mixed solvent of lead ion salt, potassium permanganate and sodium hydroxide, forming a porous composite material in an autoclave, and then carbonizing it in an oxygen-containing gas, the solution It solves the problem that the active material of the positive electrode paste is easy to fall off, and improves the performance and life of the lead-acid battery.

CN117219768BActive Publication Date: 2024-10-29GUANGZHO ADDENDA CHEM CORP LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311050669.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-21
Publication Date
2024-10-29
Estimated Expiration
2043-08-21

AI Technical Summary

Technical Problem

In the prior art, the active material of the positive electrode lead paste is easy to fall off during the charging and discharging process, resulting in a decrease in battery performance.

Method used

A method for preparing battery positive electrode lead paste is adopted. The PbO2(cn)-Pb-MOF precursor is generated by reacting in a mixed solvent of lead ion salt, potassium permanganate and sodium hydroxide, and the high-temperature reaction is carried out in an autoclave. A porous PbO2-Pb-MOF composite material is formed, which is then carbonized in an oxygen-containing gas to generate a carbonized PbO2-Pb-MOF composite material to improve structural stability and conductivity.

Benefits of technology

This method allows lead dioxide to be generated or consumed preferentially in the carbonized MOF pores, reduces the shedding of active materials, extends the service life of the positive electrode paste, and improves the discharge capacity and cycle life of lead-acid batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004404184300000051
    Figure BDA0004404184300000051
Patent Text Reader

Abstract

The invention discloses a positive lead paste for a battery, a preparation method thereof and a storage battery, and belongs to the technical field of storage batteries. It includes dissolving lead ion salt, potassium permanganate, sodium hydroxide and an organic ligand in a mixed solvent of water and ethanol, stirring the solution until uniform, reacting the mixed solution at a temperature of 70°C to 90°C for no more than 10 minutes; transferring the dispersion to a 200mL polytetrafluoroethylene autoclave, sealing and placing it in an oven at 100°C to 120°C to react and prepare a PbO2(cn)-Pb-MOF composite material; continuing to grow lead dioxide to prepare a PbO2-Pb-MOF composite material, and then carbonizing to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 250°C to 300°C; mixing the carbonized PbO2-Pb-MOF composite material, lead powder, SnSO4, polyester staple fiber, sulfuric acid and pure water to obtain the positive lead paste. The invention can reduce the shedding of active materials and the service life of positive lead paste, and can improve the discharge capacity and cycle life of the battery plates in a lead-acid battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of storage batteries, and more specifically, relates to a battery positive electrode lead paste and a preparation method thereof, and a storage battery. Background Art

[0002] Lead-acid battery is a storage battery with lead and lead dioxide as electrodes and sulfuric acid as electrolyte. When the lead-acid battery is discharged, the active substances on the positive and negative electrodes (positive lead dioxide, negative lead) are simultaneously converted into lead sulfate; when the lead-acid battery is charged, the lead sulfate on the positive electrode is converted into lead dioxide, and the lead sulfate on the negative electrode is converted into spongy metallic lead. In order to ensure the stable reaction of the positive and negative active substances, lead paste is usually coated on the positive and negative electrode plates. The preparation of lead paste determines the capacity, energy parameters and service life of the battery. However, the positive electrode lead paste in the prior art has the problem that the active substances are easy to fall off during the charging and discharging process, which leads to the degradation of battery performance.

[0003] Therefore, it is necessary to prepare a positive electrode lead paste and a lead-acid battery with strong activity and high structural stability. Summary of the invention

[0004] 1. Problem to be solved

[0005] Aiming at the problem in the prior art that active materials in positive lead paste are easy to fall off during charging and discharging, thereby causing battery performance degradation, the present invention provides a battery positive lead paste and a preparation method thereof, and a storage battery.

[0006] 2. Technical solution

[0007] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a positive lead paste for a battery according to the present invention comprises the following steps:

[0009] (1) dissolving lead ion salt, potassium permanganate, sodium hydroxide and an organic ligand in a mixed solvent of water and ethanol, and stirring the solution until it is uniform;

[0010] (2) reacting the mixed solution of step (1) at a temperature of 70° C. to 90° C. for no more than 10 min;

[0011] In the above steps, some lead ions are initially oxidized and nucleated under the oxidation of potassium permanganate, wherein sodium hydroxide plays a role in modulating the oxidizability of potassium permanganate on the one hand, preventing its oxidizability from being too strong to cause the reaction to generate large particles of lead dioxide, and on the other hand, provides an alkaline environment for the nucleation of nano lead dioxide crystals. At the same time, some lead ions form coordination bonds with organic ligands, and it is not suitable to generate large particles of lead dioxide crystal particles at this time, otherwise it will affect the formation of the subsequent MOF structure. Therefore, it is best to react at a temperature of 70°C to 90°C for no more than 10 minutes. After the reaction, the precursor of PbO2(cn)-Pb-MOF is generated, wherein PbO2(cn) refers to the lead dioxide crystal nucleus.

[0012] (3) transferring the dispersion obtained in step (2) to a 200 mL polytetrafluoroethylene autoclave, sealing it, and placing it in an oven at 100° C. to 120° C. to react for 24 h to 48 h;

[0013] (4) cooling the reaction product obtained in step (3) to 25° C., collecting the product, and then washing the product to obtain a PbO2(cn)-Pb-MOF composite material;

[0014] In the above steps, the remaining lead ions in the dispersion will continue to combine with organic ligands in the autoclave to form a MOF structure, and finally generate a porous PbO2(cn)-Pb-MOF composite material. Since the PbO2(cn) is oxidized and nucleated near the lead ions, PbO2(cn) will preferentially combine with the coordination center ions in the MOF structure, and then distribute in the pores of the PbO2(cn)-Pb-MOF composite material, providing growth space for the subsequent growth of lead dioxide.

[0015] (5) dispersing the PbO2(cn)-Pb-MOF composite material obtained in step (4) in a mixed solvent of DMF and water, adding lead ion salt and potassium permanganate thereto and stirring evenly, and continuously stirring the reaction at a temperature of 80 to 100° C.;

[0016] (6) cooling the reaction product in step (5) to 25° C., collecting it, and then washing it to obtain a PbO2-Pb-MOF composite material;

[0017] In the above steps, potassium permanganate will continue to oxidize lead ions and continue to grow lead dioxide on PbO2(cn). Lead dioxide continues to grow in the pores of the PbO2(cn)-Pb-MOF composite material, and finally forms a PbO2-Pb-MOF composite material.

[0018] (7) Placing the PbO2-Pb-MOF composite material in an oxygen-containing gas for carbonization reaction to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 250°C to 300°C.

[0019] In the above steps, carbonizing the PbO2-Pb-MOF composite material can improve the structural stability and conductivity of the MOF skeleton, thereby improving the electron mobility between the PbO2 in the MOF pores and the carbonized MOF skeleton, thereby ensuring that the positive electrode plate made of the carbonized PbO2-Pb-MOF composite material will preferentially generate or consume lead dioxide in the MOF pores during the subsequent charge and discharge process. In addition, carbonization in an oxygen-containing gas can inhibit the pyrolysis of lead dioxide to form lead tetraoxide to a certain extent, thereby ensuring the purity of lead dioxide in the carbonized PbO2-Pb-MOF composite material.

[0020] (8) The carbonized PbO2-Pb-MOF composite material, lead powder, SnSO4, polyester staple fiber, sulfuric acid and pure water are mixed to obtain the positive electrode lead paste.

[0021] Furthermore, the organic ligand includes 5-bromosalicylaldehyde and 4-amino-1,2,4-triazole.

[0022] Furthermore, in the step (1), 10 mmol to 20 mmol of the organic ligand, 5 mmol to 10 mmol of lead sulfate, 1 mmol to 5 mmol of potassium permanganate and 1 mmol to 5 mmol of sodium hydroxide are dissolved in 50 mL of a mixed solvent of water and ethanol, and magnetically stirred at 25° C. for 10 min to 30 min, wherein the proportion of ethanol in the mixed solvent is 20-80 vol%.

[0023] Furthermore, the reaction time in step (2) is 5 min to 10 min.

[0024] Furthermore, in step (4) and step (6), the reaction product obtained by the reaction is washed 3 to 5 times with pure DMF.

[0025] Furthermore, in the step (5), the following steps are specifically included:

[0026] 1) First, 80 to 100 parts by mass of PbO2(cn)-Pb-MOF composite material and 10 to 30 parts by mass of potassium permanganate are dispersed in 80 mL to 100 mL of a mixed solvent of DMF and water, and heating and stirring are started at a stirring speed of 50 rpm to 150 rpm; wherein the proportion of DMF in the mixed solvent is 40 vol% to 60 vol%;

[0027] 2) After the temperature is raised to 80° C. to 100° C., 20 mL to 30 mL of a lead ion salt solution is added dropwise to the dispersion of step 1) at a rate of 5 mL / min to 10 mL / min, wherein the lead ion mass fraction in the lead ion salt is 4 to 12 parts;

[0028] 3) After the dripping is completed, continue the reaction for 8 minutes to 30 minutes.

[0029] The above steps 1) to 3) are essentially the specific process of oxidizing lead ions with potassium permanganate and continuing to grow lead dioxide on PbO2(cn). Since potassium permanganate has strong oxidizing properties, it can react quickly with lead ions to generate lead dioxide after contacting. If the lead ion salt is directly mixed with potassium permanganate, it is easy to generate lead dioxide precipitation in the reaction solution. However, by using the slow dripping redox method of the above steps 1) to 3), adding the lead ion salt solution during continuous stirring can make the lead ions and the PbO2(cn)-Pb-MOF composite material fully mixed, and preferentially grow lead dioxide on PbO2(cn), so that the lead dioxide grows in the pores of the PbO2(cn)-Pb-MOF composite material.

[0030] Furthermore, in step (7), the oxygen in the oxygen-containing gas accounts for 30 vol%-60 vol%, and the rest includes one or more of water vapor, N2 or inert gas.

[0031] As mentioned above, carbonization in an oxygen-containing gas can inhibit the thermal decomposition of lead dioxide to form lead tetroxide to a certain extent, but excessive oxygen will also affect the carbonization of the MOF structure, so the optimal oxygen content is 30 vol%-60 vol%.

[0032] Furthermore, in the step (8), the positive electrode lead paste is prepared by taking the following raw materials in the following weight ratio: 900 to 1000 parts of lead powder, 0.5 to 1 part of SnSO4, 50 to 200 parts of the carbonized PbO2-Pb-MOF composite material, 0.5 to 1.5 parts of polyester staple fiber, 80 to 100 parts of 1.4 g / mL sulfuric acid and 105 to 115 parts of pure water;

[0033] The present invention also protects a battery positive electrode lead paste, which is prepared by any of the above-mentioned battery positive electrode lead paste preparation methods.

[0034] The present invention also protects a storage battery, which comprises the battery positive electrode lead paste.

[0035] 3. Beneficial effects

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] (1) A method for preparing a positive electrode lead paste for a battery according to the present invention. During the charging and discharging process of the battery, the active material lead dioxide in the prepared positive electrode lead paste is preferentially generated or consumed in the pores of the carbonized PbO2-Pb-MOF composite material. In this process, thanks to the structural stability of the carbonized MOF skeleton, the structure and volume of the positive electrode lead paste hardly change much. Moreover, during the charging process, the active material can be stored in the pores of the MOF skeleton, thereby reducing the shedding of the active material and increasing the service life of the positive electrode lead paste. In a lead-acid battery, this can improve the discharge capacity and cycle life of the battery plate.

[0038] (2) A storage battery of the present invention adopts the positive electrode lead paste of the present invention and has all the beneficial effects of the positive electrode lead paste of the present invention. DETAILED DESCRIPTION

[0039] The more detailed description of the embodiments of the present invention below is not intended to limit the scope of the claimed invention, but is merely for illustration and not to limit the description of the features and characteristics of the present invention, so as to propose the best mode for performing the present invention, and to be sufficient to enable those skilled in the art to implement the present invention. However, it should be understood that various modifications and variations may be made without departing from the scope of the present invention as defined by the appended claims. The detailed description should be considered only as illustrative, not restrictive, and if there are any such modifications and variations, they will all fall within the scope of the present invention described herein. In addition, the background technology is intended to illustrate the current status and significance of the research and development of the present technology, and is not intended to limit the present invention or the application field of the present application and the present invention.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs; the terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0041] The present invention is further described below in conjunction with specific embodiments.

[0042] Example 1

[0043] This embodiment provides a battery positive electrode lead paste, and the preparation method thereof specifically comprises the following steps:

[0044] (1) 8 mmol of lead sulfate, 3 mmol of potassium permanganate, 2 mmol of sodium hydroxide and 18 mmol of an organic ligand 5-bromosalicylaldehyde 4-amino-1,2,4-triazole were dissolved in 50 mL of a mixed solvent of water and ethanol, and stirred at 25° C. for 20 min until the solution became homogeneous; wherein the proportion of ethanol in the mixed solvent was 65 vol%.

[0045] (2) reacting the mixed solution of step (1) at 75° C. for 6 min;

[0046] (3) The dispersion obtained in step (2) was transferred to a 200 mL polytetrafluoroethylene autoclave, which was sealed and placed in an oven at 120° C. for reaction for 36 h;

[0047] (4) cooling the reaction product obtained in step (3) to 25° C. and collecting it, and then washing the reaction product obtained by the reaction with pure DMF for 3 times to obtain a PbO2(cn)-Pb-MOF composite material;

[0048] (5) Growth of lead dioxide:

[0049] 1) First, 100 parts by mass of PbO2(cn)-Pb-MOF composite material and 25 parts of potassium permanganate are dispersed in 100 mL of a mixed solvent of DMF and water, and heating and stirring are started at a stirring speed of 100 rpm; wherein the proportion of DMF in the mixed solvent is 50 vol%;

[0050] 2) After the temperature is raised to 90° C., 30 mL of a lead ion salt solution is added dropwise to the dispersion of step 1) at a rate of 6 mL / min, wherein the lead ion mass fraction in the lead ion salt is 10 parts;

[0051] 3) After the dripping is completed, the reaction is continued for 15 minutes to obtain the reaction product.

[0052] (6) cooling the reaction product in step (5) to 25° C. and collecting it, and then washing the reaction product with pure DMF three times to obtain a PbO2-Pb-MOF composite material;

[0053] (7) Placing the PbO2-Pb-MOF composite material in an oxygen-containing gas for carbonization reaction to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 270°C; wherein the oxygen in the oxygen-containing gas accounts for 40 vol%, and the rest is N2.

[0054] (8) The following raw materials were prepared into positive electrode lead paste in the following proportions by weight: 150 parts of carbonized PbO2-Pb-MOF composite material, 950 parts of lead powder, 1.2 parts of polyester staple fiber, and 0.8 parts of stannous sulfate were dry-mixed and stirred for 5 minutes, 110 parts of pure water were added and wet-mixed for 10 minutes at room temperature, and then 90 parts of sulfuric acid with a density of 1.4 g / mL was added and stirred for 15 minutes. The reaction temperature was controlled not to be higher than 60°C, and an apparent specific gravity of 4.3 g / cm was obtained. 3 Positive lead paste.

[0055] This embodiment also provides a lead-acid battery, wherein the positive lead paste of this embodiment is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0056] The lead-acid battery prepared in this embodiment was subjected to initial performance (2HR capacity) and cycle performance measurement: the lead-acid battery was discharged to 10.5V / battery at 10A and charged to 14.8V / battery at 10A for 5h. The lead-acid battery was considered to be failed if the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0057] Table 1. Performance comparison of lead-acid batteries obtained in various implementation methods

[0058]

[0059] Example 2

[0060] This embodiment provides a battery positive electrode lead paste, and the preparation method thereof specifically comprises the following steps:

[0061] (1) 7 mmol of lead sulfate, 2 mmol of potassium permanganate, 1.5 mmol of sodium hydroxide and 15 mmol of an organic ligand 5-bromosalicylaldehyde 4-amino-1,2,4-triazole were dissolved in 50 mL of a mixed solvent of water and ethanol, and stirred at 25° C. for 20 min until the solution became homogeneous; wherein the proportion of ethanol in the mixed solvent was 60 vol%.

[0062] (2) reacting the mixed solution of step (1) at 75° C. for 6 min;

[0063] (3) The dispersion obtained in step (2) was transferred to a 200 mL polytetrafluoroethylene autoclave, which was sealed and placed in an oven at 120° C. for reaction for 36 h;

[0064] (4) cooling the reaction product obtained in step (3) to 25° C. and collecting it, and then washing the reaction product obtained by the reaction with pure DMF for 3 times to obtain a PbO2(cn)-Pb-MOF composite material;

[0065] (5) Growth of lead dioxide:

[0066] 1) First, 95 parts by weight of PbO2(cn)-Pb-MOF composite material and 23 parts of potassium permanganate are dispersed in 100 mL of a mixed solvent of DMF and water, and heating and stirring are started at a stirring speed of 90 rpm; wherein the proportion of DMF in the mixed solvent is 60 vol%;

[0067] 2) After the temperature is raised to 90° C., 25 mL of a lead ion salt solution is added dropwise to the dispersion of step 1) at a rate of 5 mL / min, wherein the lead ion mass fraction in the lead ion salt is 10 parts;

[0068] 3) After the dripping is completed, the reaction is continued for 18 minutes to obtain the reaction product.

[0069] (6) cooling the reaction product in step (5) to 25° C. and collecting it, and then washing the reaction product with pure DMF three times to obtain a PbO2-Pb-MOF composite material;

[0070] (7) Placing the PbO2-Pb-MOF composite material in an oxygen-containing gas for carbonization reaction to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 280°C; wherein the oxygen in the oxygen-containing gas accounts for 40 vol%, and the rest is argon.

[0071] (8) The following raw materials were prepared into positive electrode lead paste in the following proportions by weight: 180 parts of carbonized PbO2-Pb-MOF composite material, 1000 parts of lead powder, 1.2 parts of polyester staple fiber, and 0.8 parts of stannous sulfate were dry-mixed and stirred for 5 minutes, 110 parts of pure water were added and wet-mixed for 10 minutes at room temperature, and then 90 parts of sulfuric acid with a density of 1.4 g / mL was added and stirred for 15 minutes. The reaction temperature was controlled not to be higher than 60°C, and an apparent specific gravity of 4.3 g / cm was obtained. 3 Positive lead paste.

[0072] This embodiment also provides a lead-acid battery, wherein the positive lead paste of this embodiment is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0073] The lead-acid battery prepared in this embodiment was subjected to initial performance (2HR capacity) and cycle performance measurement: the lead-acid battery was discharged to 10.5V / battery at 10A and charged to 14.8V / battery at 10A for 5h. The lead-acid battery was considered to be failed if the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0074] Example 3

[0075] This embodiment provides a battery positive electrode lead paste, and the preparation method thereof specifically comprises the following steps:

[0076] (1) 8 mmol of lead sulfate, 3 mmol of potassium permanganate, 2 mmol of sodium hydroxide and 18 mmol of an organic ligand 5-bromosalicylaldehyde 4-amino-1,2,4-triazole were dissolved in 50 mL of a mixed solvent of water and ethanol, and stirred at 25° C. for 20 min until the solution became homogeneous; wherein the proportion of ethanol in the mixed solvent was 65 vol%.

[0077] (2) reacting the mixed solution of step (1) at a temperature of 75° C. for no more than 6 minutes;

[0078] (3) The dispersion obtained in step (2) was transferred to a 200 mL polytetrafluoroethylene autoclave, which was sealed and placed in an oven at 120° C. for reaction for 36 h;

[0079] (4) cooling the reaction product obtained in step (3) to 25° C. and collecting it, and then washing the reaction product obtained by the reaction with pure DMF for 3 times to obtain a PbO2(cn)-Pb-MOF composite material;

[0080] (5) Growth of lead dioxide:

[0081] 1) First, 100 parts by mass of PbO2(cn)-Pb-MOF composite material and 26 parts of potassium permanganate are dispersed in 100 mL of a mixed solvent of DMF and water, and heating and stirring are started at a stirring speed of 100 rpm; wherein the proportion of DMF in the mixed solvent is 50 vol%;

[0082] 2) After the temperature is raised to 90° C., 30 mL of a lead ion salt solution is added dropwise to the dispersion of step 1) at a rate of 6 mL / min, wherein the lead ion mass fraction in the lead ion salt is 10 parts;

[0083] 3) After the dripping is completed, the reaction is continued for 15 minutes to obtain the reaction product.

[0084] (6) cooling the reaction product in step (5) to 25° C. and collecting it, and then washing the reaction product with pure DMF three times to obtain a PbO2-Pb-MOF composite material;

[0085] (7) Placing the PbO2-Pb-MOF composite material in an oxygen-containing gas for carbonization reaction to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 270°C; wherein the oxygen in the oxygen-containing gas accounts for 40 vol%, and the rest is helium.

[0086] (8) The following raw materials in mass proportion were used to prepare positive electrode lead paste: 100 parts of carbonized PbO2-Pb-MOF composite material, 1000 parts of lead powder, 1.2 parts of polyester staple fiber, and 0.8 parts of stannous sulfate were dry-mixed and stirred for 5 minutes, 110 parts of pure water were added and wet-mixed for 10 minutes at room temperature, and then 90 parts of sulfuric acid with a density of 1.4 g / mL was added and stirred for 15 minutes. The reaction temperature was controlled not to be higher than 60°C, and an apparent specific gravity of 4.3 g / cm was obtained. 3 Positive lead paste.

[0087] This embodiment also provides a lead-acid battery, wherein the positive lead paste of this embodiment is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0088] The lead-acid battery prepared in this embodiment was subjected to initial performance (2HR capacity) and cycle performance measurement: the lead-acid battery was discharged to 10.5V / battery at 10A and charged to 14.8V / battery at 10A for 5h. The lead-acid battery was considered to be failed if the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0089] Comparative Example 1

[0090] The present comparative example provides a conventional positive electrode lead paste, which is prepared by taking the following raw materials in the following mass proportions: 1000 parts of lead powder, 1.2 parts of polyester staple fiber, 0.8 parts of stannous sulfate and 3 parts of graphite are dry-mixed and stirred for 5 minutes, 110 parts of pure water are added at room temperature and wet-mixed for 10 minutes, and then 90 parts of sulfuric acid with a density of 1.4 g / mL is added and stirred for 15 minutes, and the reaction temperature is controlled not to be higher than 60°C to obtain a positive electrode lead paste with an apparent specific gravity of 4.3 g / cm 3 Positive lead paste.

[0091] The positive electrode lead paste ratios of Comparative Example 1 and Example 1 are basically the same, with the main difference being that graphite is used instead of the carbonized PbO2-Pb-MOF composite material.

[0092] This comparative example also provides a lead-acid battery, wherein the positive lead paste of this comparative example is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0093] The lead-acid battery prepared in this comparative example was subjected to initial performance (2HR capacity) and cycle performance measurements: the lead-acid battery was discharged at 10A to 10.5V / battery and charged at 10A to 14.8V / battery for 5h. The lead-acid battery was considered to be ineffective when the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0094] By comparison, it can be seen that the performance of the lead-acid battery of Comparative Example 1 basically meets the design requirements of GB / T 22199-2017, while the performance of the lead-acid batteries prepared in Examples 1 to 3 is significantly improved, among which the lead-acid battery of Example 1 has the best performance, indicating that the positive electrode lead paste prepared by adding the carbonized PbO2-Pb-MOF composite material of the present invention can effectively improve the capacity and cycle life of the lead-acid battery, especially the cycle life is greatly improved. This is largely because the pores of the carbonized PbO2-Pb-MOF composite material provide growth and storage space for the positive electrode active substance lead dioxide, thereby extending the structural stability and life of the positive electrode lead paste.

[0095] Comparative Example 2

[0096] This comparative example provides a battery positive electrode lead paste, and its specific preparation method is basically the same as that of Example 1, with the main difference being that the reaction time in step (2) is 20 min.

[0097] This comparative example also provides a lead-acid battery, wherein the positive lead paste of this comparative example is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0098] The lead-acid battery prepared in this comparative example was subjected to initial performance (2HR capacity) and cycle performance measurements: the lead-acid battery was discharged at 10A to 10.5V / battery and charged at 10A to 14.8V / battery for 5h. The lead-acid battery was considered to be ineffective when the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0099] By comparison, it can be seen that the cycle life of the lead-acid battery in Comparative Example 2 is greatly reduced compared with that in Example 1. This may be because the MOF structure has not yet been fully grown in step (2), and the excessively long redox reaction time will generate a large amount of lead dioxide and agglomerate, resulting in a large amount of lead dioxide growing outside the MOF structure in the subsequent step (5). The lead dioxide outside the MOF structure is very easy to fall off during the charge and discharge process and changes the mechanical structure of the positive electrode lead paste, thereby reducing the cycle life of the lead-acid battery.

[0100] Comparative Example 3

[0101] This comparative example provides a battery positive electrode lead paste, and its specific preparation method is basically the same as that of Example 1, with the main difference being that in step (5), all the reaction raw materials are directly mixed and reacted at 90° C. for 15 minutes.

[0102] This comparative example also provides a lead-acid battery, wherein the positive lead paste of this comparative example is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0103] The lead-acid battery prepared in this comparative example was subjected to initial performance (2HR capacity) and cycle performance measurements: the lead-acid battery was discharged at 10A to 10.5V / battery and charged at 10A to 14.8V / battery for 5h. The lead-acid battery was considered to be ineffective when the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0104] By comparison, the cycle life of the lead-acid battery in Comparative Example 3 is also greatly reduced compared with Example 1. As mentioned above, this is probably because a large amount of lead dioxide is generated outside the MOF structure, which makes the active material relatively easy to fall off, thereby reducing the cycle life of the lead-acid battery. It can be seen that controlling the reaction time of step (2) and the reaction conditions of step (5) is very necessary for the stable and orderly growth of lead dioxide.

[0105] Comparative Example 4

[0106] This comparative example provides a battery positive electrode lead paste, and its specific preparation method is basically the same as that of Example 1, with the main difference being that in step (7), the oxygen-containing gas is replaced by pure N2.

[0107] This comparative example also provides a lead-acid battery, wherein the positive lead paste of this comparative example is coated on the positive grid of 6-DZF-20, and the coating amount is 200g. After coating, the surface is acid-sprayed, the surface is dried, solidified, dried and cut to make a positive plate. The positive plate is assembled with a negative plate and a separator into a semi-finished battery, and a lead-acid battery is obtained through processes such as formation.

[0108] The lead-acid battery prepared in this comparative example was subjected to initial performance (2HR capacity) and cycle performance measurements: the lead-acid battery was discharged at 10A to 10.5V / battery and charged at 10A to 14.8V / battery for 5h. The lead-acid battery was considered to be ineffective when the discharge capacity was lower than 0.8C (96min) three times in a row. The effective number of charge and discharge cycles was recorded. The results are recorded in Table 1.

[0109] By comparison, it can be seen that the performance of the lead-acid battery in Comparative Example 4 is lower than that in Example 1. This may be due to the pyrolysis of part of the lead dioxide during the carbonization process, resulting in impure lead dioxide, which in turn affects the performance of the lead-acid battery.

[0110] The present invention has been described in detail above in conjunction with specific exemplary embodiments. However, it should be understood that various modifications and variations may be made without departing from the scope of the present invention as defined by the appended claims. The detailed description should be considered only as illustrative, not restrictive, and any such modifications and variations, if any, will fall within the scope of the present invention described herein. In addition, the background art is intended to illustrate the current status and significance of the research and development of the present technology and is not intended to limit the present invention or the application field of the present application and the present invention.

[0111] More specifically, although exemplary embodiments of the present invention have been described herein, the present invention is not limited to these embodiments, but includes any and all embodiments that are recognizable by those skilled in the art based on the foregoing detailed description, such as combinations between the various embodiments, adaptive changes and / or replacements. The limitations in the claims may be interpreted broadly based on the language used in the claims and are not limited to the examples described in the foregoing detailed description or during the implementation of the application, which examples should be considered non-exclusive. Any steps listed in any method or process claim may be performed in any order and are not limited to the order presented in the claim. Therefore, the scope of the present invention should be determined solely by the attached claims and their legal equivalents, rather than by the description and examples given above.

[0112] Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail. When flow, power, refractive index, time, or other values ​​or parameters are expressed as ranges, preferred ranges, or a series of upper preferred values ​​and lower preferred values, this should be understood to specifically disclose all ranges formed by any pairing of any upper range limit or preferred value with any lower range limit or preferred value, regardless of whether the range is disclosed separately. For example, a range of 1-50 is understood to include any number, combination of numbers, or subrange selected from 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50, and all decimal values ​​between the above integers, for example, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, and 1.9. With respect to subranges, "nested subranges" extending from any endpoint within the range are specifically contemplated. For example, nested sub-ranges of the exemplary range 1-50 may include 1-10, 1-20, 1-30, and 1-40 in one direction, or 50-40, 50-30, 50-20, and 50-10 in the other direction.

Claims

1. A method for preparing a positive lead paste for a battery, characterized in that: The steps include: (1) dissolving lead ion salt, potassium permanganate, sodium hydroxide and an organic ligand in a mixed solvent of water and ethanol, and stirring the solution until it is uniform; (2) reacting the mixed solution of step (1) at a temperature of 70° C. to 90° C. for no more than 10 min; (3) transferring the dispersion obtained in step (2) to a 200 mL polytetrafluoroethylene autoclave, sealing it, and placing it in an oven at 100° C. to 120° C. to react for 24 h to 48 h; (4) cooling the reaction product obtained in step (3) to 25° C., collecting the product, and then washing the product to obtain a PbO2(cn)-Pb-MOF composite material; (5) dispersing the PbO2(cn)-Pb-MOF composite material obtained in step (4) in a mixed solvent of DMF and water, adding lead ion salt and potassium permanganate thereto and stirring evenly, and continuously stirring the reaction at a temperature of 80° C. to 100° C.; (6) cooling the reaction product in step (5) to 25° C., collecting it, and then washing it to obtain a PbO2-Pb-MOF composite material; (7) placing the PbO2-Pb-MOF composite material in an oxygen-containing gas for carbonization reaction to obtain a carbonized PbO2-Pb-MOF composite material, wherein the temperature of the carbonization reaction is 250° C. to 300° C.; (8) The carbonized PbO2-Pb-MOF composite material, lead powder, SnSO4, polyester staple fiber, sulfuric acid and pure water are mixed to obtain the positive electrode lead paste.

2. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: The organic ligand includes 5-bromosalicylaldehyde and 4-amino-1,2,4-triazole.

3. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: In the step (1), 10 mmol to 20 mmol of an organic ligand, 5 mmol to 10 mmol of lead sulfate, 1 mmol to 5 mmol of potassium permanganate and 1 mmol to 5 mmol of sodium hydroxide are dissolved in 50 mL of a mixed solvent of water and ethanol, and magnetically stirred at 25° C. for 10 min to 30 min, wherein the proportion of ethanol in the mixed solvent is 20 vol% to 80 vol%.

4. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: The reaction time in step (2) is 5 to 10 minutes.

5. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: In the step (4) and the step (6), the reaction product obtained by the reaction is washed 3 to 5 times with pure DMF.

6. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: In the step (5), the following steps are specifically included: 1) First, 80 to 100 parts by mass of PbO2(cn)-Pb-MOF composite material and 10 to 30 parts by mass of potassium permanganate are dispersed in 80 mL to 100 mL of a mixed solvent of DMF and water, and heating and stirring are started at a stirring speed of 50 rpm to 150 rpm; wherein the proportion of DMF in the mixed solvent is 40 vol% to 60 vol%; 2) After the temperature is raised to 80° C. to 100° C., 20 mL to 30 mL of a lead ion salt solution is added dropwise to the dispersion of step 1) at a rate of 5 mL / min to 10 mL / min, wherein the lead ion mass fraction in the lead ion salt is 4 to 12 parts; 3) After the dripping is completed, continue the reaction for 8 minutes to 30 minutes.

7. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: In step (7), the oxygen in the oxygen-containing gas accounts for 30 vol%-60 vol%, and the rest includes one or more of water vapor, N2 or inert gas.

8. The method for preparing a positive electrode lead paste for a battery according to claim 1, characterized in that: In step (8), the positive electrode lead paste is prepared by taking the following raw materials in the following weight ratio: 900 to 1000 parts of lead powder, 0.5 to 1 part of SnSO4, 50 to 200 parts of the carbonized PbO2-Pb-MOF composite material, 0.5 to 1.5 parts of polyester staple fiber, 80 to 100 parts of 1.4 g / mL sulfuric acid and 105 to 115 parts of pure water.

9. A battery positive electrode lead paste, characterized in that: The positive electrode lead paste is prepared by the method for preparing a positive electrode lead paste for a battery according to any one of claims 1 to 8.

10. A storage battery, characterized in that: The invention comprises the battery positive electrode lead paste as claimed in claim 9.

Citation Information

Patent Citations

  • Preparation method for lithium battery anode material by taking metal organic frame as template

    CN105932285A

  • Lead carbon battery negative electrode material and preparation method thereof

    CN108550819A