A machine-washable, wrinkle-resistant, naturally elastic all-wool fabric and its preparation method
Through biological mercerization technology, the problem that all-wool fabrics cannot be machine washed and are prone to wrinkles has been solved. It has achieved efficient anti-wrinkle and improved weft elasticity, improved hand feel, and reduced production costs and environmental pollution. It is suitable for high-end textile industry.
Patent Information
- Application Number
- CN202311237741.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing all-wool fabrics are not washable during use, are prone to wrinkles, and are not comfortable enough, and existing machine washable processing methods have problems such as environmental pollution, high costs, and fiber damage.
Using biological mercerization finishing method, the whole wool fabric is contacted with a mixture containing non-ionic penetrant and protease to modify the surface scales of wool fibers to achieve the comprehensive effects of machine washability, anti-wrinkle and weft elasticity.
It realizes the machine washable function of all-wool fabrics, while improving the anti-wrinkle performance and weft elasticity, giving it a better hand feel. The process is pollution-free, simple to operate, low in cost, and is suitable for industrial production.
Smart Images

Figure BDA0004466148550000091 
Figure BDA0004466148550000101 
Figure BDA0004466148550000111
Abstract
Description
Technical Field
[0001] The invention relates to a full wool machine washable, wrinkle-resistant and naturally elastic fabric and a preparation method thereof. Background Art
[0002] Pure wool (the wool spinning industry calls products with a wool content of more than 95% pure wool products) suits or casual wear have always been high-end clothing. However, until now, users have been troubled by the fact that they cannot be washed and must be dry-cleaned, are prone to wrinkles and are difficult to take care of, and are not comfortable enough. It is even more difficult for wool + spandex stretch fabrics to achieve the above functions.
[0003] Although there are currently some processing methods that can make all-wool fabrics machine washable, there are more or less corresponding disadvantages.
[0004] For example, one of the treatment methods is to use chemical mercerized wool raw materials to make worsted fabrics. The principle is to chlorinate the wool fibers before dyeing, and peel off all or most of the scales on the surface of the wool fibers (because the wool fibers have evenly and closely arranged scales on the surface, these fibers have directional sliding under mechanical movement or washing conditions, thereby forming felt shrinkage, making the size of the all-wool fabric smaller), and then evenly cover the fiber surface with a layer of resin. Eventually, the treated wool fiber surface will have the characteristics of extremely smoothness and almost no curling. The all-wool fabric made of this fiber only means that this fiber has the conditions to make the fabric machine washable. This is the mainstream method used in the current market to produce machine-washable all-wool fabrics. Its disadvantages are: ⑴ Chlorination of wool fibers will release a large amount of chlorine gas and wastewater containing chloride ions, causing great pollution to the environment; ⑵ The scaled wool fibers are particularly sensitive to heating auxiliaries and equipment performance during dyeing, which can easily cause dyeing; ⑶ Because the surface of the treated wool fibers is very smooth and has less curl, the cohesion between the fibers is weakened, making spinning extremely difficult, that is, excellent yarn counts cannot be spun, the count deviation will shrink by more than 10%, and good yarn evenness cannot be spun, and the yarn evenness will deteriorate by more than 15%; ⑷ Since the chemical mercerizing method uses oxidation The agent will damage the strength of wool to a certain extent, and the single fiber strength will be reduced by 10-15%, which will greatly increase the consumption of spinning, and the increase will be more than 2% on the original normal basis; ⑸ The price of chemical mercerized wool is 10-12 yuan higher per kilogram than the normal wool price (market fair price). If we take 300 grams per meter of worsted fabric as an example, the total cost of raw materials and processing costs will increase by 8-10 yuan per meter of cloth (it is difficult to produce using mercerized wool, and the processing cost will also increase by more than 5 yuan per meter of cloth), and the market competitiveness is small; ⑹ Textile fabrics made of chemical mercerized wool have lost the fluffy and crisp texture inherent in the wool fiber itself.
[0005] The second treatment method is: during the processing of the finished fabric, resin coating is used in the post-finishing process to make the fabric machine washable. The fabric finished by this process feels hard and has lost the rich, fluffy and soft characteristics of wool. In addition, the fabric can only be washed a limited number of times and will lose its machine washability after several washes. This method was tried in the early 1980s and has now been eliminated.
[0006] The third treatment method is to use the Croix mercerizing equipment produced in Italy to mercerize the grey cloth of wool fabric. The principle is the same as the first method. The difference is that the first method acts on the fibers, while this method is to finish the semi-finished grey cloth. Although it solves the problems of easy dyeing and spinning, it will also cause environmental pollution and the cost is also extremely high. The finished fabric loses the natural elasticity of the wool fiber. Because of the expensive equipment, this method has rarely been used in China since the late 1990s. Summary of the invention
[0007] The purpose of the present invention is to provide a full wool fabric which has a machine washable function and has better wrinkle resistance and better weft elasticity.
[0008] Another object of the present invention is to provide a method for preparing a machine-washable all-wool fabric which is pollution-free or low-pollution, simple to operate and low-cost.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] A pure wool fabric, wherein the pure wool fabric is subjected to bio-mercerization finishing, wherein the bio-mercerization finishing comprises contacting the pure wool fabric with a first mixed solution containing a non-ionic penetrant and a first protease, and then contacting the pure wool fabric with a second mixed solution containing a non-ionic penetrant and a second protease, wherein the second protease is different from the first protease,
[0011] The raw materials of the all-wool fabric are wool or wool and elastic fiber. When the raw material of the all-wool fabric is wool, the all-wool fabric is woven by single yarn and ply yarn made of wool, the twist coefficient of the single yarn is 70-100, the twist coefficient of the ply yarn is 230-250, and double warp and double weft weaving is adopted; when the raw materials of the all-wool fabric are wool and elastic fiber, the wool accounts for more than 95% of the total mass of the wool and elastic fiber, the all-wool fabric is woven by single yarn made of wool and elastic fiber, the twist coefficient of the single yarn is 150-160, and single warp and single weft weaving is adopted.
[0012] Preferably, the first protease is copper blue oxidase.
[0013] In some preferred embodiments, the first protease is laccase.
[0014] Preferably, the concentration of the first protease in the first mixed solution is 0.5-1.5 g / L, for example, 0.5 g / L, 0.8 g / L, 1 g / L, 1.3 g / L or 1.5 g / L.
[0015] Preferably, the second protease is subtilisin.
[0016] In some preferred embodiments, the second protease is protease 16L.
[0017] Preferably, the concentration of the second protease in the second mixed solution is 0.8-1 g / L, for example 0.8 g / L, 0.9 g / L or 1 g / L.
[0018] Preferably, the nonionic permeabilizing agent includes one or more of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, such as JFC, JFC-1, JFC-2, JFC-E, etc.
[0019] Preferably, the concentration of the nonionic permeabilizing agent in the first mixed solution is 0.5-1.5 g / L, for example, 0.5 g / L, 0.8 g / L, 1 g / L, 1.3 g / L or 1.5 g / L.
[0020] Preferably, the concentration of the nonionic permeabilizing agent in the second mixed solution is 0.5-1.5 g / L, for example, 0.5 g / L, 0.8 g / L, 1 g / L, 1.3 g / L or 1.5 g / L.
[0021] Preferably, the pH of the second mixed solution is 8-10, more preferably 9-10.
[0022] Preferably, the temperature at which the all-wool fabric contacts the first mixed liquid and the second mixed liquid is independently 50-60° C., and the time at which the all-wool fabric contacts the first mixed liquid and the second mixed liquid is independently 40-50 minutes.
[0023] Preferably, the bio-mercerization finishing further comprises performing enzyme inactivation treatment on the all-wool fabric after contact with the second mixed solution.
[0024] In some embodiments, the enzyme inactivation treatment comprises immersing the pure wool fabric treated with the second mixed solution into a third mixed solution, wherein the third mixed solution is an acid solution and has a pH of 4 to 4.5.
[0025] Furthermore, the temperature of the third mixed liquid is controlled to be 70-90°C, further 75-85°C, for example 80°C.
[0026] Furthermore, the acid solution is an acetic acid solution.
[0027] Preferably, when the raw material of the all-wool fabric is wool, the total tightness coefficient of the all-wool fabric is 90-100, and the ratio of the upper machine width to the lower machine width is (1.23-1.30):1, for example (190-195):(150-152).
[0028] Preferably, when the raw materials of the all-wool fabric are wool and elastic fiber, the total tightness coefficient of the all-wool fabric is 95-100, and the ratio of the upper machine width to the lower machine width is (1.25-1.33):1, for example, (195-200)-152.
[0029] Preferably, the elastic fiber is spandex.
[0030] In some preferred embodiments, the spandex is core-spun 40D colorless spandex.
[0031] Preferably, the wrinkle resistance index of the all-wool fabric is ≥ level 3.5.
[0032] Preferably, the weft elasticity of the all-wool fabric is greater than or equal to 7%.
[0033] Preferably, the relaxed dimensional change rate of the all-wool fabric is: width not less than -3%, length not less than -3%; the total dimensional change rate is: width not less than -3%, length not less than -3%; the edge shrinkage rate is: width not less than -1%, length not less than -1%.
[0034] Further preferably, the relaxed dimensional change rate of the all-wool fabric is: width not less than -1%, length not less than -2.5%; the total dimensional change rate is: width not less than -1%, length not less than -2.5%; the edge shrinkage rate is: length not less than -0.5%, width not less than -0.5%.
[0035] The present invention also provides a method for preparing a pure wool fabric, comprising the following steps:
[0036] Step 1: making wool tops, selectively weaving the wool tops with elastic fibers into yarns, and then weaving them into grey cloth;
[0037] Step 2, finishing the grey cloth to make the finished product; wherein the finishing includes raw repair → selective high temperature shaping → singeing → continuous boiling → washing → rope-shaped water absorption → flat washing and continuous boiling → drying → finished repair → selective high temperature shaping → bio-mercerization finishing → softening finishing → baking → shearing → wet storage → steaming → pre-shrinking → ironing → pre-shrinking → can steaming → finished product.
[0038] Preferably, the bio-mercerization finishing specifically comprises the following steps:
[0039] (1) immersing the grey cloth into a first mixed solution, wherein the first mixed solution comprises a nonionic penetrant and a laccase, wherein the concentration of the nonionic penetrant in the first mixed solution is 0.5 to 1.5 g / L, the concentration of the laccase is 0.5 to 1.5 g / L, the immersion temperature is 50 to 60° C., the immersion time is 40 to 50 min, and the bath ratio is 1:(5 to 15);
[0040] (2) immersing the grey cloth treated with the first mixed solution into a second mixed solution, wherein the second mixture includes a nonionic penetrant and protease 16L, the pH of the second mixed solution is 8-10, the concentration of the nonionic penetrant is 0.5-1.5 g / L, the concentration of the protease 16L is 0.8-1 g / L, the immersion temperature is 50-60° C., the immersion time is 40-50 min, and the bath ratio is 1:(5-15);
[0041] (3) Immersing the grey cloth treated with the second mixed solution into a third mixed solution, wherein the third mixed solution is an acid solution with a pH of 4 to 4.5, an immersion temperature of 70 to 90° C., an immersion time of 5 to 10 min, and a bath ratio of 1:(10 to 15).
[0042] Preferably, the bio-mercerization finishing further comprises, after step (3), the steps of rope-shaped water absorption and drying of the grey cloth, wherein the drying temperature is 140-150° C., the speed is 35-40 m / min, and the overfeed is 5-10%.
[0043] Preferably, when the raw material of the all-wool fabric is wool, the step one specifically includes: wool top → blending → first needle combing → second needle combing → third needle combing → fourth needle combing → coarse yarn → fine yarn → automatic winding → parallel thread → double twisting → yarn steaming → warping → weaving → white grey cloth off the machine.
[0044] Preferably, when the raw materials of the all-wool fabric are wool and elastic fiber, the step one specifically includes: wool top→blending→first needle combing→second needle combing→third needle combing→fourth needle combing→coarse yarn→spun yarn→automatic winding→steaming→warping→weaving→white grey cloth off the machine.
[0045] In some embodiments, the method for preparing wool tops comprises: wool→rewashing and oiling→sliver blending 1→sliver blending 2→pin combing 1→pin combing 2→combing→pin combing 3→pin combing 4→slivering.
[0046] Furthermore, when the raw material of the all-wool fabric is wool, the fineness of the wool is 20 to 21 microns; when the raw materials of the all-wool fabric are wool and elastic fiber, the fineness of the wool is 19 to 20 microns.
[0047] Preferably, when the raw material of the all-wool fabric is wool, the post-finishing does not undergo high-temperature setting; when the raw materials of the all-wool fabric are wool and elastic fiber, the post-finishing undergoes high-temperature setting, and the high-temperature setting temperature is 180-200°C and the speed is 15-20m / min.
[0048] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0049] The all-wool fabric of the present invention has the function of being machine washable, and has better wrinkle resistance, better weft elasticity and better hand feel;
[0050] The preparation method of the invention has no pollution or low pollution, simple operation and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a photo of the fiber after bio-mercerization finishing in Example 1;
[0052] Figure 2 This is a photograph of the fiber of Example 1 before bio-mercerization finishing. DETAILED DESCRIPTION
[0053] Since 2000, the inventor has been committed to developing a method for preparing a quick, pollution-free or low-pollution, simple-to-operate, low-cost all-wool (i.e., pure wool) machine-washable fabric. After some attempts, certain results have been achieved, which are briefly introduced here as a prelude to the present invention.
[0054] At the beginning of this century, bio-enzyme technology emerged in the domestic textile printing and dyeing industry. Bio-protease is a type of enzyme with biological activity. They can effectively decompose protein by breaking the peptide bonds that connect amino acids into polypeptide chains. Protease can be divided into thousands of types according to its different effects, and each type has a different effect on protein. This pure biological preparation is like the targeted drug for treating cancer in the medical field. Each bio-enzyme corresponds to a fiber or substance and can undergo biological reactions under certain conditions. Similarly, for protein fiber wool, there is also a protease that has a biological effect on it. Based on this principle, the inventor thought about whether this protease could be used to descale all-wool fabrics, so that the fabrics can be machine washed. This was also the initial prototype of the present invention. At first, the test method used was a one-step method of single biological protease. However, the test results were unstable in practice, the fabric was not completely machine washable, and the shrinkage rate of the fabric was unstable. Using a 500-fold electron microscope to observe the changes in the scale structure on the fiber surface, it was found that although the scales had changed, the scale edges still existed to varying degrees. The reason is that proteases react mildly to proteins and have less force. In addition, the scale layer on the surface of wool fibers is tightly arranged and hard, making it difficult for it to be completely effective. The relevant paper was published in the fifth issue of "Textile Guide" in 2003.
[0055] The inventor did not give up the idea of using biological enzymes. Instead, according to the characteristics of this auxiliary agent, in 2005, he wanted to use a treatment method that combines chemical and biological methods to treat all wool fabrics. The premise of using chemical auxiliary agents is that the auxiliary agent has little pollution. The role of this auxiliary agent is first to pry open a gap in the tight scale layer on the surface of the wool fiber, and then let the biological protease act on all the pried scale edges and corners, corroding most of the scale edges and corners, so that the surface of the wool fiber is smooth and loses the felt shrinkage function. The chemical auxiliary agent used is Basulan 2448 auxiliary agent. This auxiliary agent is an oxidant. Although it does not release chlorine, the wastewater contains chloride ions and harmful components. The final machine washable test result is good, but we did not carry out industrial production. The reasons are: ⑴ Sewage pollutes the environment; ⑵ It has a stripping effect on colored fabrics and is not suitable for yarn-dyed fabrics; ⑶ At that time, the domestic piece dyeing technology had not yet passed the test, and it was difficult to be suitable for industrial production, because this technology is more suitable for piece dyeing of high-end all-wool clothing fabrics for men and women (mercerizing the white grey fabric of all-wool fabrics, and then dyeing the grey fabrics after finishing).
[0056] In 2015, domestic piece-dyeing technology gradually matured, and all-wool piece-dyeing fabrics were in the ascendant. It has been developing to this day. Due to the rise of foreign spot goods and domestic e-commerce platforms, all-wool machine-washable fabrics are becoming more and more popular in the market. Although there are documents that mention the use of proteases to treat wool fibers or fabrics, such documents basically stay at reducing the effect of anti-felting of wool fabrics, and are still far from being able to make wool fabrics machine washable. The present invention is a preparation method that is not complicated and does not increase costs, but is easy to operate, so that it can eventually achieve industrial production after years of experiments and research.
[0057] The inventor independently developed a biological additive called laccase through the professional bio-enzyme production company, Novozymes of Denmark, which specifically acts on the surface scales of wool to replace the chemical additive Basulan 2448 mentioned above, achieving the effect of full biological additives and zero pollution emissions. The inventor called this process bio-mercerization. Bio-mercerization retains the inherent advantages of wool fiber, such as sufficient elasticity, crispness, fluffy and good warmth retention, and the production cost of bio-mercerization only needs to increase by 1-2 yuan per meter of cloth, which is low cost. However, the inventor found that bio-mercerization has the following problems: ⑴ It has a stripping effect on colored yarn-dyed grey fabrics. ⑵ It does not achieve the effect of machine washability on loose-structured all-wool fabrics (i.e., existing ordinary all-wool fabrics). ⑶ The specification design process of the fabric has a great influence on the machine washability function; ⑷ The finishing process after the fabric treatment has a great influence on the machine washability index by effectively removing the internal and external stresses of the fibers and yarns.
[0058] The inventor further designed the parameters of the all-wool fabric and improved the post-finishing process, so that the all-wool fabric has the function of machine washability, and at the same time has better wrinkle resistance, better natural elasticity in the weft direction, and better hand feel.
[0059] The advantages of the present invention include at least:
[0060] (1) The present invention uses pure biological technology instead of chemical technology to mercerize wool fibers and fabrics, thereby laying a feasible technological foundation for making all-wool fabrics machine washable.
[0061] (2) The treatment process of the present invention achieves zero pollution emission, adapts to the concept of green and low-carbon development of human social civilization, and lays a foundation for the industrial production of green wool products.
[0062] (3) The present invention fully maintains the fluffy, soft and warm characteristics of wool fibers, the processing process is simple and easy to operate, the product has a wide range of applications, low cost, and is suitable for industrial production.
[0063] (4) The present invention organically combines the innovation of fabric design parameters, post-finishing process innovation, and bio-mercerization finishing process innovation to create a high-end pure wool fabric with composite functions that combines wrinkle resistance, easy care, weft elastic comfort, and machine washability.
[0064] In terms of innovation in fabric design parameters, the present invention adopts an unconventional twist coefficient for the following purposes: A. In order to release greater stress, the yarn must increase its retraction, so that greater fabric elasticity can be obtained. B. A larger twist coefficient can effectively prevent the directional slippage of wool fibers, thereby reducing the shrinkage rate of the fabric during machine washing and enhancing the machine washability of the fabric. C. A larger yarn twist can effectively reduce the head end of the wool fiber in the yarn cross section, greatly enhancing the smoothness of the fabric surface. The use of a larger tightness coefficient has the following purposes: After the fabric is sorted and the warp and weft yarns are fully retracted, the yarns on the surface of the fabric are kept at a higher fullness. When washing, there will be no large relative slippage between the yarns, thereby improving the machine washability. A smaller tightness coefficient will not have this effect.
[0065] In terms of post-finishing process innovation: the present invention has adopted several process steps such as overfeeding, wet storage, and pre-shrinkage, with the purpose of preventing the fabric from being subjected to additional external stress during the post-finishing process. If these external stresses are not effectively eliminated, the machine washability parameters will be seriously affected. More seriously, no matter what kind of mercerized wool is used to make all-wool fabrics, the external stress cannot be effectively eliminated, and the machine washability index will not be qualified. Because the post-finishing equipment for worsted fabrics must use a large tension to make the equipment operate normally, the external stress generated can only be generated by optimizing the process parameters and steps, and eliminating the external stress while generating it. This key is crucial.
[0066] In terms of bio-mercerized finishing: the present invention optimizes the above process parameters to make the edges and corners of the scales on the surface of the wool fiber smoother (see Figure 1 ), the whole process does not damage the wool fiber. If the relaxation shrinkage rate and total size change rate of the fabric in the machine washable index are qualified by the high twist coefficient and the large total tightness coefficient and the external stress release of the post-finishing, then the edge shrinkage index is the most able to illustrate the chemical mercerization effect in the present invention. This index requires only 1%, which is much smaller than the previous two shrinkage indexes, proving that this index is particularly critical. It can directly reflect the quality of the wool fiber mercerization effect or whether it is qualified. The edge shrinkage index is the reason that the edge of the fabric has no force to hold the fiber, which is in a naturally loose state. If washed in a washing machine, these fibers will be felted together if they still have a directional slip function, and the shrinkage rate will be much greater than 1%. Therefore, the bio-mercerization process of the present invention is very successful. The fibers that have been finished with bio-mercerization have been tested by an international third-party authority and the fineness is 0.14 microns.
[0067] (5) The present invention also attempts to make the elastic all-wool woven fabric (25002) containing spandex wrinkle-resistant, easy-care and machine-washable. As mentioned above, the innovative concepts of product design innovation, post-finishing process innovation, and bio-mercerized finishing are better than those of the 25001 product in terms of machine washability, which further expands the scope of application of the present invention and further illustrates the advanced feasibility of the present invention. The technical innovation that all-wool + spandex elastic fabric can be machine-washed has created a new era in the field of high-end all-wool elastic fabrics.
[0068] (6) The products tested in the present invention are all white and can be dyed according to customer requirements after the bio-mercerization process is completed. In the field of wool worsted, this process is called piece dyeing. Colored pure wool fabrics cannot be bio-mercerized because the colored fabrics will fade after bio-mercerization (bio-mercerization has a small amount of decolorization function). In addition to solid-color products, wool worsted products also include tweed products. Tweed products are ever-changing. These fabrics need to be completed by color weaving. The present invention is also suitable for these fabrics. At this time, the process steps must be changed, and the bio-mercerization process must be carried out in front. The effect of the present invention can also be achieved. The specific process is as follows: (fiber bio-mercerization-dyeing) (performed in the wool strip dyeing cylinder)-recombing-spinning-weaving-finishing-finished product. This process step is called strip dyeing, and the present invention is also suitable for it, so it will not be repeated here.
[0069] (7) The present invention performs bio-mercerization finishing on all-wool white grey fabric, which effectively improves the whiteness quality of the grey fabric. People in the industry know that wool fiber itself has yellow oil sweat, which causes the whiteness of white fabrics made of wool fiber to be poor. If a very white all-wool fabric is required, hydrogen peroxide must be used for bleaching. For piece-dyed products, the whiteness of the grey fabric is not enough, which will seriously affect the brightness of the dyeing. In the present invention, the whiteness of the grey fabric after bio-mercerization finishing is nearly 20%, which greatly improves the color brightness of the piece-dyed product limit, and can produce piece-dyed fabrics with bright colors.
[0070] (8) In the present invention, due to the biological mercerization effect, the arrangement density of the scales on the surface of the wool fiber is destroyed and opened, making it easier for the dye molecules to penetrate the scales during dyeing and combine with the protein chemical bonds of the wool fiber, further improving the dye absorption rate and utilization rate. Practice has shown that when the fabrics before and after biological mercerization are dyed the same color, the dye consumption is saved by 10%, and the economic benefit is good.
[0071] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0072] Unless otherwise specified, the raw materials used in the present invention are all commercially available products.
[0073] Example 1
[0074] A pure wool fabric, comprising the following preparation process:
[0075] (1) Selection of raw materials:
[0076] White wool top (wool fineness is 20.5 microns).
[0077] (2) Recombing, spinning and weaving process:
[0078] White wool top→re-washing and oiling→blending 1→blending 2→pin combing 1→pin combing 2→combing→pin combing 3→pin combing 4→balling→blending→first pin combing→second pin combing→third pin combing→fourth pin combing→coarse yarn→fine yarn→automatic winding→doubling→double twisting→yarn steaming→warping→weaving→white grey cloth off the machine.
[0079] Among them, the above-mentioned processes such as rewashing and oiling, blending, and needle combing can refer to the existing technology unless otherwise specified. The difference between the above-mentioned process flow and the existing technology mainly lies in: spun yarn, double twisting and weaving. The specific process design parameters are shown in Table 1 below.
[0080] Table 1
[0081]
[0082] The inventors also designed different parameters for the twist coefficient of the strands, the total tightness coefficient and the upper machine width during the exploration process, and found that when the twist coefficient of the strands is too small (less than 230) or the total tightness coefficient is too small (less than 90) or the upper machine width is too small (less than 190), the fabric performance is poor. See Table 2 for specific parameter design and fabric performance.
[0083] Table 2
[0084] Ply yarn twist factor Total tightness coefficient Machine width Finished product width Hand feel evaluation Anti-wrinkle index Weft elasticity Remark 150 86 178 cm 152 cm Relatively soft and slippery Level 1.6 4.3% Normal fabric 170 88 180 cm 152 cm Appropriately soft and slippery Level 2.1 4.9% Also within the normal range 195 92 185 cm 152 cm Normal slightly hard 2.8 5.9% Also within the normal range 230 90 190 cm 152 cm Swelling feeling Level 3.5 7.8% Distinctive features and good drape 240 90 190 cm 150cm The board feels stiff enough 3.7 7.8% Feels a bit hard
[0085] Among them, the hand feel evaluation refers to the Japanese FAST fabric style evaluation index. The fabric has a swelling feeling mainly refers to the feeling of swelling when holding the fabric with hands, which shows that the fabric has good elasticity. The test method of the anti-wrinkle index refers to ISO9867-2009, and the determination method of the weft elasticity refers to FZ / T 01034-2008.
[0086] It should be noted that the national standard stipulates that wrinkle-resistant products have an anti-wrinkle index of ≥3.5, with the highest being level 5. There is no requirement for the weft elasticity of fabrics. Generally, the weft elasticity of wool blended fabrics is 2-4%, and pure wool products are slightly higher than wool blended products. There is no specific national standard limit for this parameter, but the greater the weft elasticity of the fabric, the more conducive it is for the clothing to have greater stretch and be more comfortable to wear. The greater the elasticity, the easier it is for the fabric to recover and will not deform. The above-mentioned 25001 product is a double-warp and double-weft design, and it is preferred to use fabrics with the parameters shown in Table 1 for subsequent finishing.
[0087] (3) Post-finishing wet finishing process:
[0088] White grey cloth raw repair → singeing → continuous boiling (85℃, 35m / min) → scouring (CIMI washing and shrinking combined machine, 45℃, 40min, 3kg of detergent, the detergent is not specifically limited, conventional detergents in the field can be used) → rope-shaped water absorption → flat washing and continuous boiling (85℃, Angora setting agent 2g / L) → drying (LB334, 145℃, 38m / min, overfeed 8%, 25001 width 158cm) → finishing → bio-mercerization finishing.
[0089] Among them, unless otherwise specified, processes such as hair treatment and singeing can refer to the prior art. This embodiment creatively uses the bio-mercerization finishing process, and the following focuses on the bio-mercerization finishing process.
[0090] (4) Bio-mercerization finishing process:
[0091] A. Pretreatment:
[0092] The grey cloth was immersed in a pretreatment solution, wherein the pretreatment solution included: 1 g / L of a nonionic penetrant (fatty alcohol polyoxyethylene ether, purchased from Zhangjiagang Hongda Additive Factory, brand KOC) (its function was to help the biological enzyme further penetrate the wool fabric), 1.0 g / L of a protease DENILITE II S2.5L (laccase) (purchased from Novozymes); bath ratio: 1:10; the temperature of the pretreatment solution was 55°C, and the immersion time was 40 minutes.
[0093] B. Protease treatment:
[0094] The pretreated grey cloth is treated with protease, and the process of protease treatment includes immersing the grey cloth in a protease solution, wherein the protease solution includes: non-ionic penetrant KOC: 1 g / L, protease Savinase 16L (purchased from Novozymes): 0.8 g / L, pH value 9.0-10.0; bath ratio: 1:10; the temperature of the protease solution is 55°C, and the immersion time is 45 minutes.
[0095] C. Enzyme inactivation:
[0096] Add glacial acetic acid to the above protease solution to adjust the pH to 4-4.5, the bath ratio to 1:10-15, and raise the temperature to 80°C for 5-10 minutes.
[0097] D. Rope-shaped water absorption → drying (LB334, 145°C, 38 m / min, overfeed 8%, 25001, width 157 cm).
[0098] During the process of exploration, the inventors also conducted comparative experiments on the above-mentioned step (4) bio-mercerization finishing process (mainly comparing the protease treatment process, the pretreatment and enzyme inactivation process are as above) to explore more suitable protease solution concentration, pH, and treatment temperature and time. The specific comparative experiments of the bio-mercerization finishing process are shown in Table 3 below.
[0099] Table 3
[0100]
[0101]
[0102] As shown in Table 3, after bio-mercerization finishing, the strength of the grey fabrics decreased to a certain extent, but with the increase of the amount of protease Savinase16L, the increase of pH value and the extension of finishing time, the trend of strength decline was alleviated. Considering the comprehensive cost and grey fabric performance, the amount of Savinase16L is preferably 0.8-1 g / L. With the further increase of the amount, the wool will be damaged, resulting in the decrease of fabric strength and uneven coloring in the subsequent dyeing. The pH is preferably 9-10, the temperature is preferably 55°C, and the time is preferably 40-50 min.
[0103] In addition, the inventor has also conducted the following explorations:
[0104] 1) When the protease DENILITE II S2.5L was not used in the pretreatment, it was found that the appearance structure of the scales was basically unchanged when observed under a fiberscope. Furthermore, when the amount of protease DENILITE II S2.5L was too small (e.g., less than 0.5 g / L), the effect on the scales on the wool surface was minimal.
[0105] 2) Using ordinary pure wool fabrics (such as the normal fabrics shown in Table 2) for bio-mercerization finishing can reduce the felting of wool fibers, but it still does not meet the machine washability index.
[0106] (5) Post-finishing process flow:
[0107] Softening finishing (amino silicone softener 3 kg / 100 liters, rolling rate 70%, 2 dips and 2 rolls) → baking (LB334 equipment, 150℃, 38 m / min, overfeed 8%, 25001 width 154 cm) → shearing → wet storage for 8 hours → steaming → pre-shrinking → ironing (125℃, speed 20 m / min) → pre-shrinking → tank steaming 163 → finished product (the width of the finished product is about 152 cm).
[0108] Example 2
[0109] It is substantially the same as Example 1, except that:
[0110] (1) Selection of raw materials:
[0111] White wool top (wool fineness is 19.5 microns), siro-spun core-spun 40D colorless spandex.
[0112] (2) Product recombing, spinning and weaving process:
[0113] White wool top → re-washing and oiling → blending 1 → blending 2 → combing 1 → combing 2 → combing → combing 3 → combing 4 → balling → blending → first combing → second combing → third combing → fourth combing → coarse yarn → fine yarn (using siro-spun core-spun 40D colorless spandex) → automatic winding → yarn steaming → warping → weaving → white grey cloth off the machine.
[0114] The finished product design parameters of the fabric are specifically shown in Table 4 below.
[0115] Table 4
[0116]
[0117] During the exploration process, the inventors also designed different parameters of single yarn twist coefficient, total tightness coefficient and machine width for this type of fabric, and found that when the single yarn twist coefficient is too small (lower than 150) or the total tightness coefficient is too small (less than 95) or the machine width is too small (lower than 195), the performance of the fabric is poor. The design of specific fabric parameters and fabric performance are shown in Table 5.
[0118] Table 5
[0119] Single yarn twist coefficient Total tightness coefficient Machine width Finished product width Anti-wrinkle index Hand feel evaluation Remark 135 86 190cm 150cm Level 2.5 Relatively soft and slippery Normal fabric 140 88 190cm 150cm Level 2.5 Appropriately soft and slippery Also within the normal range 145 90 193cm 151cm Level 3 Normal slightly hard Also within the normal range 150 95 196cm 152cm Level 3.5 Swelling feeling Distinctive features and good drape 155 95 196cm 152cm Level 3.5 The board feels stiff enough Feels a bit hard
[0120] (3) Post-finishing wet finishing process:
[0121] White grey cloth raw repair → high temperature setting (190℃, speed 18m / min, overfeed 8%) → singeing → continuous boiling (85℃, 35m / min) → scouring (CIMI washing and shrinking combined machine, 45℃, 40min, 3kg detergent) → rope-shaped water absorption → flat washing and continuous boiling (85℃, Angora setting agent 2g / L) → drying (LB334, 145℃, 38m / min, overfeed 8%, 25002 width 172cm) → finishing → high temperature setting (190℃, speed 18m / min, overfeed 8%) → bio-mercerization finishing.
[0122] Performance Testing:
[0123] The following performance tests were performed on the products of Example 1 and Example 2, respectively. The test results are shown in Table 6 below.
[0124] Table 6
[0125]
[0126] Among them, the test method for wrinkle recovery refers to ISO 9867-2009, the test methods for relaxation shrinkage, felt shrinkage and total shrinkage refer to FZ / T 70009-2021 "Two-dimensional stability of washing resistance", and the extension test method under 30N force refers to FZ / T01034-2008; the test report number for 25001 is WUXT01471393; the test report number for 25002 is WUXT01471395.
[0127] The product prepared in the embodiment of the present invention has excellent machine washability, and its relaxed dimensional change rate and total dimensional change rate are much better than the first-class product index requirements of GB / T26382-2011 "Combed Wool Fabrics" for machine washable products after washing (relaxed dimensional change rate: width not less than -3%, length not less than -3%; total dimensional change rate width not less than -3%, length not less than -3%, edge not less than -1%).
[0128] It should be noted that, due to the large elasticity of spandex, the size of the fabric itself is unstable, and it is unrealistic to make it machine washable. Chemical mercerized wool is difficult to wrap the spandex due to its smooth surface, especially spinning high-count yarn (single yarn 40Nm, ply yarn 80Nm or more). At present, there is no report that all-wool + spandex woven fabric can be machine washed. The present invention creates a machine washable all-wool + spandex fabric that has both anti-wrinkle function and elasticity through innovation of design process and finishing process.
[0129] The inventors also compared the fiber fineness and whiteness of the products of Example 1 and Example 2 before and after bio-mercerization treatment. The specific results are shown in Table 7 below.
[0130] Table 7
[0131]
[0132] Among them, the fiber diameter determination method refers to ISO 137-2015, and the test report number of 25001 is WUXT01471390.
[0133] The whiteness test method refers to ISO 105-J02:1997, TW, 10-(+) green hue; (-) red hue; (0) light hue, and the test report number is WUXT01473680. After the biological mercerization finishing of the present invention, the whiteness of the grey cloth is increased by about 20%, which greatly improves the color brightness of the piece-dyed product and can produce piece-dyed fabrics with bright colors.
[0134] The inventors also used a microscope to observe the product of Example 1 before and after the bio-mercerization treatment at 500 times magnification. Figure 1 (After treatment, the fiber edges are clearly smooth) and Figure 2 (Before treatment, it is obvious that there are protrusions on the fiber surface caused by the edges of scales). It is found that the wool fiber treated with the bio-mercerization of the present invention is smoother and the whole process does not damage the wool fiber.
[0135] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them. It does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A pure wool fabric, characterized in that: The all-wool fabric is subjected to bio-mercerization finishing, wherein the bio-mercerization finishing comprises contacting the all-wool fabric with a first mixed solution containing a non-ionic penetrant and a first protease, and then contacting the all-wool fabric with a second mixed solution containing a non-ionic penetrant and a second protease, wherein the second protease is different from the first protease, The raw material of the all-wool fabric is wool or wool and elastic fiber. When the raw material of the all-wool fabric is wool, the all-wool fabric is woven by single yarn and ply yarn made of wool, the twist coefficient of the single yarn is 70-100, the twist coefficient of the ply yarn is 230-250, double warp and double weft weaving is adopted, the total tightness coefficient of the all-wool fabric is 90-100, and the ratio of the upper machine width to the lower machine width is (1.23-1.30):1; when the raw material of the all-wool fabric is wool and elastic fiber, the wool accounts for more than 95% of the total mass of the wool and elastic fiber, the all-wool fabric is woven by single yarn made of wool and elastic fiber, the twist coefficient of the single yarn is 150-160, single warp and single weft weaving is adopted, the total tightness coefficient of the all-wool fabric is 95-100, and the ratio of the upper machine width to the lower machine width is (1.25-1.33):
1.
2. The all-wool fabric according to claim 1, characterized in that: The first protease is copper blue oxidase, and the second protease is subtilisin.
3. The all-wool fabric according to claim 2, characterized in that: The first protease is specifically laccase, and the concentration of the first protease in the first mixed solution is 0.5-1.5 g / L; and / or, The second protease is specifically protease 16L, and the concentration of the second protease in the second mixed solution is 0.8-1 g / L.
4. The all-wool fabric according to claim 1, characterized in that: The nonionic penetrant includes one or more of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, the concentration of the nonionic penetrant in the first mixed solution is 0.5-1.5 g / L, and the concentration of the nonionic penetrant in the second mixed solution is 0.5-1.5 g / L; and / or, The pH of the second mixed solution is 8-10; and / or, The temperature of the all-wool fabric in contact with the first mixed liquid and the second mixed liquid is independently 50-60° C., and the time is independently 40-50 minutes; and / or, The bio-mercerization finishing further comprises performing enzyme inactivation treatment on the all-wool fabric after contact with the second mixed solution.
5. The all-wool fabric according to claim 1, characterized in that: The elastic fiber is spandex.
6. The all-wool fabric according to claim 1, characterized in that: The wrinkle resistance index of the all-wool fabric is ≥ level 3.5; the weft elasticity is greater than or equal to 7%; the relaxation size change rate: the width is not less than -3%, the length is not less than -3%; the total size change rate: the width is not less than -3%, the length is not less than -3%; the edge shrinkage rate: the width is not less than -1%, the length is not less than -1%.
7. The method for preparing the all-wool fabric according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: Step 1: making wool tops, selectively weaving the wool tops with elastic fibers into yarns, and then weaving them into grey cloth; Step 2, finishing the grey cloth to make the finished product; wherein the finishing includes raw repair → selective high temperature shaping → singeing → continuous boiling → washing → rope-shaped water absorption → flat washing and continuous boiling → drying → finished repair → selective high temperature shaping → bio-mercerization finishing → softening finishing → baking → shearing → wet storage → steaming → pre-shrinking → ironing → pre-shrinking → can steaming → finished product.
8. The preparation method according to claim 7, characterized in that: The bio-mercerization finishing specifically comprises the following steps: (1) immersing the grey cloth into a first mixed solution, wherein the first mixed solution comprises a nonionic penetrant and a laccase, wherein the concentration of the nonionic penetrant in the first mixed solution is 0.5-1.5 g / L, the concentration of the laccase is 0.5-1.5 g / L, the immersion temperature is 50-60° C., the immersion time is 40-50 min, and the bath ratio is 1:(5-15); (2) immersing the grey cloth treated with the first mixed solution into a second mixed solution, wherein the second mixture includes a nonionic penetrant and protease 16L, the pH of the second mixed solution is 8-10, the concentration of the nonionic penetrant is 0.5-1.5 g / L, the concentration of the protease 16L is 0.8-1 g / L, the immersion temperature is 50-60°C, the immersion time is 40-50 min, and the bath ratio is 1:(5-15); (3) Immersing the grey cloth treated with the second mixed solution into a third mixed solution, wherein the third mixed solution is an acid solution with a pH value of 4-4.5, an immersion temperature of 70-90° C., an immersion time of 5-10 min, and a bath ratio of 1:(10-15).
9. The preparation method according to claim 7, characterized in that: When the raw material of the all-wool fabric is wool, the step one specifically includes: wool top → blending → first needle combing → second needle combing → third needle combing → fourth needle combing → roving → spun yarn → automatic winding → paralleling → double twisting → steaming → warping → weaving → white grey cloth off the machine; when the raw materials of the all-wool fabric are wool and elastic fiber, the step one specifically includes: wool top → blending → first needle combing → second needle combing → third needle combing → fourth needle combing → roving → spun yarn → automatic winding → steaming → warping → weaving → white grey cloth off the machine; and / or, When the raw material of the all-wool fabric is wool, the post-finishing does not undergo high-temperature setting. When the raw materials of the all-wool fabric are wool and elastic fiber, the post-finishing undergoes high-temperature setting. The temperature of the high-temperature setting is 180-200° C. and the speed is 15-20 m / min.