A high-temperature resistant ink for PLA sanitary materials
By using titanate or zirconate chelate in inks, a combination of resin, filler and additives, to form a chelate coating, the insufficient adhesion and heat resistance of existing high-temperature resistant inks to PLA materials is solved. The problem of this problem achieves better adhesion and high temperature resistance, and reduces curling phenomenon.
Patent Information
- Application Number
- CN202310859625.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-07-13
AI Technical Summary
The existing high-temperature resistant inks have insufficient adhesion and heat resistance to PLA materials. Especially after using phthalate coupling agent to enhance the connection performance, the heat resistance is not significantly improved and it is easy to reverse sticking and curl.
Using titanate or zirconate chelate with resin, filler and additives to form a chelate coating to improve the adhesion and temperature resistance of ink to PLA materials, specifically including adding nanocarbonic acid to prefabricated semi-finished products Calcium, PU resin, nitrocellulose and modified rosin resins, and a high temperature resistant ink is formed through a specific mixing and stirring process.
It significantly improves the adhesion and high-temperature resistance of ink to PLA materials, reduces curling phenomenon, enhances the heat resistance and viscosity of ink, and meets the stable use needs in high-temperature environments.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printing inks, and in particular to a high temperature resistant ink for PLA sanitary materials. Background Art
[0002] PLA sanitary materials are appliances made of PLA materials. PLA materials refer to polylactic acid, also known as polylactide, which is a polyester polymer obtained by polymerization of lactic acid as the main raw material. It is a new type of biodegradable material. However, PLA sanitary materials have poor tolerance to high temperatures and require an external coating to enable PLA sanitary materials to withstand high temperatures. Existing high-temperature resistant inks do not have good adhesion to PLA, and inks that can achieve relevant adhesion properties cannot achieve relevant high-temperature resistance properties. In the field of inks, phthalates are often used to strengthen the connection between inks and PLA sanitary materials, but they have poor heat resistance and are prone to anti-sticking and curling.
[0003] Phthalate esters (PAEs), also known as phthalic acid esters, are mainly used in polyvinyl chloride materials to change polyvinyl chloride from hard plastic to elastic plastic, playing the role of plasticizer. In the prior art, inks are prepared using phthalate-related coupling agents during the preparation process. For example, in CN111019432A, the hydrophilic and hydrophobic groups in the phthalate coupling agent are used to cross-link with substances of different properties through reactions. However, its connection performance enhances the mechanical properties, but the improvement in heat resistance is not very significant. Summary of the invention
[0004] In view of this, the present invention provides a high temperature resistant ink for PLA sanitary materials, which can greatly improve the adhesion of the ink to the PLA sanitary materials and also improve the high temperature resistance of the ink.
[0005] In order to solve the above technical problems, the present invention provides a high temperature resistant ink for PLA sanitary materials, wherein the high temperature resistant ink has different components in two types of pigments, the two types of pigments include organic color and carbon black pigment types and white pigment types, and the high temperature resistant ink includes the following components:
[0006] Prefabricated semi-finished products, nano calcium carbonate, titanate, supplements;
[0007] The prefabricated semi-finished product includes a mixed solvent, a connecting material, a pigment, and an additive;
[0008] The connecting material comprises PU resin+nitrocellulose and modified rosin resin.
[0009] The present invention encapsulates the pigment by combining titanate chelate or zirconate chelate with resin, filler and additives. The chelate coating formed by the components has good bonding strength with the substrate, thereby making the ink coating have good adhesion and temperature resistance on the PLA degradable film.
[0010] Furthermore, the high temperature resistant ink of the organic color and carbon black pigment type comprises the following components in parts by weight:
[0011] Prefabricated semi-finished products 75%, nano calcium carbonate 10%, titanate 1% to 3%, supplemented to 100% with supplements;
[0012] The prefabricated semi-finished product comprises 45% of mixed solvent, 25% of connecting material, 25% of pigment and 10% of auxiliary agent;
[0013] The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
[0014] Furthermore, the high temperature resistant ink of the organic color and carbon black pigment type comprises the following components in parts by weight:
[0015] Prefabricated semi-finished products 75%, nano calcium carbonate 15%, titanate 1% to 3%, supplemented to 100% with supplements;
[0016] The prefabricated semi-finished product comprises 45% of mixed solvent, 25% of connecting material, 25% of pigment and 10% of auxiliary agent;
[0017] The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
[0018] Furthermore, the white pigment type high temperature resistant ink comprises the following components in parts by weight:
[0019] Prefabricated semi-finished product 55%, nano calcium carbonate 10%, titanate 1% to 3%, supplemented to 100% with supplements;
[0020] The prefabricated semi-finished product comprises 20% of mixed solvent, 20% of connecting material, 50% of titanium dioxide pigment and 10% of auxiliary agent;
[0021] The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
[0022] Furthermore, the high temperature resistant ink of the organic color and carbon black pigment type
[0023] Mixed solvent: n-propyl acetate: ethyl acetate: anhydrous ethanol: propylene glycol methyl ether = 50:20:10:20;
[0024] In the additive mixed paste, ethyl acetate: dispersant: plasticizer: polyethylene wax powder = 10: 10: 40: 40;
[0025] The supply is a mixture of ethanol and ethyl acetate, and the ratio of ethanol to ethyl acetate is 1:1.
[0026] Further, the mixed solvent: n-propyl acetate: ethyl acetate: anhydrous ethanol: propylene glycol methyl ether = 50:25:15:10;
[0027] The ratio of the additive mixed paste: ethyl acetate: dispersant: plasticizer: polyethylene wax powder = 10:10:40:40.
[0028] Furthermore, the auxiliary agent includes a dispersant, polyethylene wax powder, a plasticizer, and an anti-precipitation agent;
[0029] The mixed solvent comprises ethanol, ethyl acetate, n-propyl acetate, propylene glycol methyl ether and propylene glycol methyl ether acetate.
[0030] Further, the method comprises the following preparation steps:
[0031] S1, mixing the mixed solvent and dividing it into a mixed liquid A and a mixed liquid B, adding a plasticizer and nitrocellulose to the mixed liquid A and stirring until the mixed liquid is completely dissolved to obtain a semi-finished liquid;
[0032] S2, adding a connecting material and remaining additives to the semi-finished product liquid to form a prefabricated semi-finished product, adding nano calcium carbonate to the prefabricated semi-finished product, setting the stirring speed to 600-1500 r / min, and the stirring time to 30-60 min to obtain a paste;
[0033] S3, grinding the paste 3 to 5 times, and mixing it with the mixed liquid B to obtain a semi-finished product of high temperature resistant ink;
[0034] S4. After the temperature of the semi-finished high temperature resistant ink is lower than 50°C, add phthalate to the semi-finished high temperature resistant ink, set the stirring speed to 500-900r / min, and the stirring time to 15-30min. After the stirring is completed, filter to obtain the finished high temperature resistant ink.
[0035] During the printing and coating process, after the solvent in the ink evaporates after passing through the drying oven, the pigment, binder and additives form a chelate coating in the titanate chelate or zirconate chelate, and each component has a good bonding strength with the substrate.
[0036] Furthermore, the volume ratio of the mixed liquid A to the mixed liquid B is 3 to 8:2.
[0037] Furthermore, the fineness of the paste after grinding is ≤5 μm. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0039] Embodiment 1
[0040] In this embodiment, high temperature resistant ink of organic pigment is prepared, and the organic pigment adopts the following types:
[0041] Yellow powder PY13, PY83, PY150, red powder PR2, PR48:2, PR48:3, PR:53:1, PR57:1, PR146, PR254, PR170 (5RK), PR122, PO5 blue powder PB15:3, PB15:4, green powder PG7, purple powder PV23, black 100# carbon black.
[0042] Additives include dispersants, polyethylene wax powder, plasticizers, and anti-precipitation agents;
[0043] The mixed solvent consists of ethanol, ethyl acetate, n-propyl acetate, propylene glycol methyl ether, and propylene glycol methyl ether acetate;
[0044] First, the ratio of each component is determined. In this embodiment, the ratio of prefabricated semi-finished product A: nano-calcium carbonate: titanate = 75:10:1 is used for weighing and configuration. Then, the ratio of 45% of the mixed solvent to 25% of the connecting material, 20% of the pigment, and 10% of the auxiliary agent in the prefabricated semi-finished product is determined, and the preparation method described below is carried out;
[0045] S1, mixing the mixed solvent and dividing it into a mixed liquid A and a mixed liquid B, adding a plasticizer and nitrocellulose to the mixed liquid A and stirring until the mixed liquid is completely dissolved to obtain a semi-finished liquid;
[0046] S2, adding a connecting material and remaining additives to the semi-finished product liquid to form a prefabricated semi-finished product, adding nano calcium carbonate to the prefabricated semi-finished product, setting the stirring speed to 600-1500 r / min, and the stirring time to 30-60 min to obtain a paste;
[0047] S3, grinding the paste 3 to 5 times, and mixing it with the mixed liquid B to obtain a semi-finished product of high temperature resistant ink;
[0048] S4. After the temperature of the semi-finished high temperature resistant ink is lower than 50°C, add phthalate to the semi-finished high temperature resistant ink, set the stirring speed to 500-900r / min, and the stirring time to 15-30min. After the stirring is completed, filter to obtain the finished high temperature resistant ink.
[0049] The finished liquid high temperature resistant ink is stored and matured at room temperature for 24 hours, and then its performance is tested.
[0050] In this embodiment, the proportion of the connecting material is changed as follows:
[0051] 1. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:30:20;
[0052] 2. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 30:30:40;
[0053] 3. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 15:30:55;
[0054] 4. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 60:20:20;
[0055] 5. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 70:10:20;
[0056] 6. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:20:30;
[0057] 7. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:10:40;
[0058] 8. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 60:30:10;
[0059] 9. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 70:30:0.
[0060] Embodiment 2
[0061] The difference between this embodiment and the first embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 75:10:3 for weighing and configuration.
[0062] Embodiment 3
[0063] The difference between this embodiment and the first embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 75:10:5 for weighing and configuration.
[0064] Embodiment 4
[0065] The difference between this embodiment and the first embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 75:10:7 for weighing and configuration.
[0066] Embodiment 5
[0067] The difference between this embodiment and the first embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 75:15:1 for weighing and configuration.
[0068] Embodiment 6
[0069] The difference between this embodiment and the first embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 75:15:3 for weighing and configuration.
[0070] Experimental Project
[0071] The above embodiment is subjected to various experimental measurements of 17 kinds of pigments, and the experimental method is as follows:
[0072] The viscosity of the finished ink is 15 to 35 seconds / 4# Zahn cup: Test conditions: 25±1℃, 4# Zahn cup. When the viscosity is ≥55 seconds, it is marked as "-", which means it does not meet the basic design requirements, and other properties are not tested as "-".
[0073] Adhesion test: dilute the ink 100: (anhydrous ethanol: ethyl acetate = 1:1 mixture) 30, and dry it in a PLA degradable film coating oven at 65°C for 1 hour until the bottom is dry; after sticking the coating layer with 3M tape, observe the ink adhered to the tape and calculate it)
[0074] Curl: Dilute the ink 100: (anhydrous ethanol: ethyl acetate = 1:1 mixture) 30, then coat on PLA degradable film and dry in oven at 65℃ for 1h until the bottom is cut. Coat 10cmx10cm, and measure four upward angles at the center point. ≤5° indicates no obvious; 5°~10° is slight; 10°~15° is obvious; ≥15° is serious; (coat three films and take the average value)
[0075] Temperature resistance test: heat sealer (upper and lower heating, pressure 2KG force)
[0076] In Example 1, the experimental data of the number 1, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:30:20 is as follows:
[0077]
[0078]
[0079] In Example 1, the experimental data of the number 2, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 30:30:40, are as follows:
[0080]
[0081] In Example 1, the experimental data of the number 3, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 15:30:55 is as follows:
[0082]
[0083]
[0084] In Example 1, the experimental data of the number 4, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 60:20:20, are as follows:
[0085]
[0086] In Example 1, the experimental data of the number 5, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:10:20 is as follows:
[0087]
[0088]
[0089] In Example 1, the experimental data of the number 6, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:20:30 is as follows:
[0090]
[0091] In Example 1, the experimental data of the number 7, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:10:40 is as follows:
[0092]
[0093]
[0094] In Example 1, the experimental data of the number 7, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 60:30:10 is as follows:
[0095]
[0096] In Example 1, the sample No. 8 has a connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:30:10. The experimental data obtained show that the curling is not obvious and the sample is resistant to anti-sticking at 90°C.
[0097] In Example 1, the experimental data of the sample No. 9, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:30:0, are as follows:
[0098]
[0099] In Example 2, numbered 1, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 50:30:20 are as follows:
[0100]
[0101] In Example 2, the experimental data of the number 2, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 30:30:40, are as follows:
[0102]
[0103]
[0104] In Example 2, the experimental data of number 3, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 15:30:55, are as follows:
[0105]
[0106] In Example 2, numbered 4, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:20:20 are as follows:
[0107]
[0108]
[0109] In Example 2, numbered 5, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 70:10:20 are as follows:
[0110]
[0111] In Example 2, numbered 6, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 50:20:30 are as follows:
[0112]
[0113]
[0114] In Example 2, number 7, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 50:10:40 are as follows:
[0115]
[0116] In Example 2, No. 8, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 60:30:10, and the experimental data obtained are all that the curling is not obvious.
[0117] In Example 2, No. 9, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 70:30:0, and the experimental data obtained are all serious curling.
[0118] In Example 3, the experimental data of the number 1, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:30:20 is as follows:
[0119]
[0120] In Example 3, the experimental data of No. 2, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 30:30:40, are as follows:
[0121]
[0122]
[0123] In Example 3, the experimental data of the number 3, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 15:30:55, are as follows:
[0124]
[0125] In Example 3, numbered 4, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:20:20 are as follows:
[0126]
[0127]
[0128] In Example 3, No. 5, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 70:10:20. The experimental data obtained are all severe curling and no anti-sticking.
[0129] In Example 3, the experimental data of No. 6, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:20:30, are as follows:
[0130]
[0131] In Example 3, the experimental data of No. 7, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:10:40, are as follows:
[0132]
[0133]
[0134] In Example 3, No. 8, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 60:30:10, and the experimental data obtained are all that the curling is not obvious.
[0135] In Example 3, No. 9, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 70:30:0, and the experimental data obtained are all serious curling.
[0136] In Example 4, which is numbered 1, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 50:30:20, and the experimental data obtained all show severe curling.
[0137] In Example 4, numbered 2, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 30:30:40 are as follows:
[0138]
[0139]
[0140] In Example 4, numbered 3, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 15:30:55 are as follows:
[0141]
[0142] In Example 4, numbered 4, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:20:20 are as follows:
[0143]
[0144]
[0145] In Example 4, No. 5, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 70:10:20, and the experimental data obtained are all normal curling without anti-sticking.
[0146] In Example 4, No. 6, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:20:30, and the experimental data obtained are all severe curling and no anti-sticking
[0147] In Example 4, numbered 7, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 50:10:40 are as follows:
[0148]
[0149] In Example 4, the finished product of high temperature resistant ink numbered 8, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 60:30:10, generally has high viscosity and is meaningless to test, and the performance test is cancelled.
[0150] In Example 4, the finished product of high temperature resistant ink numbered 9, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:30:0, generally has high viscosity and is meaningless to test, and the performance test is cancelled.
[0151] In Example 5, the experimental data of number 1, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:30:20 is as follows:
[0152]
[0153] In Example 5, the experimental data of number 2, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 30:30:40, are as follows:
[0154]
[0155]
[0156] In Example 5, the experimental data of No. 3, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 15:30:55, are as follows:
[0157]
[0158] In Example 5, numbered 4, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:20:20 are as follows:
[0159]
[0160]
[0161] In Example 5, numbered 5, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 70:10:20, and the experimental data obtained all show severe curling.
[0162] In Example 5, No. 6, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 50:20:30, and the experimental data obtained all show severe curling.
[0163] In Example 5, No. 7, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 50:10:40, and the experimental data obtained are all serious curling.
[0164] In Example 5, the finished product No. 8, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 60:30:10, has a generally high viscosity of the high temperature resistant ink, which is meaningless to test, and the performance test is cancelled.
[0165] In Example 5, the finished product No. 9, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:30:0, has a generally high viscosity of the high temperature resistant ink, which is meaningless to test, and the performance test is cancelled.
[0166] In Example 6, the experimental data of the number 1, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:30:20 is as follows:
[0167]
[0168]
[0169] In Example 6, the experimental data of number 2, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 30:30:40, are as follows:
[0170]
[0171] In Example 6, the experimental data of number 3, where the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 15:30:55, are as follows:
[0172]
[0173]
[0174] In Example 6, numbered 4, the experimental data of the connecting material ratio of nitrocellulose: PU resin: modified rosin resin = 60:20:20 are as follows:
[0175]
[0176] In Example 6, No. 5, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:10:20, and the experimental data obtained all show curling.
[0177] In Example 6, numbered 6, the ratio of the connecting materials is nitrocellulose: PU resin: modified rosin resin = 50:20:30, and the experimental data obtained all show curling.
[0178] In Example 6, No. 7, the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 50:10:40, and the experimental data obtained all show curling.
[0179] In Example 6, the finished product of high temperature resistant ink numbered 8, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 60:30:10, generally has high viscosity and is meaningless to test, and the performance test is cancelled.
[0180] In Example 6, the finished product of high temperature resistant ink numbered 9, in which the ratio of the connecting material is nitrocellulose: PU resin: modified rosin resin = 70:30:0, generally has high viscosity and is meaningless to test, and the performance test is cancelled.
[0181] Analysis: From Examples 1 to 6, it can be seen that for organic color and carbon black inks, the temperature resistance of titanate chelate (zirconate chelate) increases with the increase of titanate chelate. The increase of titanate chelate will improve the adhesion of ink and increase the viscosity.
[0182] Embodiment 7
[0183] In this embodiment, a high temperature resistant ink with a white pigment is prepared. The white pigment is a titanium dioxide pigment with a model of Zhongti R606.
[0184] Additives include dispersants, polyethylene wax powder, plasticizers, and anti-precipitation agents;
[0185] The mixed solvent includes ethanol + ethyl acetate + n-propyl acetate + propylene glycol methyl ether + propylene glycol methyl ether acetate (two or more);
[0186] First, the ratio of each component is determined. In this embodiment, the ratio of prefabricated semi-finished product A: nano-calcium carbonate: titanate = 55:10:1 is used for weighing and configuration. Then, the ratio of 20% of the mixed solvent to 20% of the connecting material, 50% of the pigment, and 10% of the auxiliary agent in the prefabricated semi-finished product is determined, and the preparation method described below is carried out;
[0187] S1, mixing organic solvents of n-propyl acetate, ethyl acetate, anhydrous ethanol and propylene glycol methyl ether in a ratio of 50:20:10:20, and dividing into mixed liquid A and mixed liquid B, adding plasticizer and nitrocellulose to the mixed liquid A and stirring until completely dissolved to obtain a semi-finished product liquid;
[0188] S2, adding PU resin, dispersant, titanium dioxide pigment, polyethylene wax powder and nano calcium carbonate to the semi-finished product liquid, setting the stirring speed to 600-1500r / min, and the stirring time to 30-60min to obtain a paste;
[0189] S3, grinding the paste 3 to 5 times, and mixing it with the mixed liquid B to obtain a semi-finished product of high temperature resistant ink;
[0190] S4. After the temperature of the semi-finished high temperature resistant ink is lower than 50°C, add phthalate to the semi-finished high temperature resistant ink, set the stirring speed to 500-900r / min, and the stirring time to 15-30min. After the stirring is completed, filter to obtain the finished high temperature resistant ink.
[0191] The finished liquid high temperature resistant ink is stored and matured at room temperature for 24 hours, and then its performance is tested.
[0192] In this embodiment, the proportion of the connecting material is changed as follows:
[0193] 1. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:30:20;
[0194] 2. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 30:30:40;
[0195] 3. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 15:30:55;
[0196] 4. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 60:20:20;
[0197] 5. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 70:10:20;
[0198] 6. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:20:30;
[0199] 7. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 50:10:40;
[0200] 8. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 60:30:10;
[0201] 9. Connecting material ratio: nitrocellulose: PU resin: modified rosin resin = 70:30:0.
[0202] Embodiment 8
[0203] The difference between this embodiment and the seventh embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 55:10:3 for weighing and configuration.
[0204] Embodiment 9
[0205] The difference between this embodiment and the seventh embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 55:10:5 for weighing and configuration.
[0206] Embodiment 10
[0207] The difference between this embodiment and the seventh embodiment is that this embodiment uses the prefabricated semi-finished product A: nano-calcium carbonate: titanate in a ratio of 55:10:7 for weighing and configuration.
[0208] Experimental Project
[0209] The above embodiment is subjected to various experimental measurements of 17 kinds of pigments, and the experimental method is as follows:
[0210] The viscosity of the finished ink is 15 to 35 seconds / 4# Zahn cup: Test conditions: 25±1℃, 4# Zahn cup. When the viscosity is ≥55 seconds, it is marked as "-", which means it does not meet the basic design requirements, and other properties are not tested as "-".
[0211] Adhesion test: dilute the ink 100: (anhydrous ethanol: ethyl acetate = 1:1 mixture) 30, and dry it in a PLA degradable film coating oven at 65°C for 1 hour until the bottom is dry; after sticking the coating layer with 3M tape, observe the ink adhered to the tape and calculate it)
[0212] Curl: Dilute the ink 100: (anhydrous ethanol: ethyl acetate = 1:1 mixture) 30, then coat on PLA degradable film and dry in oven at 65℃ for 1h until the bottom is cut. Coat 10cmx10cm, and measure four upward angles at the center point. ≤5° indicates no obvious; 5°~10° is slight; 10°~15° is obvious; ≥15° is serious; (coat three films and take the average value)
[0213] Temperature resistance test: heat sealer (upper and lower heating, pressure 2KG force)
[0214] The test data of each ratio numbered 1-9 in Example 7 are as follows:
[0215]
[0216] The test data of each ratio numbered 1-9 in Example 8 are as follows:
[0217]
[0218]
[0219] The test data of each ratio numbered 1-9 in Example 9 are as follows:
[0220]
[0221] The test data of each ratio numbered 1-9 in Example 10 are as follows:
[0222]
[0223]
[0224] Analysis: From Examples 7 to 10, it can be seen that for white pigment inks, the heat resistance of titanate chelates (zirconate chelates) increases with the increase of titanate chelates, but the yellowing resistance decreases with the increase of modified rosin resin. The increase of titanate chelates will improve the adhesion of the ink and increase the viscosity.
[0225] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high temperature resistant ink for PLA sanitary materials, characterized in that: The high temperature resistant ink comprises the following components: Prefabricated semi-finished products, nano calcium carbonate, titanate, supplements; The prefabricated semi-finished product includes a mixed solvent, a connecting material, a pigment, and an additive; The connecting material comprises PU resin, nitrocellulose and modified rosin resin; The high temperature resistant ink comprises the following components in parts by weight: Prefabricated semi-finished products 55%-75%, nano calcium carbonate 10-15%, titanate 1%-3%, supplemented to 100% with supplements; The prefabricated semi-finished product comprises 20-45% of mixed solvent, 20-25% of connecting material, 20-50% of pigment and 10% of auxiliary agent; The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
2. The high temperature resistant ink for PLA sanitary materials according to claim 1, characterized in that: The high temperature resistant ink comprises the following components in parts by weight: Prefabricated semi-finished products 75%, nano calcium carbonate 15%, titanate 1% to 3%, supplemented to 100% with supplements; The prefabricated semi-finished product comprises 45% of mixed solvent, 25% of connecting material, 20% of pigment and 10% of auxiliary agent; The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
3. The high temperature resistant ink for PLA sanitary materials according to claim 1, characterized in that: The white pigment type high temperature resistant ink comprises the following components in parts by weight: Prefabricated semi-finished product 55%, nano calcium carbonate 10%, titanate 1% to 3%, supplemented to 100% with supplements; The prefabricated semi-finished product comprises 20% of mixed solvent, 20% of connecting material, 50% of titanium dioxide pigment and 10% of auxiliary agent; The connecting material comprises 10-30% of PU resin, 15-70% of nitrocellulose and 0-30% of modified rosin resin.
4. The high temperature resistant ink for PLA sanitary materials according to claim 1, characterized in that: The mixed solvent comprises n-propyl acetate, ethyl acetate, anhydrous ethanol and propylene glycol methyl ether, and the weight ratio of n-propyl acetate, ethyl acetate, anhydrous ethanol and propylene glycol methyl ether is 50:20 to 25:10 to 15:20; The auxiliary agent includes ethyl acetate, a dispersant, a plasticizer and polyethylene wax powder, and the weight ratio of the ethyl acetate, the dispersant, the plasticizer and the polyethylene wax powder is 10:10:40:
40.
5. The high temperature resistant ink for PLA sanitary materials according to claim 1, characterized in that: The tonic is a mixed solution of ethanol and ethyl acetate, and the weight ratio of the ethanol to ethyl acetate is 1:
1.
6. The high temperature resistant ink for PLA sanitary materials according to claim 4, characterized in that: The auxiliary agent also includes an anti-precipitation agent.
7. A method for preparing a high temperature resistant ink for PLA sanitary materials, characterized in that: The method comprises the following preparation steps: S1, mixing the mixed solvent and dividing it into a mixed liquid A and a mixed liquid B, adding a plasticizer and nitrocellulose to the mixed liquid A and stirring until the mixed liquid is completely dissolved to obtain a semi-finished liquid; S2, adding a binder, a pigment, an additive and a supplement to the semi-finished product liquid to form a prefabricated semi-finished product, adding nano calcium carbonate to the prefabricated semi-finished product, setting the stirring speed to 600-1500 r / min, and the stirring time to 30-60 min to obtain a paste; the binder includes PU resin, nitrocellulose and modified rosin resin; S3, grinding the paste 3 to 5 times, and mixing it with the mixed liquid B to obtain a semi-finished product of high temperature resistant ink; S4. After the temperature of the semi-finished high temperature resistant ink is lower than 50°C, titanate is added to the semi-finished high temperature resistant ink, the stirring speed is set to 500-900r / min, the stirring time is 15-30min, and after the stirring is completed, filtering is performed to obtain the finished high temperature resistant ink.
8. The method for preparing the high temperature resistant ink for PLA sanitary materials according to claim 7, characterized in that: The volume ratio of the mixed liquid A to the mixed liquid B is 3 to 8:
2.
9. The method for preparing the high temperature resistant ink for PLA sanitary materials according to claim 7, characterized in that: The fineness of the paste after grinding is ≤5 μm.