A sodium ion battery positive electrode material and preparation method thereof

By using doping and coating technology in sodium-ion battery cathode materials, the problems of material structural instability and transition metal dissolution are solved, battery cycle performance and stability are improved, and it is suitable for large-scale production.

CN117334857BActive Publication Date: 2024-10-11GUANG DONG GUANG NA XIN CAI KE JI YOU XIAN GONG SI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311230203.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-22
Publication Date
2024-10-11
Estimated Expiration
2043-09-22

AI Technical Summary

Technical Problem

Existing sodium-rich layered oxide cathode materials suffer from structural instability, transition metal dissolution, and high-voltage lattice oxygen precipitation during long-term cycling, resulting in capacity fading and performance degradation of sodium-ion batteries.

Method used

Through the synergistic effect of doping and coating, the O3 phase layered cathode material main body and Na3Ti3In(PO4)6 coating layer are used to reduce the volume change of the material during charge and discharge, and inhibit the dissolution of transition metals and the precipitation of high-voltage lattice oxygen. , improve material stability and battery cycle performance.

Benefits of technology

It significantly improves the structural stability and battery cycle performance of the cathode material, reduces battery gas production, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117334857B_ABST
    Figure CN117334857B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of sodium ion battery positive electrode materials, and discloses a sodium ion battery positive electrode material and a preparation method thereof. The positive electrode material is composed of a material body and a coating layer. The chemical formula of the material body is Na x Ni a Fe b Mn c O2, the chemical formula of the coating layer is Na3Ti3In(PO4)6; its preparation method is: S1, preparing a mixed solution A of water-soluble nickel salt, iron salt and manganese salt, a complexing agent solution B and a precipitant solution C; S2, mixing solutions A, B and C and conducting a co-precipitation reaction; S3, mixing a hydroxide precursor with a titanium source, an indium source, a phosphorus source and a sodium salt and ball milling to obtain a precursor; S4, sintering the precursor powder and cooling to obtain a sodium ion battery positive electrode material; the present invention improves the stability of the positive electrode material and the high-voltage cycle performance of the battery by synergistically doping and coating the main body of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] Energy storage technology has developed rapidly over the past few decades. Secondary batteries, as the most efficient energy storage technology, are a powerful support for clean energy technologies. Lithium-ion batteries, due to their high energy density and stability, have become the most representative electrochemical energy storage technology and are widely used in commercial mobile electronic devices and electric vehicles. However, limited lithium resources and high production costs have hindered the large-scale application of lithium-ion batteries for electrical energy storage, prompting researchers in this field to explore new energy storage systems. Sodium, which belongs to the same main group as lithium and has similar chemical properties to lithium, has a much higher abundance in the earth's crust (2.64%) than lithium (0.006%). Furthermore, sodium-ion batteries (SIBs), which operate on similar principles to lithium-ion batteries, have attracted increasing attention.

[0003] In sodium-ion batteries, the cathode material is one of the most important components, and the performance of the cathode material directly affects the electrochemical performance of the battery. Among them, sodium-rich layered oxide is a high-capacity cathode material that can significantly improve the energy density of sodium-ion batteries and broaden the application range of sodium-ion batteries. However, existing sodium-rich layered oxide materials still have the following technical problems:

[0004] 1) Although sodium-rich layered oxides can achieve relatively high capacity, they suffer from structural instability caused by multiphase conversion, resulting in rapid capacity decay during long-term cycling.

[0005] 2) Harmful side reactions occur between the particle surface and the electrolyte, accelerating the dissolution of transition metals, leading to obstruction of Na+ transmission channels and performance degradation;

[0006] 3) When charged to above 4.3V, the lattice oxygen on the surface of the material is violently precipitated, resulting in battery cycle capacity decay, voltage decay, and battery flatulence, affecting the normal use of the sodium ion battery. Summary of the Invention

[0007] The present invention aims to provide a sodium-ion battery cathode material and its preparation method. By synergistically doping and coating the material, the material's volume change during charge and discharge is reduced, improving its stability, reducing transition metal dissolution and high-voltage lattice oxygen precipitation, enhancing the high-voltage cycling performance of the cathode material and battery, and reducing battery gassing. This solves the problems described in the background art.

[0008] In order to achieve the above object, the present invention provides the following technical solutions:

[0009] A sodium ion battery positive electrode material, the positive electrode material is composed of a material body and a coating layer; the material body is an O3 phase layered positive electrode material, the chemical formula is Na x Ni a Fe b Mn c O2, wherein a, b, and c correspond to the molar percentages of the elements respectively, and 0.67<x≤1, a+b+c=1, 0.33≤a<1, 0.33≤b<1, 0.33≤c<1, and the elements in the chemical formula satisfy charge balance and stoichiometric conservation; the chemical formula of the coating layer is Na3Ti3In(PO4)6, and the mass of the coating layer is 1 to 10% of the mass of the main body of the material.

[0010] The above-mentioned method for preparing a positive electrode material for a sodium ion battery comprises the following steps:

[0011] S1. Prepare a mixed solution of water-soluble nickel salt, iron salt and manganese salt, recorded as solution A, wherein the total concentration of metal ions in solution A is 0.5-2 mol / L; prepare a complexing agent solution with a concentration of 2-5 mol / L, recorded as solution B; prepare a precipitant solution with a concentration of 2-10 mol / L, recorded as solvent C;

[0012] S2, at a speed of 300 to 800 rpm and a temperature of 50 to 60 ° C, the solution A, solution B and solution C obtained in step S1 are added to the reactor in sequence, the mixture is mixed, the pH of the reaction system is controlled to 9 to 11, and a coprecipitation reaction is carried out; the mixture is allowed to stand for 12 to 20 hours, and the hydroxide precursor Ni is obtained after separation and drying. a Fe b Mn c (OH)2, wherein a+b+c=1, 0.33≤a<1, 0.33≤b<1, 0.33≤c<1;

[0013] S3, mixing the hydroxide precursor obtained in step S2 with a titanium source, an indium source, a phosphorus source, and a sodium salt, and ball-milling the mixture to obtain a positive electrode material precursor;

[0014] S4. The cathode material precursor powder obtained in step S3 is placed in a muffle furnace and sintered under a protective atmosphere. After cooling, the desired sodium ion battery cathode material is obtained.

[0015] Furthermore, in S1, the nickel salt is one or more of nickel sulfate, nickel nitrate and nickel acetate; the iron salt is one or more of ferrous sulfate, ferrous nitrate, ferrous acetate and ferrous chloride; the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese acetate; the complexing agent is one or more of ammonium bicarbonate, ammonium carbonate and ammonia water; and the precipitant is one or both of 2-10 mol / L sodium hydroxide solution and potassium hydroxide solution.

[0016] Further, in S2, the hydroxide precursor Ni a Fe b Mn c The particle size of (OH)2 ranges from 3 to 18 μm.

[0017] Furthermore, in S3, the titanium source is one or more of titanium oxide, titanium chloride, and tetrabutyl titanate; the indium source is one or more of indium oxide, indium chloride, and indium nitrate; the phosphorus source is one or more of ammonium dihydrogen phosphate, ammonium hydrogen phosphate, and phosphoric acid; and the sodium salt is one or more of sodium acetate, sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, and disodium hydrogen phosphate.

[0018] Furthermore, in S3, the molar ratio of nickel, manganese, iron and sodium in the obtained positive electrode material precursor is 1:1.02-1.07.

[0019] Furthermore, in S4, the sintering conditions are as follows: in an oxygen or air atmosphere, first heating to 450-600°C at a heating rate of 1-10°C / min, pre-burning for 3-6 hours, then heating to 750-950°C at a heating rate of 1-10°C / min, and calcining for 10-16 hours.

[0020] The beneficial effects of the technical solution are:

[0021] 1. The sodium ion positive electrode material provided by the present invention can partially replace the transition metal layer by doping with titanium and indium, which can change the binding energy of the oxygen element in the lattice oxygen, thereby inhibiting lattice distortion, improving the structural stability of the material, and reducing the volume change of the material during the charge and discharge process, thereby improving the positive electrode material and battery cycle performance;

[0022] 2. The sodium ion positive electrode material provided by the present invention has a coating layer with good stability in the electrolyte, can be well attached to the surface of the material body, isolates the material body from side reactions with the electrolyte, effectively inhibits the dissolution of transition metals, and improves the structural stability of the layered oxide sodium ion battery positive electrode material;

[0023] 3. The preparation method of the sodium ion positive electrode material provided by the present invention is simple, easy to operate, low-cost, and environmentally friendly. It is suitable for large-scale industrial production and can effectively improve the structural stability of layered oxide sodium ion battery positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the SEM of the hydroxide precursor prepared in Example 1 of the present invention;

[0025] Figure 2 This is the SEM of the sodium ion battery positive electrode material prepared in Example 1 of the present invention;

[0026] Figure 3 This is the SEM of the sodium ion battery positive electrode material prepared in Comparative Example 1 of the present invention;

[0027] Figure 4 This is the SEM of the sodium ion battery positive electrode material prepared in Comparative Example 2 of the present invention;

[0028] Figure 5 This is the SEM of the sodium ion battery positive electrode material prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments:

[0030] Example 1

[0031] Nickel sulfate, ferrous sulfate, and manganese sulfate were prepared into a solution A with a metal ion concentration of 2 mol / L according to the molar ratio of Ni, Fe, and Mn of 4:2:4. A 25% ammonia solution B and a 3 mol / L sodium hydroxide solution C were added at a speed of 600 rpm and 50 ° C. Solutions A, B, and C were added to the reactor respectively. The pH of the reaction system was controlled to 10, and a coprecipitation reaction was carried out. After washing, filtration, and drying, the hydroxide precursor Ni was obtained. 0.4 Fe 0.2 Mn 0.4 (OH)2, the SEM of the sodium hydroxide precursor is as follows Figure 1 As shown;

[0032] The dried sodium hydroxide precursor, sodium carbonate, titanium oxide, indium nitrate and diammonium dihydrogen phosphate mixture was ball-milled, and the transition metal and sodium were mixed in a molar ratio of 1:1.03. After the mixture was evenly mixed, it was placed in a muffle furnace for sintering, heated to 450°C at a heating rate of 2°C / min and kept warm for 5 hours, and then heated to 800°C at a heating rate of 2°C / min and kept warm for 12 hours. The calcination atmosphere was air to obtain a sodium ion battery positive electrode material. The SEM of the sodium ion positive electrode material is as follows Figure 2 shown.

[0033] Example 2

[0034] Nickel sulfate, ferrous sulfate, and manganese sulfate were prepared into a solution A with a metal ion concentration of 2.5 mol / L according to the molar ratio of Ni, Fe, and Mn of 4:2:4. A 25% ammonia solution B and a 4 mol / L sodium hydroxide solution C were added at a speed of 650 rpm and 50 ° C. Solutions A, B, and C were added to the reactor respectively. The pH of the reaction system was controlled to 10.5, and a coprecipitation reaction was carried out. After washing, filtration, and drying, the hydroxide precursor Ni was obtained. 0.4 Fe 0.2 Mn 0.4 (OH)2;

[0035] The dried sodium hydroxide precursor, sodium carbonate, titanium oxide, indium oxide and phosphoric acid mixture were ball-milled, and the transition metal and sodium were mixed in a molar ratio of 1:1.05. After mixing, they were placed in a muffle furnace for sintering, heated to 480°C at a heating rate of 4°C / min and kept warm for 4 hours, and then heated to 850°C at a heating rate of 4°C / min and kept warm for 10 hours. The calcination atmosphere was oxygen to obtain a sodium ion battery positive electrode material.

[0036] Example 3

[0037] Nickel sulfate, ferrous sulfate, and manganese sulfate were prepared into a solution A with a metal ion concentration of 2 mol / L according to the molar ratio of Ni, Fe, and Mn of 4:2:4. A 25% ammonia solution B and a 3 mol / L sodium hydroxide solution C were added at a speed of 750 rpm and 60 ° C. Solutions A, B, and C were added to the reactor respectively. The pH of the reaction system was controlled to 11.5, and a coprecipitation reaction was carried out. After washing, filtration, and drying, the hydroxide precursor Ni was obtained. 0.4 Fe 0.2 Mn 0.4 (OH)2;

[0038] The dried sodium hydroxide precursor, sodium carbonate, titanium oxide, indium sulfate and ammonium hydrogen phosphate mixture were ball-milled, and the transition metal and sodium were mixed in a molar ratio of 1:1.03. After mixing, they were placed in a muffle furnace for sintering, heated to 550°C at a heating rate of 5°C / min and kept warm for 6 hours, and then heated to 800°C at a heating rate of 5°C / min and kept warm for 16 hours. The calcination atmosphere was air to obtain a sodium ion battery positive electrode material.

[0039] Comparative Example 1:

[0040] The synthesis method is similar to that of Example 1, except that the pH of the reaction system is controlled to be 11. The SEM of the prepared sodium ion battery cathode material is as follows: Figure 3 shown.

[0041] Comparative Example 2:

[0042] The synthesis method is similar to that of Example 1, except that sodium hydroxide is added during the mixing process. The SEM of the prepared sodium ion battery positive electrode material is as follows: Figure 4 shown.

[0043] Comparative Example 3:

[0044] The synthesis method is similar to that of Example 1, except that a solution A with a metal ion concentration of 2 mol / L and a molar ratio of Ni, Fe, and Mn of 1:1:1 is used for coprecipitation reaction to prepare a sodium ion battery positive electrode material. Figure 5 shown.

[0045] The precursors and cathode materials prepared in Comparative Examples 1, 2, 3 and Example 1 were observed by SEM:

[0046] from Figure 1 It can be seen that the pores inside the sodium hydroxide precursor prepared by the method provided by the present invention are evenly distributed;

[0047] from Figures 2 to 5 It can be seen that the residual sodium on the surface of the positive electrode material prepared by the method provided by the present invention is significantly reduced.

[0048] The positive electrode materials prepared in the comparative example and Example 1 above, along with SP and KS-6 as conductive agents and PVDF as a binder, were mixed in a mass ratio of 85:10:5 and placed in a high-speed blender mold. After adding an appropriate amount of N-methylpyrrolidone, the mixture was stirred at 1000 rpm for 15 minutes to obtain a slurry with appropriate viscosity. This slurry was then coated onto aluminum foil using a pre-coated slurry and dried in a 120°C vacuum oven for 24 hours. The dried electrode sheets were rolled to the appropriate thickness, cut into 12mm diameter pieces, and assembled into button cells in a vacuum glove box. A sodium metal sheet was used as the counter electrode in the 2032-type button cells. Charge and discharge tests were conducted using a Blue Power CT2001A electrochemical tester with a voltage range of 2-4.3V, a current density of 1C, and 100 cycles. The experimental results are shown in Table 1.

[0049] Table 1 Electrochemical properties of the positive electrode materials corresponding to the examples and comparative examples

[0050] Serial number <![CDATA[Initial specific capacity (mAh g -1 )]]> Capacity retention after 100 cycles (%) Example 1 130.7 81.2 Comparative Example 1 129.3 65.4 Comparative Example 2 121.3 75.4 Comparative Example 3 109.2 73.0

[0051] The above is only an embodiment of the present invention, and common knowledge such as the specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the description can be used to interpret the content of the claims.

Claims

1. A method for preparing a positive electrode material for a sodium ion battery, wherein the positive electrode material is composed of a material body and a coating layer; the material body is an O3 phase layered positive electrode material, and the chemical formula is Na x Ni a Fe b Mn c O2, wherein a, b, c correspond to the molar percentage of the element respectively, and 0.67<x≤1, a+b+c=1, 0.33≤a<1, 0.33≤b<1, 0.33≤c<1, and the elements in the chemical formula satisfy the charge balance and stoichiometric conservation; the chemical formula of the coating layer is Na3Ti3In(PO4)6, and the mass of the coating layer is 1-10% of the mass of the main body of the material; characterized in that, The method for preparing the positive electrode material comprises the following steps: S1. Prepare a mixed solution of water-soluble nickel salt, iron salt and manganese salt, recorded as solution A, the total concentration of metal ions in solution A is 0.5-2 mol / L; prepare a complexing agent solution with a concentration of 2-5 mol / L, recorded as solution B; prepare a precipitant solution with a concentration of 2-10 mol / L, recorded as solvent C; wherein the molar ratio of Ni, Fe and Mn in the nickel salt, iron salt and manganese salt is 4:2:4; the precipitant solution is a 3 mol / L sodium hydroxide solution; S2, at a speed of 300 to 800 rpm and a temperature of 50 to 60° C., adding solution A, solution B and solution C obtained in step S1 to the reactor in sequence, mixing them, controlling the pH of the reaction system to 10, and performing a coprecipitation reaction; standing and aging for 12 to 20 hours, separating and drying to obtain a hydroxide precursor Ni a Fe b Mn c (OH)2, wherein a+b+c=1, 0.33≤a<1, 0.33≤b<1, 0.33≤c<1; S3, mixing the hydroxide precursor obtained in step S2 with a titanium source, an indium source, a phosphorus source and a sodium salt, and ball-milling the mixture to obtain a positive electrode material precursor; S4. Place the cathode material precursor powder obtained in step S3 in a muffle furnace and sinter it in an oxygen or air atmosphere to obtain the desired sodium ion battery cathode material after cooling.

2. The method for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: In S1, the nickel salt is one or more of nickel sulfate, nickel nitrate and nickel acetate; the iron salt is one or more of ferrous sulfate, ferrous nitrate, ferrous acetate and ferrous chloride; the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese acetate; the complexing agent is one or more of ammonium bicarbonate, ammonium carbonate and ammonia water.

3. The method for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: In S2, the hydroxide precursor Ni is separated and dried. a Fe b Mn c The particle size range of (OH)2 is 3 to 18 μm.

4. The method for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: In S3, the titanium source is one or more of titanium oxide, titanium chloride, and tetrabutyl titanate; the indium source is one or more of indium oxide, indium chloride, and indium nitrate; the phosphorus source is one or more of diammonium phosphate, ammonium hydrogen phosphate, and phosphoric acid; and the sodium salt is one or more of sodium acetate, sodium carbonate, sodium bicarbonate, sodium dihydrogen phosphate, and disodium hydrogen phosphate.

5. The method for preparing a sodium ion battery positive electrode material according to claim 1, characterized in that: In S3, the molar ratio of nickel, manganese, iron and sodium in the obtained positive electrode material precursor is 1:1.02-1.

07.

6. The method for preparing a sodium ion battery positive electrode material according to claim 1, characterized in that: In S4, the sintering conditions are: firstly increase the temperature to 450-600°C at a heating rate of 1-10°C / min, pre-sinter for 3-6h, then increase the temperature to 750-950°C at a heating rate of 1-10°C / min, and calcine for 10-16h.