A method for preparing antibacterial, anti-creep and strong-adhesion ultra-high molecular weight polyethylene fiber and its product
Product B is formed through the reaction of UIO-66-NH2 and dopamine, and combined with the multi-stage thermal drawing process, the problem of multi-step processing of UHMWPE fiber is solved, the antibacterial, anti-creep and adhesion properties are improved, and the process is simplified. and reduce costs.
Patent Information
- Application Number
- CN202311059058.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-08-21
AI Technical Summary
In the existing technology, improving the antibacterial, creep resistance and adhesion properties of ultra-high molecular weight polyethylene (UHMWPE) fibers requires multi-step processing, resulting in cumbersome processes and increased production costs.
Intermediate product A is obtained by reacting UIO-66-NH2 with ethylene glycol diglycidyl ether, and dopamine is added to form product B. The ultra-high molecular weight polyethylene powder is then spun into jelly fibers and soaked in a specific solution. Processing, including extraction, drying and multi-stage heat drawing, results in fibers with antibacterial, creep resistance and strong adhesion properties.
It has improved the antibacterial, creep resistance and surface adhesion properties of UHMWPE fiber, simplified the process and reduced production costs, while maintaining the excellent mechanical properties of the fiber.
Smart Images

Figure CN117306253B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-performance fiber preparation, and specifically relates to a preparation method of an antibacterial, creep-resistant and strongly-adhesive ultra-high molecular weight polyethylene fiber and a product thereof. Background Art
[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber is one of the three traditional high-performance fibers. It has excellent properties such as high strength and modulus, resistance to ultraviolet radiation, chemical corrosion, and low dielectric constant. It is widely used in military, aviation, aerospace, and sports equipment. However, the polyethylene molecular chain in the fiber has high crystallinity and orientation, lacks branching, is prone to creep under long-term stress, and has a smooth and non-polar surface, which makes it difficult for the coating to adhere firmly and permanently to the fiber surface when the functional coating is applied to the polyethylene fiber. In addition, it also leads to weak interaction with the resin matrix when used as a reinforcing material, and is prone to fiber degumming and matrix resin cracking when subjected to stress, which seriously restricts its application in the field of composite materials.
[0003] In order to improve the creep resistance of UHMWPE fibers, at present, it is mainly achieved by partial crosslinking inside the UHMWPE fibers. Patent application number CN202011219644.1 discloses a high modulus creep-resistant ultra-high molecular weight polyethylene fiber and a preparation method thereof. Ultraviolet sensitizer, crosslinking agent, and silane coupling agent are added to the UHMWPE spinning raw material to achieve mild crosslinking, and finally achieve the purpose of improving creep resistance. In addition, the patent can also effectively control the crosslinking area and crosslinking point density of UHMWPE macromolecules, and the prepared UHMWPE fiber has high modulus, creep resistance, tensile resistance and other properties. Patent application number CN201410142484.3 discloses a preparation method of silane crosslinked modified ultra-high molecular weight polyethylene fiber. The UHMWPE fiber that has not been dried is placed in a modified solution, ultrasonically treated, and then subjected to multi-stage hot stretching to obtain a modified fiber with creep resistance and surface adhesion.
[0004] In order to improve the antibacterial properties of UHMWPE fibers, it is mainly achieved by coating an antibacterial coating on the surface of UHMWPE fibers. The Chinese invention patent with application number CN202210187597.X discloses a medical antibacterial UHMWPE suture and a preparation method thereof. The patent applies a cross-linked network absorbent swellable antibacterial coating composed of polydimethylsiloxane and povidone iodine to the fiber surface to achieve antibacterial properties. The Chinese invention patent with application number CN 202110504950.8 discloses an antibacterial ultra-high molecular weight polyethylene colored fiber and a preparation method thereof. The patent immerses UHMWPE dry freeze-gel fibers into a dispersion containing antibacterial particles and colored particles, so that the antibacterial particles and colored particles are evenly loaded into the UHMWPE dry freeze-gel fibers to achieve the antibacterial properties of the fibers. Improving the adhesion properties of UHMWPE fibers is mainly achieved by coating a coating containing polar groups on the surface of the UHMWPE fibers. The Chinese invention patent with application number CN202111103441.0 discloses a method for preparing ultra-high molecular weight polyethylene fibers by constructing hydrogen bonds with tannic acid and polyaniline. The coating of the above two substances effectively improves the adhesion of the fiber surface.
[0005] It can be seen that currently, the existing treatment methods can improve the creep resistance, antibacterial and surface adhesion properties of fibers, but one treatment method can only achieve a single modification effect. If you want to achieve multiple performance improvements, multi-step coating is required, which greatly increases the economic cost. Summary of the invention
[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0008] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an antibacterial, creep-resistant and strongly adhesive ultra-high molecular weight polyethylene fiber.
[0009] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing antibacterial, creep-resistant and highly adhesive ultra-high molecular weight polyethylene fibers, comprising:
[0010] UIO-66-NH2 is reacted with ethylene glycol diglycidyl ether to obtain intermediate product A;
[0011] Add dopamine to the intermediate product A to obtain product B;
[0012] The ultra-high molecular weight polyethylene powder is mixed with the solvent, stirred and mixed evenly, extruded through a twin-screw extruder, spun through a metering pump and a spinneret in sequence, and cooled in a water bath to obtain frozen collagen filaments;
[0013] After the obtained frozen collagen silk is left to stand at room temperature, it is placed in a mixture C, a mixture D, and a polar solution E in order to obtain surface-modified frozen collagen silk; wherein the mixture C is a mixture of product B and solution F, and solution F is a mixture of one or more of water, alcohol, acetone, methanol, and glycerol; the mixture D is a mixture containing tris(hydroxymethyl)aminomethane hydrochloride Tris, solution F, Cu + or Ag + ions or a mixture of two thereof; the polar solution E is a mixture of one or more of methanol, ethanol, isopropanol, n-butanol, dioxane, and tetrahydrofuran;
[0014] The modified frozen collagen fibers are left to stand at room temperature, and then extracted, dried, and subjected to multi-stage heat drawing to obtain surface-modified ultra-high molecular weight polyethylene fibers.
[0015] As a preferred embodiment of the preparation method of the present invention, the molar mass ratio of UIO-66-NH2 to ethylene glycol diglycidyl ether is 1:1.5 to 1:5, the reaction time for obtaining the intermediate product A is 1 to 24 hours, the reaction temperature is 20 to 60°C, and the pH of the reaction system is 9 to 12.
[0016] As a preferred embodiment of the preparation method of the present invention, the molar mass ratio of UIO-66-NH2 to ethylene glycol diglycidyl ether is 1:1.5 to 1:3.
[0017] As a preferred embodiment of the preparation method of the present invention, the molar mass ratio of the intermediate product A to dopamine is 1:0.5 to 1:3, the reaction time for obtaining the intermediate product B is 1 to 24 hours, the reaction temperature is 20 to 60°C, and the pH of the reaction system is 9 to 12.
[0018] As a preferred embodiment of the preparation method of the present invention, the ultra-high molecular weight polyethylene powder accounts for 4 to 15 wt% of the total mass of the mixed solution, and the solvent in the mixed solution is one or more hydrocarbons, including one or more of decalin, tetralin, kerosene, paraffin oil, and white oil.
[0019] As a preferred embodiment of the preparation method of the present invention, wherein: the mixed solution C, wherein the mass proportion of product B in the mixture is 0.5 to 20 wt%;
[0020] The frozen collagen fibers are immersed in the mixed solution C for 0.1 to 2 hours at a temperature of 10 to 70°C.
[0021] As a preferred embodiment of the preparation method of the present invention, wherein: in the mixed solution D, the mass of Tris accounts for 0.1-2 wt% of the mass of the mixed solution D, the pH is 6-10, and Cu + or Ag + The mass of the ions accounts for 1 to 8 wt% of the mass of the mixed solution D;
[0022] The frozen collagen strands are immersed in the mixed solution D for 0.2 to 3 hours at a temperature of 20 to 60°C.
[0023] As a preferred embodiment of the preparation method of the present invention, the frozen collagen filaments immersed in the mixed solution C and the mixed solution D are immersed in the polar solution E, wherein the immersion time is 2 to 60 minutes and the immersion temperature is 20 to 60°C.
[0024] As a preferred embodiment of the preparation method of the present invention, the modified frozen collagen filaments are allowed to stand at room temperature and then extracted, dried, and subjected to multi-stage hot stretching, wherein the extractant is one or a mixture of xylene, dichloromethane, petroleum ether, and 120# gasoline, the extraction temperature is 20-40°C, the drying temperature is 20-80°C, the stretching hot box in the multi-stage hot stretching process is 3-6 levels, the stretching temperature is 80-148°C, and the hot stretching multiple is 10-40 times.
[0025] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an ultra-high molecular weight polyethylene fiber with antibacterial, creep resistance and strong adhesion, characterized in that the fiber surface contains polar groups and has excellent antibacterial, creep resistance and mechanical properties.
[0026] Beneficial effects of the present invention:
[0027] (1) The traditional preparation of UHMWPE fibers with antibacterial, anti-creep and improved surface adhesion functions often requires multiple steps of treatment to make the fibers have the above functions, which leads to problems such as cumbersome processing technology and increased production costs. The present invention processes the frozen collagen filaments and then extracts and dries them, performs super-heat stretching and other processes to obtain UHMWPE fibers with antibacterial, anti-creep and improved surface adhesion.
[0028] (2) The present invention soaks the novel filler product B in the frozen collagen filaments. The product B contains both a porous organic skeleton structure UIO-66-NH2 and a dopamine structure that improves adhesion. Then, under certain conditions, the product B is polymerized and firmly adhered to the surface of the frozen collagen filaments. In addition, the UIO-66-NH2 structure can not only entangle the UHMWPE molecular chains, but also transfer the antibacterial ion Cu + or Ag + The ions are adsorbed into the interior of UIO-66-NH2 to achieve the sustained release of antibacterial properties. Finally, through subsequent process treatment, functional UHMWPE fibers with antibacterial, anti-creep and improved surface adhesion are finally obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0030] Figure 1 This is a preparation process diagram of the new filler product B in an embodiment of the present invention. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0033] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0034] The UHMWPE powder in the present invention is purchased from Shanghai Lianle Chemical Technology Co., Ltd., and has a viscosity average molecular weight of 7 million.
[0035] The fiber density test standard in the present invention is: FZ / T 01057.7-2007, density gradient method; fiber strength and elongation at break test standard: GB / T 19975-2005; fiber creep resistance test standard: see GB / T19975.10-2005; single filament pull-out force and interface shear strength test refer to GB 2942-2009; viscosity average molecular weight test standard: ASTM D4020-2018.
[0036] Example 1
[0037] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio of 1:1.5) are reacted to obtain intermediate product A, the reaction time of intermediate product A is 4 h, the reaction temperature is 45° C., and the pH of the reaction system is 10;
[0038] Then dopamine is added (the molar mass ratio of intermediate product A to dopamine is 1:0.5) to obtain product B. The process diagram of the preparation is shown in Figure 1 , the reaction time of intermediate product B is 2.5h, the reaction temperature is 40℃, and the pH of the reaction system is 11;
[0039] (2) Mixing the selected UHMWPE powder with the solvent (white oil) (the UHMWPE powder accounts for 6 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments, wherein the spinning solution concentration is 6 wt%, the twin-screw spinning temperature is 220° C., the twin-screw speed is 120 RPM, and the distance between the spinneret and the water bath is 3 cm;
[0040] (3) placing the obtained frozen collagen strands at room temperature and then sequentially placing them into mixed solution C, mixed solution D, and polar solution E to obtain surface-modified UHMWPE frozen collagen strands;
[0041] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 0.5wt%, the immersion time of frozen collagen fibers in the mixed solution C is 0.1 hour, and the immersion temperature is 10°C;
[0042] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag. + ion mixture, the mass of Tris accounts for 0.1wt% of the mass of the mixed solution D, the pH is 6, the immersion time is 0.2 hours, the immersion temperature is 20℃, Ag + The mass of the ions accounts for 1wt% of the mass of the mixed solution D;
[0043] The polar solution E is ethanol, the immersion time in the polar solution E is 2 minutes, and the immersion temperature is 20°C;
[0044] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is dichloromethane, the extraction temperature is 25° C., the drying temperature is 40° C., the multi-stage hot drawing process has three-stage drawing hot boxes, the temperatures of the three-stage drawing hot boxes are 100, 130, and 147° C., respectively, and the hot drawing multiple is 26 times;
[0045] The density of the UHMWPE / modified PE composite fiber is 0.96 g / cm 3 The strength is 36cN / dtex, the elongation at break is 2.7%, the contact angle between the fiber and water is 90°, and the fiber cross section is subjected to EDX test. It is found that the Zr content in the central area of the fiber (the circular area with the center of the circular cross section as the center and 0.9r as the radius) is 0.3wt%, and the Ag content is 0.4wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 0.4wt%, and the Ag content is 0.5wt%. The viscosity-average molecular weight of the composite fiber is 3.67 million.
[0046] The pull-out force of the epoxy resin embedded test single fiber was 8 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 18 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 97%.
[0047] Creep resistance: creep is 2% after being subjected to 1000MPa tensile force for 30 minutes at 70℃;
[0048] Antibacterial performance: The antifungal rate was 99% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 99% when tested according to the FZ / T 73023-2006 standard.
[0049] Example 2
[0050] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio of 1:5) are reacted to obtain intermediate product A, the reaction time of intermediate product A is 2 h, the reaction temperature is 55° C., and the pH of the reaction system is 11;
[0051] Then dopamine was added (the molar mass ratio of intermediate product A to dopamine was 1:3) to react to obtain product B. The reaction time of intermediate product B was 3 h, the reaction temperature was 49° C., and the pH of the reaction system was 10.5;
[0052] (2) Mixing the selected UHMWPE powder with the solvent (decalin) (the UHMWPE powder accounts for 8 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments, wherein the spinning solution concentration is 8 wt%, the twin-screw spinning temperature is 205° C., the twin-screw speed is 110 RPM, and the distance between the spinneret and the water bath is 2.5 cm;
[0053] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0054] Wherein, the mixed solution C is a mixture of product B and acetone, the mass proportion of product B in the mixture is 20wt%, the immersion time of frozen collagen fibers in the mixed solution C is 2 hours, and the immersion temperature is 70°C;
[0055] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), glycerol and Cu + ion mixture, the mass of Tris accounts for 2wt% of the mass of the mixed solution D, the pH is 10, the immersion time is 3 hours, the immersion temperature is 60°C, and the mass of Cu+ ions accounts for 8wt% of the mass of the mixed solution D;
[0056] The polar solution E is dioxane, the immersion time in the polar solution E is 60 minutes, and the immersion temperature is 60°C;
[0057] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is xylene, the extraction temperature is 35° C., the drying temperature is 50° C., the multi-stage hot drawing process has five-stage drawing hot boxes, the temperatures of the five-stage drawing hot boxes are 90, 110, 130, 140, and 148° C., respectively, and the hot drawing multiple is 34 times;
[0058] The density of the UHMWPE / modified PE composite fiber is 0.98 g / cm 3 , strength is 39cN / dtex, elongation at break is 2.5%, contact angle of fiber with water is 90°, EDX test is performed on fiber cross section, and it is found that the Zr content in the central area of the fiber (circular area with the center of the circular cross section as the center and 0.9r as the radius) is 0.2wt%, and the Cu content is 0.1wt%. The Zr content in the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 8wt%, and the Cu content is 5wt%. The viscosity-average molecular weight of the composite fiber is 3.9 million.
[0059] The pull-out force of the epoxy resin embedded test single fiber was 10 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 20 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 98%.
[0060] Creep resistance: creep is 1% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0061] Antibacterial performance: The antifungal rate was 100% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times, the antifungal rate was 100% when tested according to the FZ / T 73023-2006 standard.
[0062] Example 3
[0063] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio of 1:3) are reacted to obtain intermediate product A, the reaction time of intermediate product A is 8 hours, the reaction temperature is 35° C., and the pH of the reaction system is 11;
[0064] Then dopamine was added (the molar mass ratio of intermediate product A to dopamine was 1:2) to react to obtain product B. The reaction time of intermediate product B was 5 h, the reaction temperature was 46° C., and the pH of the reaction system was 10;
[0065] (2) Mixing the selected UHMWPE powder with the solvent (tetralin) (the UHMWPE powder accounts for 7 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments, wherein the spinning solution concentration is 7 wt%, the twin-screw spinning temperature is 215° C., the twin-screw speed is 140 RPM, and the distance between the spinneret and the water bath is 3.5 cm;
[0066] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0067] Wherein, the mixed solution C is a mixture of product B and acetone, the mass proportion of product B in the mixture is 10wt%, the immersion time of frozen collagen fibers in the mixed solution C is 1 hour, and the immersion temperature is 40°C;
[0068] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), methanol and Ag. + ion mixture, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 8, the immersion time is 1.5 hours, the immersion temperature is 40°C, and the mass of Ag+ ions accounts for 4.5wt% of the mass of the mixed solution D;
[0069] The polar solution E is tetrahydrofuran, the immersion time in the polar solution E is 31 minutes, and the immersion temperature is 40°C;
[0070] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is 120# gasoline, the extraction temperature is 30°C, the drying temperature is 50°C, the multi-stage hot drawing process has four-stage drawing hot boxes, the temperatures of the four-stage drawing hot boxes are 100, 120, 140, and 145°C, respectively, and the hot drawing multiple is 32 times;
[0071] The UHMWPE / modified PE composite fiber has a density of 0.97 g / cm3, a strength of 37 cN / dtex, an elongation at break of 2.9%, a contact angle between the fiber and water of 80°, and an EDX test on the fiber cross section. It was found that the Zr content in the central area of the fiber (a circular area with the center of the circular cross section as the center and 0.9r as the radius) was 0.2wt%, and the Ag content was 0.2wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) was 4wt%, and the Ag content was 2.5wt%. The viscosity-average molecular weight of the composite fiber was 3.74 million.
[0072] The pull-out force of the epoxy resin embedded test single fiber was 7 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 16 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 99%.
[0073] Creep resistance: creep is 3% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0074] Antibacterial performance: The antifungal rate was 99% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 100% when tested according to the FZ / T 73023-2006 standard.
[0075] Example 4
[0076] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio of 1:3) were reacted to obtain intermediate product A. The reaction time of intermediate product A was 4.5 h, the reaction temperature was 38° C., and the pH of the reaction system was 10.5;
[0077] Then dopamine was added (the molar mass ratio of intermediate product A to dopamine was 1:1) to react to obtain product B. The reaction time of intermediate product B was 3.5 h, the reaction temperature was 45° C., and the pH of the reaction system was 9.5;
[0078] (2) Mixing the selected UHMWPE powder with the solvent (paraffin oil) (the UHMWPE powder accounts for 5 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments, wherein the spinning solution concentration is 5 wt%, the twin-screw spinning temperature is 200 ° C, the twin-screw speed is 128 RPM, and the distance between the spinneret and the water bath is 2.8 cm;
[0079] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0080] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 2wt%, the immersion time of frozen collagen fibers in the mixed solution C is 0.5 hours, and the immersion temperature is 20°C;
[0081] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), methanol and Cu + ion mixture, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 9, the immersion time is 2 hours, the immersion temperature is 30°C, and the mass of Cu+ ions accounts for 3wt% of the mass of the mixed solution D;
[0082] The polar solution E is isopropanol, the immersion time in the polar solution E is 10 minutes, and the immersion temperature is 30°C;
[0083] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fibers, wherein the extractant is petroleum ether, the extraction temperature is 34° C., the drying temperature is 60° C., the multi-stage hot drawing process has four-stage drawing hot boxes, the temperatures of the four-stage drawing hot boxes are 100, 115, 135, and 145° C., respectively, and the hot drawing multiple is 31 times;
[0084] Among them, the UHMWPE / modified PE composite fiber has a density of 0.97g / cm3, a strength of 36cN / dtex, an elongation at break of 3.0%, a contact angle between the fiber and water of 72°, and an EDX test on the fiber cross section. It was found that the Zr content in the central area of the fiber (a circular area with the center of the circular cross section as the center and 0.9r as the radius) was 0.05wt%, and the Cu content was 0.03wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) was 7wt%, and the Cu content was 4wt%. The viscosity-average molecular weight of the composite fiber was 3.58 million.
[0085] The pull-out force of the epoxy resin embedded test single fiber was 7 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 16 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 96%.
[0086] Creep resistance: creep is 3% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0087] Antibacterial performance: The antifungal rate was 100% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 98% when tested according to the FZ / T 73023-2006 standard.
[0088] Example 5
[0089] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio of 1:2.5) are reacted to obtain intermediate product A, the reaction time of intermediate product A is 10 h, the reaction temperature is 25° C., and the pH of the reaction system is 11;
[0090] Then dopamine was added (the molar mass ratio of intermediate product A to dopamine was 1:1.5) to obtain product B. The reaction time of intermediate product B was 6 h, the reaction temperature was 30° C., and the pH of the reaction system was 10;
[0091] (2) Mixing the selected UHMWPE powder with the solvent (white oil) (the UHMWPE powder accounts for 8 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments, wherein the spinning solution concentration is 8 wt%, the twin-screw spinning temperature is 220° C., the twin-screw speed is 100 RPM, and the distance between the spinneret and the water bath is 3.2 cm;
[0092] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0093] Wherein, the mixed solution C is a mixture of product B and methanol, the mass proportion of product B in the mixture is 6wt%, the immersion time of frozen collagen fibers in the mixed solution C is 1 hour, and the immersion temperature is 30°C;
[0094] The mixed solution D is a mixture of tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag+ ions, the mass of Tris accounts for 0.5wt% of the mass of the mixed solution D, the pH is 8, the immersion time is 1 hour, the immersion temperature is 40°C, and the mass of Ag+ ions accounts for 6wt% of the mass of the mixed solution D;
[0095] The polar solution E is a mixture of ethanol and isopropanol. The immersion time in the polar solution E is 25 minutes and the immersion temperature is 45°C.
[0096] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fibers, wherein the extractant is dichloromethane, the extraction temperature is 32° C., the drying temperature is 45° C., the multi-stage hot drawing process has five-stage drawing hot boxes, the temperatures of the five-stage drawing hot boxes are 90, 110, 125, 135, and 146° C., respectively, and the hot drawing multiple is 37 times;
[0097] Among them, the UHMWPE / modified PE composite fiber has a density of 0.97g / cm3, a strength of 40cN / dtex, an elongation at break of 2.6%, a contact angle between the fiber and water of 78°, and an EDX test on the fiber cross section. It was found that the Zr content in the central area of the fiber (a circular area with the center of the circular cross section as the center and 0.9r as the radius) was 0.3wt%, and the Ag content was 0.3wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) was 5wt%, and the Ag content was 2wt%. The viscosity-average molecular weight of the composite fiber was 3.94 million.
[0098] The pull-out force of the epoxy resin embedded test single fiber was 9 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 19 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 98%.
[0099] Creep resistance: creep is 2% after being subjected to 1000MPa tensile force for 30 minutes at 70℃;
[0100] Antibacterial performance: The antifungal rate was 100% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times, the antifungal rate was 99% when tested according to the FZ / T 73023-2006 standard.
[0101] Comparative Example 1 (unmodified fiber)
[0102] (1) The selected UHMWPE powder is mixed with a solvent (the UHMWPE powder accounts for 4 wt% of the total mass of the mixed solution), mechanically stirred to make the mixture uniform, and then extruded through a twin-screw extruder, spun through a metering pump and a spinneret in sequence, and cooled in a water bath to obtain frozen collagen filaments.
[0103] (2) The obtained modified frozen collagen fibers are left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fibers, wherein the extractant is dichloromethane, the extraction temperature is 35° C., the drying temperature is 50° C., the multi-stage hot drawing process has four-stage drawing hot boxes, the temperatures of the four-stage drawing hot boxes are 100, 115, 135, and 145° C., respectively, and the hot drawing multiple is 28 times;
[0104] (3) The UHMWPE / modified PE composite fiber has a density of 0.96 g / cm3, a strength of 35 cN / dtex, an elongation at break of 3.4%, a contact angle between the fiber and water of 110°, and an EDX test on the fiber cross section. It was found that the zirconium element Zr content in the central area of the fiber (a circular area with the center of the circular cross section as the center and 0.9r as the radius) was 0wt%, the silver (or copper) element Ag (or Cu) content was 0wt%, the Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) was 0wt%, the Ag (or Cu) content was 0wt%, and the viscosity-average molecular weight of the composite fiber was 3.54 million.
[0105] The pull-out force of the single fiber in the epoxy resin embedding test was 2 cN, and the shear strength of the epoxy resin / modified fiber composite interface was 6 MPa;
[0106] After 2 hours of ultrasound, the retention rate of the single-filament pull-out force and the interface shear strength was 80%.
[0107] Creep resistance: creep is 15% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0108] Antibacterial performance: The antifungal rate was 1% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times, the antifungal rate was 3% when tested according to the FZ / T 73023-2006 standard.
[0109] Comparative Example 2 (Mixed Solution C soaking time is too long and the temperature is too low)
[0110] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:1.5) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:1) to react to obtain product B;
[0111] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 5 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0112] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0113] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 10wt%, the immersion time of frozen collagen fibers in the mixed solution C is 4 hours, and the immersion temperature is 0°C;
[0114] The mixed solution D is a mixture of tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag+ ions, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 7, the immersion time is 2 hours, the immersion temperature is 50°C, and the mass of Ag+ ions accounts for 4wt% of the mass of the mixed solution D;
[0115] The polar solution E is methanol, the immersion time in the polar solution E is 60 minutes, and the immersion temperature is 40°C;
[0116] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is xylene, the extraction temperature is 30° C., the drying temperature is 40° C., the multi-stage hot drawing process has three-stage drawing hot boxes, the temperatures of the three-stage drawing hot boxes are 100, 130, and 147° C., respectively, and the hot drawing multiple is 23 times;
[0117] The density of the UHMWPE / modified PE composite fiber is 0.96 g / cm 3 The strength is 23cN / dtex, the elongation at break is 3.2%, the contact angle of the fiber with water is 78°, and the fiber cross section is subjected to EDX test. It is found that the Zr content in the central area of the fiber (the circular area with the center of the circular cross section as the center and 0.9r as the radius) is 3wt%, and the Ag content is 2wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 10wt%, and the Ag content is 8wt%. The viscosity-average molecular weight of the composite fiber is 3.38 million.
[0118] The single-filament pull-out force of the epoxy resin embedding test was 5 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 12 MPa.
[0119] After 2 hours of ultrasound, the retention rate of single-filament pull-out force and interface shear strength was 96%.
[0120] Creep resistance: creep is 3% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0121] Antibacterial performance: The antifungal rate was 99% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 98% when tested according to the FZ / T 73023-2006 standard.
[0122] Comparative Example 3 (Mixed Solution C Immersion Time is Too Short and Temperature is Too High)
[0123] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:1.5) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:1) to react to obtain product B;
[0124] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 5 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0125] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0126] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 10wt%, the immersion time of the frozen collagen silk in the mixed solution C is 0.05 hours (compared with comparative example 2, this parameter is changed), and the immersion temperature is 80°C;
[0127] The mixed solution D is a mixture of tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag+ ions, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 7, the immersion time is 3 hours, the immersion temperature is 40°C, and the mass of Ag+ ions accounts for 5wt% of the mass of the mixed solution D;
[0128] The polar solution E is methanol, the immersion time in the polar solution E is 30 minutes, and the immersion temperature is 10°C;
[0129] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fibers, wherein the extractant is petroleum ether, the extraction temperature is 38° C., the drying temperature is 45° C., the multi-stage hot drawing process has five-stage drawing hot boxes, the temperatures of the five-stage drawing hot boxes are 90, 110, 125, 135, and 146° C., respectively, and the hot drawing multiple is 26 times;
[0130] The density of the UHMWPE / modified PE composite fiber is 0.97 g / cm 3The strength is 26cN / dtex, the elongation at break is 11%, the contact angle between the fiber and water is 100°, and the fiber cross section is subjected to EDX test. It is found that the Zr content in the central area of the fiber (the circular area with the center of the circular cross section as the center and 0.9r as the radius) is 0.2wt%, and the Ag content is 0.3wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 0.1wt%, and the Ag content is 0.2wt%. The viscosity-average molecular weight of the composite fiber is 3.19 million.
[0131] The single-filament pull-out force of the epoxy resin embedding test was 2 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 9 MPa.
[0132] After 2 hours of ultrasound, the retention rate of the single-filament pull-out force and the interface shear strength was 50%.
[0133] Creep resistance: creep is 30% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0134] Antibacterial performance: The antifungal rate was 80% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 50% when tested according to the FZ / T 73023-2006 standard.
[0135] Comparative Example 4 (Mixed Solution D Immersion Time is Too Short and Temperature is Too Low)
[0136] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:3) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:2) to react to obtain product B;
[0137] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 10 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0138] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0139] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 7wt%, the immersion time of frozen collagen fibers in the mixed solution C is 2 hours, and the immersion temperature is 60°C;
[0140] Mixed solution D is a mixture of tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag+ ions, the mass of Tris accounts for 0.8wt% of the mass of mixed solution D, the pH is 9, the immersion time is 0.1 hour, the immersion temperature is 5°C, and the mass of Ag+ ions accounts for 6wt% of the mass of mixed solution D;
[0141] The polar solution E is methanol, the immersion time in the polar solution E is 40 minutes, and the immersion temperature is 50°C;
[0142] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is 120# gasoline, the extraction temperature is 32°C, the drying temperature is 48°C, the drawing hot box in the multi-stage hot drawing process is four-stage, the temperatures of the four-stage drawing hot boxes are 100, 115, 135, and 145°C, respectively, and the hot drawing multiple is 23 times;
[0143] The density of the UHMWPE / modified PE composite fiber is 0.98 g / cm 3 The strength is 24cN / dtex, the elongation at break is 9%, the contact angle between the fiber and water is 95°, and the fiber cross section is subjected to EDX test. It is found that the Zr content in the central area of the fiber (the circular area with the center of the circular cross section as the center and 0.9r as the radius) is 0.3wt%, and the Ag content is 0.4wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 0.5wt%, and the Ag content is 0.7wt%. The viscosity-average molecular weight of the composite fiber is 3.05 million.
[0144] The single-filament pull-out force of the epoxy resin embedding test was 3cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 8MPa.
[0145] After 2 hours of ultrasound, the retention rate of single-filament pull-out force and interface shear strength was 70%.
[0146] Creep resistance: creep is 40% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0147] Antibacterial performance: The antifungal rate was 70% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 65% when tested according to the FZ / T 73023-2006 standard.
[0148] Comparative Example 5 (Mixed Solution D soaking time is too long and the temperature is too high)
[0149] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:3) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:2) to react to obtain product B;
[0150] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 10 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, and then extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0151] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0152] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 7wt%, the immersion time of frozen collagen fibers in the mixed solution C is 2 hours, and the immersion temperature is 60°C;
[0153] The mixed solution D is a mixture of tris(hydroxymethyl)aminomethane hydrochloride (Tris), alcohol and Ag+ ions, the mass of Tris accounts for 0.8wt% of the mass of the mixed solution D, the pH is 9, the immersion time is 4 hours, the immersion temperature is 80°C, and the mass of Ag+ ions accounts for 7wt% of the mass of the mixed solution D;
[0154] The polar solution E is methanol, the immersion time in the polar solution E is 50 minutes, and the immersion temperature is 60°C;
[0155] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is xylene, the extraction temperature is 30° C., the drying temperature is 45° C., the multi-stage hot drawing process has four-stage drawing hot boxes, the temperatures of the four-stage drawing hot boxes are 110, 120, 135, and 147° C., respectively, and the hot drawing multiple is 21 times;
[0156] The density of the UHMWPE / modified PE composite fiber is 0.98 g / cm 3 The strength is 13cN / dtex, the elongation at break is 6%, the contact angle of the fiber with water is 75°, and the fiber cross section is subjected to EDX test. It is found that the Zr content in the central area of the fiber (the circular area with the center of the circular cross section as the center and 0.9r as the radius) is 1wt%, and the Ag content is 1wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) is 3wt%, and the Ag content is 4wt%. The viscosity-average molecular weight of the composite fiber is 2.95 million.
[0157] The single-filament pull-out force of the epoxy resin embedding test was 2 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 15 MPa.
[0158] After 2 hours of ultrasound, the retention rate of single-filament pull-out force and interface shear strength was 96%.
[0159] Creep resistance: creep is 3% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0160] Antibacterial performance: The antifungal rate was 99% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 98% when tested according to the FZ / T 73023-2006 standard.
[0161] Comparative Example 6 (Cu + The mass of the ion in the mixed solution D is too high)
[0162] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:3) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:1) to react to obtain product B;
[0163] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 5 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0164] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0165] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 2wt%, the immersion time of frozen collagen fibers in the mixed solution C is 0.5 hours, and the immersion temperature is 20°C;
[0166] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), methanol and Cu + ion mixture, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 9, the immersion time is 1 hour, the immersion temperature is 40°C, and the mass of Cu+ ions accounts for 20wt% of the mass of the mixed solution D;
[0167] The polar solution E is isopropanol, the immersion time in the polar solution E is 30 minutes, and the immersion temperature is 40°C;
[0168] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fiber, wherein the extractant is dichloromethane, the extraction temperature is 36° C., the drying temperature is 40° C., the multi-stage hot drawing process has three-stage drawing hot boxes, the temperatures of the three-stage drawing hot boxes are 100, 135, and 144° C., respectively, and the hot drawing multiple is 18 times;
[0169] Among them, the UHMWPE / modified PE composite fiber has a density of 0.97g / cm3, a strength of 10cN / dtex, an elongation at break of 1.0%, a contact angle between the fiber and water of 78°, and an EDX test on the fiber cross section. It was found that the Zr content in the central area of the fiber (a circular area with the center of the circular cross section as the center and 0.9r as the radius) was 1wt%, and the Cu content was 1wt%. The Zr content at the edge of the fiber cross section (the annular area between 0.9r and r from the center of the circular cross section) was 10wt%, and the Cu content was 7wt%. The viscosity-average molecular weight of the composite fiber was 3.06 million.
[0170] The pull-out force of the epoxy resin embedded test single fiber is 6 cN, and the interface shear strength of the epoxy resin / modified fiber composite material is 13 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength is 97%.
[0171] Creep resistance: creep is 2% after being subjected to 1000MPa tensile force for 30 minutes at 70℃;
[0172] Antibacterial performance: The antifungal rate was 100% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times with water, the antifungal rate was 98% when tested according to the FZ / T 73023-2006 standard.
[0173] Comparative Example 7 (Cu + The mass of the ion in mixed solution D is too low)
[0174] (1) UIO-66-NH2 and ethylene glycol diglycidyl ether (molar mass ratio is 1:3) are reacted to obtain an intermediate product A, and then dopamine is added (the molar mass ratio of the intermediate product A to dopamine is 1:1) to react to obtain product B;
[0175] (2) Mixing the selected UHMWPE powder with the solvent (the UHMWPE powder accounts for 5 wt% of the total mass of the mixed solution), mechanically stirring to make the mixture uniform, extruding it through a twin-screw extruder, spinning it through a metering pump and a spinneret in sequence, and cooling it in a water bath to obtain frozen collagen filaments;
[0176] (3) The obtained frozen collagen fibers are allowed to stand at room temperature and then placed into mixed solution C, mixed solution D, and polar solution E in sequence to obtain surface-modified UHMWPE frozen collagen fibers;
[0177] Wherein, the mixed solution C is a mixture of product B and water, the mass proportion of product B in the mixture is 2wt%, the immersion time of frozen collagen fibers in the mixed solution C is 0.5 hours, and the immersion temperature is 20°C;
[0178] Mixture D is tris(hydroxymethyl)aminomethane hydrochloride (Tris), methanol and Cu + ion mixture, the mass of Tris accounts for 1wt% of the mass of the mixed solution D, the pH is 9, the immersion time is 1 hour, the immersion temperature is 50°C, and the mass of Cu+ ions accounts for 1wt% of the mass of the mixed solution D;
[0179] The polar solution E is isopropanol, the immersion time in the polar solution E is 10 minutes, and the immersion temperature is 30°C;
[0180] (4) The obtained modified frozen collagen raw silk is left to stand at room temperature, and then extracted, dried, and multi-stage hot drawing is performed to obtain surface-modified UHMWPE fibers, wherein the extractant is petroleum ether, the extraction temperature is 35° C., the drying temperature is 55° C., the multi-stage hot drawing process has four-stage drawing hot boxes, the temperatures of the four-stage drawing hot boxes are 100, 110, 130, and 145° C., respectively, and the hot drawing multiple is 26 times;
[0181] The UHMWPE / modified PE composite fiber has a density of 0.97g / cm3, a strength of 30cN / dtex, an elongation at break of 11%, a contact angle between the fiber and water of 97°, and an EDX test of the fiber cross section. It is found that the Zr content in the fiber center area (a circular area with the center of the circular cross section as the center and 0.9r as the radius) is 0.1wt%, the Cu content is 0.1wt%, the Zr content in the fiber cross section edge (annular area between 0.9r and r from the center of the circular cross section) is 0.3wt%, the Cu content is 0.4wt%, and the composite fiber viscosity average molecular weight is 3.26 million.
[0182] The pull-out force of the epoxy resin embedded test single fiber was 8 cN, and the interface shear strength of the epoxy resin / modified fiber composite material was 17 MPa. After 2 hours of ultrasound, the retention rate of the pull-out force of the single fiber and the interface shear strength was 98%.
[0183] Creep resistance: creep is 7% after being subjected to 1000MPa tension for 30 minutes at 70℃;
[0184] Antibacterial performance: The antifungal rate was 80% when tested by the GB / T 20944.2-2007 absorption method. After washing 50 times, the antifungal rate was 78% when tested according to the FZ / T 73023-2006 standard.
[0185] The traditional preparation of UHMWPE fibers with antibacterial, anti-creep and improved surface adhesion often requires multiple steps of processing to make the fibers have the above functions, which leads to problems such as cumbersome processing and increased production costs. The present invention processes the frozen collagen filaments, and then extracts and dries them, performs super-heat drawing and other processes to obtain UHMWPE fibers with antibacterial, anti-creep and improved surface adhesion.
[0186] The present invention soaks a novel filler product B in frozen collagen filaments. The product B contains both a porous organic skeleton structure UIO-66-NH2 and a dopamine structure for improving adhesion. Then, under certain conditions, the product B is polymerized and firmly adhered to the surface of the frozen collagen filaments. In addition, the UIO-66-NH2 structure can not only entangle the UHMWPE molecular chains, but also adsorb the antibacterial ions Cu+ or Ag+ ions into the interior of the UIO-66-NH2 to achieve a sustained release of the antibacterial properties. Finally, through subsequent process treatment, a functional UHMWPE fiber with antibacterial and creep resistance and improved surface adhesion is finally obtained.
[0187] In the present invention, the molar mass ratio of UIO-66-NH2 to ethylene glycol diglycidyl ether is more important; only when the ratio of UIO-66-NH2 to ethylene glycol diglycidyl ether is within an appropriate range, can the intermediate product A be obtained smoothly. If the content of UIO-66-NH2 is too high, the epoxy groups at both ends of ethylene glycol diglycidyl ether will all react with the amino groups of UIO-66-NH2, and the intermediate product A cannot be obtained; when the content of UIO-66-NH2 is too low, UIO-66-NH2 cannot react with ethylene glycol diglycidyl ether, and the intermediate product A cannot be generated; similarly, the molar mass ratio of the intermediate product A to dopamine will also affect the structure of the product B. When the content of dopamine is too high or too low, it is difficult to obtain the product B;
[0188] The immersion time of the frozen collagen filaments in the mixed solution C will affect the distribution of product B in the frozen collagen filaments. If the immersion time is too long, product B will penetrate into the core of the frozen collagen filaments, hindering the oriented crystallization of the fibers during hot drawing, and ultimately affecting the mechanical properties of UHMWPE. If the immersion time is too short, product B will only be on the surface of the frozen collagen filaments or penetrate less into the frozen collagen filaments, and ultimately fail to achieve the purpose of anti-creep and antibacterial and adhesion enhancement. Similarly, the immersion temperature will also affect the penetration of product B in the frozen collagen filaments. If the temperature is too high, product B will be oxidized and the structure will be destroyed. If the temperature is too low, it is not conducive to the penetration of product B in the frozen collagen filaments.
[0189] Then, the frozen collagen filaments containing product B are polymerized in the mixed solution D. The catechol structure of dopamine can firmly adhere product B to the UHMWPE molecular chain. At the same time, Cu+ or Ag+ ions can enter the porous structure of UIO-66-NH2, achieving stable adsorption of Cu+ or Ag+ ions.
[0190] The immersion time and temperature of the frozen collagen filaments of the product B in the mixed liquid D will also affect the performance of the final product. If the immersion time is too short, the product B cannot be polymerized in the frozen collagen filaments, and it is difficult to improve the adhesion performance of the fiber. If the immersion time is too long, the product B will polymerize too much, causing the UHMWPE molecular chains to stick together, affecting the subsequent thermal stretching, which is not conducive to the oriented crystallization of the fiber and reduces the mechanical properties of the fiber. If the immersion temperature is too high, the oxidation structure of the product B will be destroyed and self-polymerization cannot occur. If the immersion temperature is too low, it is difficult for a polymerization reaction to occur. Similarly, if the mass of Cu+ or Ag+ ions in the mixed liquid D is too high, it will affect the final mechanical properties of the fiber. If the mass is too low, it cannot enter the porous structure of UIO-66-NH2, and it is difficult to achieve antibacterial properties.
[0191] Unexpectedly, the product obtained after adding product B and polymerizing, extracting and hot stretching also has good creep resistance. This is because UIO-66-NH2 in product B is a porous compound, and these pores can not only accommodate Cu + or Ag + The ions play an antibacterial role, and the UHMWPE molecular chains can be entangled in them, which ultimately inhibits the slippage of the PE molecular chains and enhances the creep resistance of the fiber.
[0192] In summary, compared with the prior art, the present invention has the following advantages and positive effects: UHMWPE fiber has antibacterial properties; creep resistance is improved; surface adhesion is improved; and excellent mechanical properties are maintained.
[0193] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing an antibacterial, anti-creep, and highly adhesive ultra-high molecular weight polyethylene fiber, characterized in that: include, UIO-66-NH2 is reacted with ethylene glycol diglycidyl ether to obtain an intermediate product A, wherein the reaction time for obtaining the intermediate product A is 1 to 24 hours, the reaction temperature is 20 to 60°C, and the pH of the reaction system is 9 to 12; Add dopamine to the intermediate product A to obtain product B. The reaction time for obtaining the intermediate product B is 1 to 24 hours, the reaction temperature is 20 to 60° C., and the pH of the reaction system is 9 to 12. The ultra-high molecular weight polyethylene powder is mixed with a solvent to obtain a mixed solution, which is stirred and mixed evenly, and then extruded through a twin-screw extruder, spun through a metering pump and a spinneret in sequence, and cooled in a water bath to obtain frozen collagen filaments; After the obtained frozen collagen silk is allowed to stand at room temperature, it is placed into the mixed solution C, the mixed solution D, and the polar solution E in sequence to obtain the surface-modified frozen collagen silk; Wherein, the mixed solution C is a mixture of product B and solution F, and solution F is a mixture of one or more of water, alcohol, acetone, methanol, and glycerol; the mixed solution D is Cu + and / or Ag + ions, tris(hydroxymethyl)aminomethane hydrochloride) Tris, and solution F; the polar solution E is a mixture of one or more of methanol, ethanol, isopropanol, n-butanol, dioxane, and tetrahydrofuran; The frozen collagen fibers are immersed in the mixed solution C for 0.1 to 2 hours at a temperature of 10 to 70°C. Wherein, in the mixed solution D, the mass of Tris accounts for 0.1-2 wt% of the mass of the mixed solution D, the pH is 6-10, and the Cu + or Ag + The mass of the ions accounts for 1 to 8 wt% of the mass of the mixed solution D; the frozen collagen strands are immersed in the mixed solution D for 0.2 to 3 hours at a temperature of 20 to 60°C; The modified frozen collagen fibers are left to stand at room temperature, and then extracted, dried, and subjected to multi-stage heat drawing to obtain surface-modified ultra-high molecular weight polyethylene fibers.
2. The preparation method according to claim 1, characterized in that: The molar mass ratio of the UIO-66-NH2 to ethylene glycol diglycidyl ether is 1:1.5 to 1:
5.
3. The preparation method according to claim 1 or 2, characterized in that: The molar mass ratio of the UIO-66-NH2 to ethylene glycol diglycidyl ether is 1:1.5 to 1:
3.
4. The preparation method according to claim 1, characterized in that: The molar mass ratio of the intermediate product A to dopamine is 1:0.5 to 1:
3.
5. The preparation method according to any one of claims 1, 2 or 4, characterized in that: The ultra-high molecular weight polyethylene powder accounts for 4-15 wt% of the total mass of the mixed solution, and the solvent in the mixed solution is one or more of decalin, tetralin, kerosene, paraffin oil, and white oil.
6. The preparation method according to claim 5, characterized in that: The mixed solution C, wherein the mass proportion of product B in the mixed solution C is 0.5-20 wt%.
7. The preparation method according to claim 1, characterized in that: The frozen collagen filaments soaked in the mixed solution C and the mixed solution D are soaked in the polar solution E, wherein the soaking time is 2 to 60 minutes and the soaking temperature is 20 to 60°C.
8. The preparation method according to claim 1, characterized in that: The modified frozen collagen filaments are allowed to stand at room temperature and then extracted, dried, and subjected to multi-stage hot stretching, wherein the extractant is one or a mixture of xylene, dichloromethane, petroleum ether, and 120# gasoline, the extraction temperature is 20-40°C, the drying temperature is 20-80°C, the stretching hot box in the multi-stage hot stretching process is 3-6 levels, the stretching temperature is 80-148°C, and the hot stretching multiple is 10-40 times.
9. The antibacterial, creep-resistant and highly adhesive ultra-high molecular weight polyethylene fiber prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The fiber surface contains polar groups.
Citation Information
Patent Citations
A method for preparing silane crosslinked modified ultra-high molecular weight polyethylene fiber
CN103993479B
A high-modulus, creep-resistant ultra-high molecular weight polyethylene fiber and its preparation method
CN112281237B
Antibacterial ultra-high molecular weight polyethylene colored fiber and preparation method thereof
CN113215821A
Preparation method for constructing hydrogen bond modified ultra-high molecular weight polyethylene fiber by using tannic acid and polyaniline
CN113667154A
A medical antibacterial UHMWPE suture and its preparation method
CN114618009B