A method for preparing copper alloy touch target material for touch device

By doping elements such as Zr, Cr, Zn, and Al in copper alloys and using specific processes, the problem of insufficient oxidation resistance of copper targets in high-temperature environments is solved, high conductivity and stability are achieved, and the film is ensured. layer performance at high temperatures.

CN117305783BActive Publication Date: 2024-10-22GEMCH MATERIAL TECH SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311183821.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-14
Publication Date
2024-10-22
Estimated Expiration
2043-09-14

AI Technical Summary

Technical Problem

Existing copper targets have insufficient antioxidant capacity in high-temperature environments, and improvements on the market have little impact on conductivity or may pose safety risks.

Method used

By doping copper alloys with elements such as Zr, Cr, Zn, and Al, and using vacuum smelting, rolling and annealing processes, high-purity alloy targets are prepared to ensure the conductivity and oxidation resistance of the film layer, and through inertness Gas removal and vacuum environment reduce oxygen content.

Benefits of technology

The stability and conductive performance of the film layer in high-temperature environments have been improved. The conductivity has reached ≥70% IACS, and the resistance value change rate has been maintained at ≤10% in a 170°C humidity environment, improving the overall performance and safety of the target. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117305783B_ABST
    Figure CN117305783B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a copper alloy touch target material of a touch device, and the technical scheme thereof mainly comprises the following specific steps: step 1, selection and proportion of target material doping elements: according to the final required film layer performance, the target material element doping elements are selected and calculated from Zr, Cr, Zn and Al, and the types and proportions of the target material element doping elements are analyzed; step 2, vacuum melting: the single substance or alloy raw material with the calculated proportion is put into a vacuum melting furnace; composition innovation, film layer stability: the pure copper target material has a very high conductivity after film coating, and one or more of the elements such as Zr, Cr, Zn and Al are doped to enhance the oxidation resistance and mechanical strength of the target material coating film layer, and the film layer conductivity is satisfied to be ≥70% IACS, and the oxygen content in the finished product can also be reduced by introducing inert gas for sufficient exhaust, thereby improving the purity of the final product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper alloy touch target materials, and in particular to a method for preparing a copper alloy touch target material for a touch device. Background Art

[0002] The coating target is a sputtering source that forms various functional thin films on the substrate through magnetron sputtering, multi-arc ion plating or other types of coating systems under appropriate process conditions. Simply put, the target material is the target material bombarded by high-speed energetic particles. When used in high-energy laser weapons, lasers with different power densities, different output waveforms, and different wavelengths interact with different target materials, different killing and destructive effects will be produced.

[0003] For example, the Chinese patent with the authorization announcement number CN214422738U discloses a copper target material, which belongs to the field of sputtering materials. The copper target material includes a plurality of grain-boundary-free copper layers stacked along the thickness direction of the target material, and each grain-boundary-free copper layer has the same lattice orientation and is one of Cu(111), Cu(110), Cu(211) and Cu(100).

[0004] The copper target material mentioned above has the advantage of good overall consistency; however, the copper target material mentioned above and the target materials commonly used on the market still have some disadvantages, such as: this target material has a very high electrical conductivity, but the antioxidant capacity of the film layer prepared by it cannot meet the requirements of long-term baking in a high-temperature environment, so it is necessary to improve its antioxidant capacity; there are also CuAl alloy targets on the market, which can meet its antioxidant capacity, but the electrical conductivity cannot meet ≥70% IACS; and the Ag element can enhance its mechanical properties, but has little effect on the enhancement of its antioxidant capacity; Fe has a fatal effect on semiconductor materials, and Mg has an impact on another component of the display. The increase of rare earth can enhance its ability to resist scandium corrosion, but rare earth is sensitive to oxygen and can easily absorb oxygen elements to turn the alloy into oxides, and there are safety risks. Summary of the invention

[0005] In view of the problems mentioned in the background technology, an object of the present invention is to provide a method for preparing a copper alloy touch target material of a touch device to solve the problems mentioned in the background technology.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] A method for preparing a copper alloy touch target material for a touch device comprises the following specific steps:

[0008] Step 1, selection and ratio of target material doping elements: according to the final required film performance, select and calculate from Zr, Cr, Zn, and Al, and analyze the type and ratio of target material doping elements;

[0009] Step 2, vacuum melting: put the calculated proportion of single element or alloy raw materials into the vacuum melting furnace;

[0010] Step 3, heating the vacuum melting furnace: according to the different alloy elements and contents, the temperature is set at 1000°C-1300°C, the vacuum melting furnace is heated to melt the single substance or alloy raw materials in the melting furnace, and the vacuum degree in the vacuum melting furnace is maintained;

[0011] Step 4, ventilation and impurity removal: After all the raw materials are melted, inert gas is introduced into the vacuum melting furnace to help the gas impurities generated after the metal solution is heated to float up and discharge, thereby removing impurities and finally obtaining a high-purity alloy target;

[0012] Step 5: Casting and molding of alloy target: Casting is performed under vacuum to ensure the fluidity of the high-temperature solution, and the alloy ingot is obtained by cooling and shaping;

[0013] Step 6, high-purity alloy target rolling treatment: the smelted alloy ingot is rolled using a hot rolling mill, the heating furnace temperature is set to 700°C-900°C, after the temperature is reached, the ingot is placed in the heating furnace for 1.5-3h, and then 5-10 rolling processes are performed;

[0014] Step 7, annealing treatment of high-purity alloy target: annealing treatment of the leveled high-purity alloy target at 500° C. to 700° C. for 1 to 1.5 hours;

[0015] Step 8, milling of high-purity alloy target: using milling machine equipment to perform surface milling on the high-purity alloy target, with an average particle size of 80 to 120 μm;

[0016] Step 9. Application of high-purity alloy target: Use metallization bonding method to bond it to the backplane of required size, so as to obtain high-conductivity copper alloy touch flat target for high-end touch devices. The size of the target is not limited.

[0017] Preferably, the doping mass of the Zr element is 1%-2%; the doping mass of the Cr element is 0.4%-1.1%, the doping mass of the Zn element is 0.03%-0.3%, and the doping mass of the Al element is 0.5%-0.7%.

[0018] Preferably, in step 2, the vacuum melting chamber is evacuated to 0.1-2.0 Pa.

[0019] Preferably, in step 3, the casting mold is preheated at the same time to prevent the high-temperature solution from solidifying instantly when the mold is cold, thereby preventing shrinkage cavities from forming poorly.

[0020] Preferably, in said step 5, during the alloy forming process, the oxygen content is controlled to be ≤160ppm.

[0021] Preferably, in the step 6, during the alloy target rolling process, the total deformation of the aluminum-scandium plate is controlled to be above 90%, the thickness is 5-15 mm, and a leveling machine is used to level the plate to ensure its flatness.

[0022] Preferably, in order to minimize the melting temperature difference during the melting process, the composition and proportion of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram.

[0023] Preferably, in step 9, when the performance of the planar target meets the requirements, a rotating target can be developed to improve its utilization rate, and the specific steps are as follows:

[0024] Step 1: Use a vacuum melting furnace for melting and casting, the process is the same as steps 1-5 of the planar target;

[0025] Step 2: Extrude the smelted alloy ingot and form it in one step by perforation extrusion to achieve the required size;

[0026] Step 3: Cut and machine the extruded tube to obtain a blank with the inner and outer diameters of the finished product;

[0027] Step 4: Calculate the length and amount of the blank based on the finished target material, and use the metallization bonding method to prepare the finished high-conductivity copper alloy touch rotary target material. The target material prepared in this way is not limited by size.

[0028] Preferably, in the step 2, the raw materials are fed in a uniform staggered manner during vacuum smelting.

[0029] In summary, the present invention mainly has the following beneficial effects:

[0030] First, in the preparation method of copper alloy touch target for touch device, the composition is innovative and the film layer is stable: the pure copper target has a high conductivity after coating, but its antioxidant capacity is not enough. In a 120°C environment, the film layer is easily oxidized. Doping with one or more elements such as Zr, Cr, Zn, Al, etc. can enhance the oxidation resistance and mechanical strength of the target coating film layer, and meet the film conductivity ≥ 70% IACS; melt uniformity: in order to minimize the melting temperature difference during the melting process, the composition and ratio of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram, thereby avoiding the phenomenon of severe oxidation of individual elements caused by excessive temperature difference;

[0031] Second, in the preparation method of copper alloy touch target materials for touch control devices, composition uniformity: a uniform staggered feeding method is adopted during the raw material feeding process to reduce composition segregation; oxygen content also has a certain influence on the performance of the final target material. In the entire process route, the melt casting and cooling are in a vacuum environment, which reduces the oxidation of the material, and the introduction of inert gas for sufficient exhaust can also reduce the oxygen content in the finished product, thereby improving the purity of the final product and increasing the composition uniformity; fine and uniform grains: the target material prepared by the rolling process can well refine the grains, and after heat treatment, the grains can be made more uniform, and uniform target material performance will result in uniform film layer performance; film layer stability: the film layer after coating the copper alloy target material doped with the above elements can be baked for 60 minutes in an environment of 170°C and 40% humidity, and the resistance value change rate is ≤10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] refer to Figure 1 A method for preparing a copper alloy touch target material for a touch device, comprising the following specific steps:

[0036] Step 1, selection and ratio of target material doping elements: according to the final required film performance, select and calculate from Zr, Cr, Zn, and Al, and analyze the type and ratio of target material doping elements;

[0037] Step 2, vacuum melting: put the calculated proportion of single element or alloy raw materials into the vacuum melting furnace;

[0038] Step 3, heating the vacuum melting furnace: according to the different alloy elements and contents, the temperature is set to 1000°C, the vacuum melting furnace is heated to melt the single substance or alloy raw materials in the melting furnace, and the vacuum degree in the vacuum melting furnace is maintained;

[0039] Step 4, ventilation and impurity removal: After all the raw materials are melted, inert gas is introduced into the vacuum melting furnace to help the gas impurities generated after the metal solution is heated to float up and discharge, thereby removing impurities and finally obtaining a high-purity alloy target;

[0040] Step 5: Casting and molding of alloy target: Casting is performed under vacuum to ensure the fluidity of the high-temperature solution, and the alloy ingot is obtained by cooling and shaping;

[0041] Step 6, high-purity alloy target rolling treatment: the smelted alloy ingot is rolled using a hot rolling mill, the heating furnace temperature is set to 700°C, and after the temperature reaches 700°C, the ingot is placed in the heating furnace for 1.5 hours, followed by 5 rolling processes;

[0042] Step 7, annealing treatment of high-purity alloy target: annealing treatment of the leveled high-purity alloy target at 500° C. for 1 hour;

[0043] Step 8: Milling of high-purity alloy target: Use milling machine equipment to perform surface milling on the high-purity alloy target, with an average particle size of 80 μm;

[0044] Step 9. Application of high-purity alloy target: Use metallization bonding method to bond it to the backplane of required size, so as to obtain high-conductivity copper alloy touch flat target for high-end touch devices. The size of the target is not limited.

[0045] Preferably, the doping mass of the Zr element is 1%; the doping mass of the Cr element is 0.4%, the doping mass of the Zn element is 0.03%, and the doping mass of the Al element is 0.5%.

[0046] Preferably, in step 2, the vacuum melting chamber is evacuated to 0.1 Pa.

[0047] Preferably, in step 3, the casting mold is preheated at the same time to prevent the high-temperature solution from instantly solidifying and shrinking when the mold is cold, resulting in poor molding.

[0048] Preferably, in step 5, during the alloy forming process, the oxygen content is controlled to be ≤160ppm.

[0049] Preferably, in step 6, during the alloy target rolling process, the total deformation of the aluminum-scandium plate is controlled to be above 90%, the thickness is 5 mm, and a leveling machine is used to level the plate to ensure its flatness.

[0050] Preferably, in order to minimize the melting temperature difference during the melting process, the composition and proportion of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram.

[0051] Preferably, in step 9, when the performance of the planar target meets the requirements, a rotating target can be developed to improve its utilization rate. The specific steps are as follows:

[0052] Step 1: Use a vacuum melting furnace for melting and casting, the process is the same as steps 1-5 of the planar target;

[0053] Step 2: Extrude the smelted alloy ingot and form it in one step by perforation extrusion to achieve the required size;

[0054] Step 3: Cut and machine the extruded tube to obtain a blank with the inner and outer diameters of the finished product;

[0055] Step 4: Calculate the length and amount of the blank based on the finished target material, and use the metallization bonding method to prepare the finished high-conductivity copper alloy touch rotary target material. The target material prepared in this way is not limited by size.

[0056] Preferably, in step 2, a uniform staggered feeding method is adopted during the raw material feeding process of vacuum smelting.

[0057] Example 2

[0058] refer to Figure 1 A method for preparing a copper alloy touch target material for a touch device, comprising the following specific steps:

[0059] Step 1, selection and ratio of target material doping elements: according to the final required film performance, select and calculate from Zr, Cr, Zn, and Al, and analyze the type and ratio of target material doping elements;

[0060] Step 2, vacuum melting: put the calculated proportion of single element or alloy raw materials into the vacuum melting furnace;

[0061] Step 3, heating the vacuum melting furnace: according to the different alloy elements and contents, the temperature is set to 1150°C, the vacuum melting furnace is heated to melt the single substance or alloy raw materials in the melting furnace, and the vacuum degree in the vacuum melting furnace is maintained;

[0062] Step 4, ventilation and impurity removal: After all the raw materials are melted, inert gas is introduced into the vacuum melting furnace to help the gas impurities generated after the metal solution is heated to float up and discharge, thereby removing impurities and finally obtaining a high-purity alloy target;

[0063] Step 5: Casting and molding of alloy target: Casting is performed under vacuum to ensure the fluidity of the high-temperature solution, and the alloy ingot is obtained by cooling and shaping;

[0064] Step 6, high-purity alloy target rolling treatment: the smelted alloy ingot is rolled using a hot rolling mill, the heating furnace temperature is set to 800°C, and after the temperature reaches 800°C, the ingot is placed in the heating furnace for 2.3 hours, followed by 8 rolling processes;

[0065] Step 7, annealing treatment of high-purity alloy target: annealing treatment of the leveled high-purity alloy target at 600° C. for 1.2 hours;

[0066] Step 8: Milling of high-purity alloy target: Use milling machine equipment to perform surface milling on the high-purity alloy target, with an average particle size of 100 μm;

[0067] Step 9. Application of high-purity alloy target: Use metallization bonding method to bond it to the backplane of required size, so as to obtain high-conductivity copper alloy touch flat target for high-end touch devices. The size of the target is not limited.

[0068] Preferably, the doping mass of the Zr element is 1.5%; the doping mass of the Cr element is 0.8%, the doping mass of the Zn element is 0.1%, and the doping mass of the Al element is 0.6%.

[0069] Preferably, in step 2, the vacuum melting chamber is evacuated to 1.0 Pa.

[0070] Preferably, in step 3, the casting mold is preheated at the same time to prevent the high-temperature solution from instantly solidifying and shrinking when the mold is cold, resulting in poor molding.

[0071] Preferably, in step 5, during the alloy forming process, the oxygen content is controlled to be ≤160ppm.

[0072] Preferably, in step 6, during the alloy target rolling process, the total deformation of the aluminum-scandium plate is controlled to be above 90%, the thickness is 10 mm, and a leveling machine is used to level the plate to ensure its flatness.

[0073] Preferably, in order to minimize the melting temperature difference during the melting process, the composition and proportion of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram.

[0074] Preferably, in step 9, when the performance of the planar target meets the requirements, a rotating target can be developed to improve its utilization rate. The specific steps are as follows:

[0075] Step 1: Use a vacuum melting furnace for melting and casting, the process is the same as steps 1-5 of the planar target;

[0076] Step 2: Extrude the smelted alloy ingot and form it in one step by perforation extrusion to achieve the required size;

[0077] Step 3: Cut and machine the extruded tube to obtain a blank with the inner and outer diameters of the finished product;

[0078] Step 4: Calculate the length and amount of the blank based on the finished target material, and use the metallization bonding method to prepare the finished high-conductivity copper alloy touch rotary target material. The target material prepared in this way is not limited by size.

[0079] Preferably, in step 2, a uniform staggered feeding method is adopted during the raw material feeding process of vacuum smelting.

[0080] Example 3

[0081] refer to Figure 1 A method for preparing a copper alloy touch target material for a touch device, comprising the following specific steps:

[0082] Step 1, selection and ratio of target material doping elements: according to the final required film performance, select and calculate from Zr, Cr, Zn, and Al, and analyze the type and ratio of target material doping elements;

[0083] Step 2, vacuum melting: put the calculated proportion of single element or alloy raw materials into the vacuum melting furnace;

[0084] Step 3, heating the vacuum melting furnace: according to the different alloy elements and contents, the temperature is set at 1300°C, the vacuum melting furnace is heated to melt the single substance or alloy raw materials in the melting furnace, and the vacuum degree in the vacuum melting furnace is maintained;

[0085] Step 4, ventilation and impurity removal: After all the raw materials are melted, inert gas is introduced into the vacuum melting furnace to help the gas impurities generated after the metal solution is heated to float up and discharge, thereby removing impurities and finally obtaining a high-purity alloy target;

[0086] Step 5: Casting and molding of alloy target: Casting is performed under vacuum to ensure the fluidity of the high-temperature solution, and the alloy ingot is obtained by cooling and shaping;

[0087] Step 6, high-purity alloy target rolling treatment: the smelted alloy ingot is rolled using a hot rolling mill, the heating furnace temperature is set to 900°C, and after the temperature reaches 900°C, the ingot is placed in the heating furnace for 3 hours, followed by 10 rolling processes;

[0088] Step 7, annealing treatment of high-purity alloy target: annealing treatment of the leveled high-purity alloy target at 700° C. for 1.5 hours;

[0089] Step 8: Milling of high-purity alloy target: Use milling machine equipment to perform surface milling on the high-purity alloy target, with an average particle size of 120 μm;

[0090] Step 9. Application of high-purity alloy target: Use metallization bonding method to bond it to the backplane of required size, so as to obtain high-conductivity copper alloy touch flat target for high-end touch devices. The size of the target is not limited.

[0091] Preferably, the doping mass of the Zr element is 2%; the doping mass of the Cr element is 1.1%, the doping mass of the Zn element is 0.3%, and the doping mass of the Al element is 0.7%.

[0092] Preferably, in step 2, the vacuum melting chamber is evacuated to 2.0 Pa.

[0093] Preferably, in step 3, the casting mold is preheated at the same time to prevent the high-temperature solution from instantly solidifying and shrinking when the mold is cold, resulting in poor molding.

[0094] Preferably, in step 5, during the alloy forming process, the oxygen content is controlled to be ≤160ppm.

[0095] Preferably, in step 6, during the alloy target rolling process, the total deformation of the aluminum-scandium plate is controlled to be above 90%, the thickness is 15 mm, and a leveling machine is used to level the plate to ensure its flatness.

[0096] Preferably, in order to minimize the melting temperature difference during the melting process, the composition and proportion of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram.

[0097] Preferably, in step 9, when the performance of the planar target meets the requirements, a rotating target can be developed to improve its utilization rate. The specific steps are as follows:

[0098] Step 1: Use a vacuum melting furnace for melting and casting, the process is the same as steps 1-5 of the planar target;

[0099] Step 2: Extrude the smelted alloy ingot and form it in one step by perforation extrusion to achieve the required size;

[0100] Step 3: Cut and machine the extruded tube to obtain a blank with the inner and outer diameters of the finished product;

[0101] Step 4: Calculate the length and amount of the blank based on the finished target material, and use the metallization bonding method to prepare the finished high-conductivity copper alloy touch rotary target material. The target material prepared in this way is not limited by size.

[0102] Preferably, in step 2, a uniform staggered feeding method is adopted during the raw material feeding process of vacuum smelting.

[0103] Through the above analysis of the current situation and exclusion of dopable elements, one or more of the elements Zr, Cr, Zn, Al, etc. were selected for doping experiments. Elements such as Zr and Cr have good stability. When doped with 1%-2% Zr, the conductivity can reach 95% IACS; when doped with 0.4%-1.1% Cr + 0.03%-0.3% Zr, the conductivity can reach 78%-86% IACS.

[0104]

[0105] Principle and advantages of use:

[0106] The preparation method of the copper alloy touch target material for touch control devices has innovative composition and film stability: the pure copper target material has a high conductivity after coating, but its oxidation resistance is insufficient. In a 120°C environment, the film is easily oxidized. Doping one or more of the elements such as Zr, Cr, Zn, and Al can enhance the oxidation resistance and mechanical strength of the target coating film, and meet the film conductivity of ≥70% IACS; melt uniformity: in order to minimize the melting temperature difference during the smelting process, the composition and ratio of the raw material alloy are calculated through a binary phase diagram or a multi-element phase diagram, thereby avoiding the phenomenon of severe oxidation of individual elements caused by excessive temperature difference; composition uniformity: uniform cross-linking is adopted during the raw material input process. The method of mis-feeding reduces component segregation; the oxygen content also has a certain influence on the performance of the final target material. In the entire process route, the melt casting and cooling are in a vacuum environment, which reduces the oxidation of the material. The introduction of inert gas for sufficient exhaust can also reduce the oxygen content in the finished product, thereby improving the purity of the final product and increasing the uniformity of the composition; fine and uniform grains: the target material prepared by the rolling process can well refine the grains, and after heat treatment, the grains can be made more uniform. The uniform target material performance will result in uniform film layer performance; film layer stability: the film layer after coating with the copper alloy target material doped with the above elements can be baked for 60 minutes in an environment of 170°C and 40% humidity, and the resistance value change rate is ≤10%.

[0107] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a copper alloy touch target material for a touch device, characterized in that: The specific steps include: Step 1, selection and ratio of target material doping elements: according to the final required film performance, select and calculate from Zr, Cr, Zn, and Al, and analyze the type and ratio of target material doping elements, the doping mass of the Zr element is 1%-2%; the doping mass of the Cr element is 0.4%-1.1%, the doping mass of the Zn element is 0.03%-0.3%, and the doping mass of the Al element is 0.5%-0.7%; Step 2, vacuum melting: put the calculated proportion of single element or alloy raw materials into the vacuum melting furnace; Step 3, heating the vacuum melting furnace: according to the different alloy elements and contents, the temperature is set at 1000°C-1300°C, the vacuum melting furnace is heated to melt the single substance or alloy raw materials in the melting furnace, and the vacuum degree in the vacuum melting furnace is maintained; Step 4, ventilation and impurity removal: After all the raw materials are melted, inert gas is introduced into the vacuum melting furnace to help the gas impurities generated after the metal solution is heated to float up and discharge, thereby removing impurities and finally obtaining a high-purity alloy target; Step 5: Casting and molding of alloy target: Casting is performed under vacuum to ensure the fluidity of the high-temperature solution, and the alloy ingot is obtained by cooling and shaping; Step 6, high-purity alloy target rolling treatment: the smelted alloy ingot is rolled using a hot rolling mill, the heating furnace temperature is set to 700°C-900°C, after the temperature is reached, the ingot is placed in the heating furnace for 1.5-3h, and then 5-10 rolling processes are performed; Step 7, annealing treatment of high-purity alloy target: annealing treatment of the leveled high-purity alloy target at 500° C. to 700° C. for 1 to 1.5 hours; Step 8, milling of high-purity alloy target: using milling machine equipment to perform surface milling on the high-purity alloy target, with an average particle size of 80 to 120 μm; Step 9. Application of high-purity alloy target: Use metallization bonding method to bond it to the backplane of required size, so as to obtain high-conductivity copper alloy touch flat target for high-end touch devices. The size of the target is not limited.

2. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In the step 2, the vacuum melting chamber is evacuated to 0.1-2.0 Pa.

3. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In the step 3, the casting mold is preheated at the same time to prevent the high-temperature solution from solidifying and shrinking instantly when the mold is cold, resulting in poor molding.

4. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In the step 5, during the alloy forming process, the oxygen content is controlled to be ≤160ppm.

5. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In the step 6, during the alloy target rolling process, the total deformation of the aluminum-scandium plate is controlled to be above 90%, the thickness is 5-15 mm, and a leveling machine is used to level the plate to ensure its flatness.

6. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In order to minimize the melting temperature difference during the melting process, the composition and proportion of the raw material alloy are calculated through a binary phase diagram or a multivariate phase diagram.

7. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In step 9, when the performance of the planar target meets the requirements, a rotating target can be developed to improve its utilization rate. The specific steps are as follows: Step 1: Use a vacuum melting furnace for melting and casting, and the process is the same as steps 1-5 of the planar target; Step 2: Extrude the melted alloy ingot and use perforation extrusion to form it in one step to achieve the required size; Step 3: Cut and machine the extruded tube to obtain a blank with the inner and outer diameters of the finished product; Step 4: Calculate the length and amount of the blank based on the finished target material, and use the metallization bonding method to prepare the finished high-conductivity copper alloy touch rotary target material. The target material prepared in this way is not limited by size.

8. The method for preparing a copper alloy touch target material for a touch device according to claim 1, characterized in that: In the step 2, during the vacuum smelting, the raw materials are fed in a uniform staggered manner.