Highly transparent and corrosion-resistant photovoltaic encapsulation film and preparation method thereof
By using porous silicon nanocomposite oxide acid antacid and grafted EVA resin in the photovoltaic encapsulation adhesive film, the problem of poor water resistance of the adhesive film is solved, the acid resistance performance is improved, the life of the photovoltaic module is extended, and the Long-term stable operation.
Patent Information
- Application Number
- CN202311505091.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-11-13
AI Technical Summary
Existing photovoltaic encapsulation adhesive films have poor water-blocking properties during long-term aging, leading to corrosion of cells. Moreover, a single metal oxide anti-acid additive cannot have both water-blocking and acid-resistant properties, and cannot prevent corrosion for a long time.
Using porous silicon nanocomposite oxide as an antacid, the porous silicon nanocomposite oxide is synthesized by combining ethyl orthosilicate and oxide precursors, and mixed with superhydrophobic additives to form a superhydrophobic modified porous silicon nanocomposite oxide. Chemical antacid, combined with grafted EVA resin, to improve the light transmittance and acid resistance of the film.
It effectively reduces the water vapor transmission rate of the adhesive film, delays the branched chain hydrolysis rate of EVA resin, improves the acetic acid adsorption and capture ability, significantly improves the anti-aging corrosion performance of photovoltaic modules, and achieves long-term stable operation of the modules.
Smart Images

Figure CN117343657B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of packaging adhesive films, and in particular relates to a high-transmittance and corrosion-resistant photovoltaic packaging adhesive film and a preparation method thereof. Background Art
[0002] In recent years, with the gradual deepening of the dual-carbon policy and the continuous advancement of energy system reform, the photovoltaic industry has developed rapidly. EVA film is the core material of photovoltaic modules, including EVA film, POE film, etc. Although the cost of film only accounts for about 4% of the module cost, it is a key factor in determining the quality and life of photovoltaic modules. In particular, EVA film and multi-layer co-extruded EPE film have always been the mainstream products in the film field, and are widely used in the packaging of PERC and Topcon batteries. However, EVA resin has the inherent defect of VA side chain hydrolysis during long-term aging, which causes the corrosion and shedding of the grid lines on the surface of the battery cell, thereby causing a significant drop in power.
[0003] In order to solve the corrosion problem of battery sheets, the common method is to introduce alkaline oxides to neutralize the free acetic acid produced by EVA aging and hydrolysis. However, there are three problems that have not been solved yet:
[0004] 1. The acid resistance of the film is improved by directly adding nano metal oxides or silane-modified nano metal oxides. Since the refractive index of conventional metal hydroxides and metal oxides is around 1.7, which is significantly different from the refractive index of conventional EVA resin (1.5), and since nano materials have high surface energy and are very easy to agglomerate, a high addition amount will result in low light transmittance and high haze of the film, thus limiting the amount of nano oxide added.
[0005] 2. The existing technology only considers adding metal oxide anti-acid additives to the film for acetic acid adsorption, without considering the improvement of the water barrier properties of the film itself. The adsorption capacity of the metal oxide anti-acid additives itself is limited. During the long-term aging process, water vapor continues to penetrate, which will cause the metal oxide anti-acid additives to fail, and then cause corrosion of the components.
[0006] 3. The addition of a single metal oxide or hydroxide will gradually become ineffective due to its limited adsorption and neutralization capabilities and the small amount added. With the continuous infiltration of water vapor during the long-term aging process, it cannot play a long-term anti-corrosion role.
[0007] Therefore, in order to effectively solve the problem of cell corrosion, it is necessary to consider both water blocking and acid resistance at the same time. Currently, there is no photovoltaic encapsulation film that can take both into account at the same time. Summary of the invention
[0008] The present invention provides a high-transmittance corrosion-resistant photovoltaic encapsulation adhesive film and a preparation method thereof, so as to solve the problem that the existing corrosion-resistant photovoltaic encapsulation adhesive film has poor water-blocking performance.
[0009] In order to solve the above technical problems, the present invention provides a method for preparing a high-transmittance and corrosion-resistant photovoltaic encapsulation film, comprising the following steps: step S1, preparing porous silicon nanocomposite oxide by using tetraethyl orthosilicate and oxide precursor / porous oxide powder; step S2, dissolving a superhydrophobic auxiliary agent in a mixed solution of ethanol and toluene, and mixing and stirring the mixture with the porous silicon nanocomposite oxide to obtain a superhydrophobic modified porous silicon nanocomposite oxide antacid; step S3, blending and granulating EVA resin, peroxide, and silane coupling agent to obtain a grafted EVA resin; step S4, blending the superhydrophobic modified porous silicon nanocomposite oxide antacid with the grafted EVA resin and EVA base material, adding an initiator, a co-crosslinking agent, a light stabilizer, an antioxidant, and a silane coupling agent, and then casting, embossing, cooling, and winding the mixture in a screw extruder to obtain a high-transmittance and corrosion-resistant photovoltaic encapsulation film.
[0010] On the other hand, the present invention also provides a high-transmittance and corrosion-resistant photovoltaic encapsulation film obtained by the preparation method as described above, wherein the mass percentage of the super-hydrophobic modified porous silicon nano-composite oxide antacid of the high-transmittance and corrosion-resistant photovoltaic encapsulation film is 0.2-1%, the transmittance is greater than 92%, and the acid value after aging is less than 50ppm.
[0011] The beneficial effect of the present invention is that the high-transmittance and corrosion-resistant photovoltaic encapsulation film and the preparation method thereof effectively reduce the water vapor permeability of the film by modifying the resin and the anti-acid additive, delay the side chain hydrolysis rate of the EVA resin, and improve the acetic acid adsorption and capture capacity, while using the porous structure of the super-hydrophobic modified porous silicon nano-composite oxide anti-acid agent to solve the problem of decreased light transmittance and increased haze of the film after the addition of nano-oxides, effectively overcome the anti-aging and corrosion problems of photovoltaic modules, and achieve long-term stable operation of the modules.
[0012] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practicing the present invention.
[0013] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 is a SEM image of the porous silicon nanocomposite oxide of the present invention;
[0016] Figure 2 It is the infrared spectrum of the super hydrophobic modified porous silicon nanocomposite oxide antacid of the present invention. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] The invention provides a method for preparing a high-transmittance and corrosion-resistant photovoltaic encapsulation adhesive film, comprising the following steps: step S1, preparing porous silicon nanocomposite oxide by tetraethyl orthosilicate (TEOS) and oxide precursor / porous oxide powder; step S2, dissolving a super-hydrophobic auxiliary agent in a mixed solution of ethanol and toluene, mixing and stirring with the porous silicon nanocomposite oxide, and obtaining a super-hydrophobic modified porous silicon nanocomposite oxide antacid; step S3, blending and granulating EVA resin, peroxide and silane coupling agent, and obtaining a grafted EVA resin; step S4, blending the super-hydrophobic modified porous silicon nanocomposite oxide antacid, the grafted EVA resin and an EVA base material, adding an initiator, a co-crosslinking agent, a light stabilizer, an antioxidant and a silane coupling agent, and then performing casting, embossing, cooling and winding in a screw extruder to obtain the high-transmittance and corrosion-resistant photovoltaic encapsulation adhesive film.
[0019] In this embodiment, specifically, the porous silicon nanocomposite oxide is referred to as an antacid; the superhydrophobic modified porous silicon nanocomposite oxide antacid is referred to as an S-antacid.
[0020] In this embodiment, specifically, step S1 includes: placing tetraethyl orthosilicate and oxide precursor / porous oxide powder in a three-necked flask, adding appropriate amount of ethanol, mixing, stirring and heating to 50-70°C to dissolve for 1 hour, then adding TMB pore expander and surfactant, mixing evenly and adding dropwise a mixture of ammonia water and deionized water in a ratio of 1:1, adjusting the pH to 7-8, and continuing to react at 50-70°C for 2-3 hours. After the reaction, transferring the reaction solution to a high-pressure reactor and crystallizing at 120°C for 12 hours, filtering, washing and drying the crystallized product, and then placing it in a muffle furnace at 400-600°C in an air atmosphere for calcining for 4 hours to prepare a porous silicon nanocomposite oxide.
[0021] In this embodiment, specifically, the porous silicon nanocomposite oxide is in the shape of nanospheres with a particle size of 30 to 100 nm; and there are stacked channels between the porous silicon nanocomposite oxides, which can more efficiently adsorb free acetic acid generated by EVA.
[0022] In this embodiment, specifically, a gel method is used to control the co-hydrolysis of silicate and alkaline metal oxide or its precursor, and a layer of inorganic nano silicon oxide shell is successfully coated on the surface of the nano oxide. Since the refractive index of silicon oxide (1.45-1.47) is close to that of EVA resin (1.5), it has better compatibility in the resin and has no obvious effect on the light transmittance of the film, which can greatly increase the amount of anti-acid additive added. At the same time, inorganic silicon oxide is a porous nano material with rich pore structure on the surface and large specific surface area. It can complement each other with nano alkaline oxide, and can enhance the ability of alkaline oxide to adsorb free acetic acid while improving the light transmittance of the film and reducing the haze of the film.
[0023] In this embodiment, specifically, the oxide precursor / porous oxide powder includes at least one of magnesium acetate, magnesium sulfate, magnesium oxide, aluminum oxide, zinc oxide, zinc acetate, aluminum hydroxide, zinc hydroxide, hydrotalcite, zeolite, and molecular sieve.
[0024] In this embodiment, specifically, the porous silicon nanocomposite oxide comprises: SiMgO X 、SiAlO X 、SiZnO X 、SiCaO X Any one or more combinations of .
[0025] In this embodiment, specifically, step S2 includes: dissolving the super-hydrophobic additive in a mixed solution of ethanol and toluene, mixing and stirring with the porous silicon nano-composite oxide, cooling and refluxing at 80° C. for 6 to 8 hours, and filtering, washing, and drying to obtain a super-hydrophobic modified porous silicon nano-composite oxide antacid.
[0026] In this embodiment, specifically, a super-hydrophobic material is used to perform hydrophobic modification on the surface of the porous silicon nano-composite oxide. The modified anti-acid additive has better compatibility with the matrix EVA resin. Due to the hydrophobic functional groups on its surface, it can effectively block water vapor, further reduce the water vapor permeability of the film, thereby reducing the hydrolysis of the side chains and reducing the aging corrosion of the film to the battery.
[0027] In the present embodiment, specifically, the super hydrophobic additive includes: n-octyl triethoxysilane, n-octyl trimethoxysilane, dimethyl silicone oil, stearic acid, stearic acid amide, glycidyl methacrylate, γ-methacryloxypropyl trimethoxysilane, γ-glycidyl ether oxygen propyl trimethoxysilane, tridecafluorooctyl trimethoxysilane, tridecafluorooctyl triethoxysilane, heptadecafluorodecyl trimethoxysilane, hexamethyldisilazane, tetramethyldivinyldisilazane, tetramethyltetravinylcyclotetrasiloxane, diethylaminomethyltriethoxysilane, any one or more of the following.
[0028] In this embodiment, specifically, the VA content of the grafted EVA resin is 12-34wt%.
[0029] In this embodiment, specifically, the peroxide is composed of one or more of tert-butyl peroxy isopropyl carbonate, 2,5-dimethyl 2,5-bis(tert-butyl peroxy) hexane, 1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, tert-butyl peroxy carbonate-2-ethylhexyl ester, 2,5-dimethyl 2,5-bis(tert-butyl peroxide) hexane, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, 2,2-bis(tert-butyl peroxy) butane, tert-amyl peroxy carbonate, and tert-butyl peroxy 3,3,5-trimethylhexanoate, mixed in any proportion.
[0030] In this embodiment, specifically, the initiator is composed of one or more of tert-butyl peroxy isopropyl carbonate, 2,5-dimethyl 2,5-bis(tert-butyl peroxy)hexane, 1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, tert-butyl peroxy carbonate-2-ethylhexyl ester, 2,5-dimethyl 2,5-bis(tert-butyl peroxide)hexane, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, 2,2-bis(tert-butyl peroxy)butane, tert-amyl peroxy carbonate, and tert-butyl peroxy 3,3,5-trimethylhexanoate, mixed in any proportion.
[0031] In this embodiment, specifically, the auxiliary cross-linking agent includes one or more of monofunctional acrylate, difunctional acrylate, trifunctional acrylate and multifunctional acrylate, selected from pentaerythritol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane triacrylate. Trimethacrylate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (400) diacrylate, polyethylene glycol (600) diacrylate, polyethylene glycol (200) dimethacrylate, polyethylene glycol (400) dimethacrylate, polyethylene glycol (600) dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, neopentyl glycol diacrylate.
[0032] In this embodiment, specifically, the light stabilizer is a hindered amine light stabilizer, which is specifically selected from one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, mono(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, and poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, and mixed in any proportion.
[0033] In this embodiment, specifically, the antioxidant includes any one of 2,6-di-tert-butyl-p-methylphenol, styrenated phenol, and 2,6-di-tert-butyl-4-n-butylphenol, or a mixture of more than one of them.
[0034] In this embodiment, specifically, the silane coupling agent includes but is not limited to vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(β-methoxyethoxy)silane, methacryloxypropyl trimethoxysilane, aminopropyl trimethoxysilane, aminopropyl triethoxysilane, aminopropyl triisopropoxysilane, preferably vinyl trimethoxysilane or vinyl triethoxysilane.
[0035] In this embodiment, specifically, the EVA resin is modified by silane grafting through a resin grafting process, and the grafted resin surface has more abundant branches, which can delay the hydrolysis of the silane coupling agent and improve the crosslinking density of the film and the peeling strength after aging.
[0036] On the other hand, the present invention also provides a high-transmittance and corrosion-resistant photovoltaic encapsulation film obtained by the preparation method as described above, wherein the mass percentage of the super-hydrophobic modified porous silicon nano-composite oxide antacid of the high-transmittance and corrosion-resistant photovoltaic encapsulation film is 0.2-1%, the transmittance is greater than 92%, and the acid value after aging is less than 50ppm.
[0037] In this embodiment, specifically, the water vapor transmission rate of the high-transmittance and corrosion-resistant photovoltaic encapsulation film is ≤18.5 g / day under the conditions of 38° C. and 90% RH.
[0038] Example 1
[0039] Step S1: 5 parts of tetraethyl orthosilicate and 20 parts of magnesium acetate are placed in a three-necked flask, 50 parts of ethanol are added, the mixture is stirred and the temperature is raised to 50-70° C. to dissolve for 1 hour, 10 parts of TMB pore expander and 15 parts of surfactant are added, the mixture of ammonia water and deionized water in a ratio of 1:1 is added dropwise after mixing evenly, the pH is adjusted to 7.5, and the reaction is continued at 55° C. for 2 hours. After the reaction is completed, the reaction solution is transferred to a high-pressure reactor and crystallized at 120° C. for 12 hours. After the crystallization product is filtered, washed and dried, it is placed in a muffle furnace and calcined in an air atmosphere at 600° C. for 4 hours to prepare a porous silicon nanocomposite oxide.
[0040] Step S2: dissolving 20 parts of super-hydrophobic additive in a mixed solution of ethanol and toluene, mixing and stirring with 80 parts of porous silicon nanocomposite oxide, cooling and refluxing at 80° C. for 6 hours, filtering, washing and drying to obtain a super-hydrophobic modified porous silicon nanocomposite oxide antacid.
[0041] Step S3: 95 parts of EVA resin, 1 part of tert-butyl peroxyisopropyl carbonate, and 4 parts of vinyltriethoxysilane are blended and granulated at 160-220° C. to obtain a grafted EVA resin;
[0042] Step S4, blending 10 parts of super-hydrophobic modified porous silicon nanocomposite oxide antacid, 10 parts of grafted EVA resin and 80 parts of EVA base material, adding 0.05 parts of tert-butyl peroxy isopropyl carbonate, 0.06 parts of pentaerythritol triacrylate, 0.01 parts of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, 0.02 parts of 2,6-di-tert-butyl-p-methylphenol and 0.03 parts of vinyl triethoxysilane, and then casting, embossing, cooling and winding in a screw extruder to obtain a high-transmittance and corrosion-resistant photovoltaic encapsulation film.
[0043] like Figure 1 As shown, the calcined antacid (porous silicon nanocomposite oxide) is in the shape of nanospheres, and there are obvious stacking channels between the particles.
[0044] like Figure 2 As shown, the modified S-antacid (superhydrophobic modified porous silicon nanocomposite oxide antacid) has a wavelength of 2850 cm -1 and 2872cm -1 Obvious characteristic peaks belonging to the stearic acid hydrophobic agent appeared, proving that the hydrophobic agent was successfully coated on the surface of the antacid.
[0045] Some components in Example 1 were adjusted to obtain a high-transmittance and corrosion-resistant photovoltaic encapsulation film. The test results are as follows:
[0046]
[0047]
[0048] Test method:
[0049] Light transmittance:
[0050] Take a piece of TPO film with a size of 30mm×30mm and two pieces of quartz glass with a size of 30mm×30mm (no embossing is required, and the transmittance is not less than 91.5%), put them into a vacuum press after overlapping the quartz glass / TPO film / quartz glass, and cross-link and cure them according to the product curing temperature and time (agreed by the supply and demand parties). After curing, take them out and put them into a dryer to cool to room temperature. The upper and lower surfaces of the cured sample should be flat and free of bubbles. Each group of samples should be no less than 3.
[0051] The samples were tested according to GB / T 2410-2008 Clause 7.2 Method B: Spectrophotometer method. The wavelength range of the spectrophotometer was set to 280nm~1100nm. At least 3 samples were tested in each group, and the results were averaged.
[0052] Water vapor transmission rate:
[0053] Take a piece of 50mm×50mm TPO film, a piece of glass, two pieces of non-adhesive films and a backboard, and stack them in the order of glass / non-adhesive film / TPO film / non-adhesive film / backboard, put them into a vacuum press, and cure them according to the product curing temperature and time (agreed by the supply and demand parties). After curing, put them into a dryer and cool them to room temperature. The surface of the cured sample should be flat and free of bubbles. Cut the cured polyolefin film into samples as required to prepare 3 samples.
[0054] The thickness of the sample was measured with a thickness gauge, and three points were measured at different locations. The average value was taken as the thickness value of the sample. According to the provisions of GB / T 26253-2010, the water vapor transmission rate of the sample was measured at a temperature of (23±0.5)℃ and a humidity of (85±2)%, and the result was taken as the average value of the three samples.
[0055] PID192h:
[0056] The PID test and DH2000 aging test are tested with reference to the IEC61215 test standard. In the PID192 test, the cells and films are first prepared into photovoltaic modules according to the standard components, and the prepared photovoltaic modules are kept at a constant temperature in a room at 25°C for one day to ensure that the surface temperature of the modules is 25±1°C. The power tester is first calibrated with a standard plate, and then the initial power of the prepared modules is tested and recorded. The average value of the three tests is taken as the initial power generation power of the sample, which is the initial Pmax. Then the tested modules are placed in an aging box, the temperature is set to 85°C, the humidity is 85% RH, and a negative pressure of -1500V is applied. The aging time is 192h. After the aging is completed, the temperature is kept at a constant temperature in a room at 25°C for one day. The power after aging is tested, which is the power after aging, which is the Pmax after aging.
[0057] PID192h power attenuation = (initial Pmax - Pmax after aging) / initial Pmax * 100%
[0058] DH1000h aging
[0059] The DH1000 aging test first prepares the solar cells and films into photovoltaic modules according to the standard components, and keeps the prepared photovoltaic modules in a room at a constant temperature of 25℃ for one day to ensure that the surface temperature of the modules is 25±1℃. First, calibrate the power tester with a standard plate, then test the initial power of the prepared modules and record it. The average value of the three tests is taken as the initial power generation power of the sample, which is the initial Pmax. Then place the tested modules in an aging box, set the temperature to 85℃, the humidity to 85%RH, and the aging time to 2000h. After the aging is completed, keep the room at a constant temperature of 25℃ for one day, and test the power after aging, which is the power after aging, which is the Pmax after aging.
[0060] DH1000 power attenuation = (initial Pmax - Pmax after aging) / initial Pmax * 100%
[0061] In summary, the high-transmittance and corrosion-resistant photovoltaic encapsulation film and its preparation method of the present invention effectively reduce the water vapor permeability of the film by modifying the resin and the anti-acid additive, delay the side chain hydrolysis rate of the EVA resin, and improve the acetic acid adsorption and capture capacity. At the same time, the super-hydrophobic modified porous silicon nano-composite oxide anti-acid agent with a porous structure solves the problem of decreased transmittance and increased haze of the film after the addition of nano-oxides, effectively overcomes the anti-aging and corrosion problems of photovoltaic modules, and realizes the long-term stable operation of the modules.
[0062] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a highly transparent and corrosion-resistant photovoltaic encapsulation film, characterized in that: The steps include: Step S1, preparing porous silicon nanocomposite oxide by reacting tetraethyl orthosilicate and oxide precursor / porous oxide powder; Step S2, dissolving the super-hydrophobic additive in a mixed solution of ethanol and toluene, and mixing and stirring the mixture with the porous silicon nanocomposite oxide to obtain a super-hydrophobic modified porous silicon nanocomposite oxide antacid; Step S3, blending and granulating the EVA resin, peroxide, and silane coupling agent to obtain a grafted EVA resin; Step S4, blending the super-hydrophobic modified porous silicon nanocomposite oxide antacid with the grafted EVA resin and the EVA base material, adding an initiator, a co-crosslinking agent, a light stabilizer, an antioxidant, and a silane coupling agent, and then casting, embossing, cooling, and winding in a screw extruder to obtain a high-transmittance and corrosion-resistant photovoltaic encapsulation film; The oxide precursor / porous oxide powder includes at least one of magnesium acetate, magnesium sulfate, magnesium oxide, aluminum oxide, zinc oxide, zinc acetate, aluminum hydroxide, zinc hydroxide, hydrotalcite, zeolite, and molecular sieve; The silane coupling agent includes any one or more combinations of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-methacryloxypropyl trimethoxysilane; The step S1 comprises: placing tetraethyl orthosilicate and oxide precursor / porous oxide powder in a three-necked flask, adding an appropriate amount of ethanol, mixing and stirring, and heating to 50-70° C. to dissolve for 1 hour, then adding TMB pore expander and surfactant, mixing evenly, and dropwise adding a mixture of ammonia water and deionized water in a ratio of 1:1, adjusting the pH to 7-8, and continuing to react at 50-70° C. for 2-3 hours, and after the reaction is completed, transferring the reaction solution to a high-pressure reactor and crystallizing at 120° C. for 12 hours, and after the crystallization product is filtered, washed, and dried, it is placed in a muffle furnace and roasted in an air atmosphere at 400-600° C. for 4 hours to prepare a porous silicon nanocomposite oxide.
2. The preparation method according to claim 1, characterized in that The porous silicon nanocomposite oxide is in the form of nanospheres with a particle size of 30 to 100 nm; and There are stacked channels between the porous silicon nanocomposite oxides.
3. The preparation method according to claim 1, characterized in that: The step S2 includes: The super-hydrophobic additive is dissolved in a mixed solution of ethanol and toluene, mixed and stirred with the porous silicon nanocomposite oxide, cooled and refluxed at 80° C. for 6 to 8 hours, and then filtered, washed and dried to obtain a super-hydrophobic modified porous silicon nanocomposite oxide antacid.
4. The preparation method according to claim 1, characterized in that: The super hydrophobic additive comprises any one or more of n-octyl triethoxysilane, n-octyl trimethoxysilane, dimethyl silicone oil, stearic acid, stearic acid amide, glycidyl methacrylate, γ-methacryloxypropyl trimethoxysilane, γ-glycidyl ether oxypropyl trimethoxysilane, tridecafluorooctyl trimethoxysilane, tridecafluorooctyl triethoxysilane, heptadecafluorodecyl trimethoxysilane, hexamethyldisilazane, tetramethyldivinyldisilazane, tetramethyltetravinylcyclotetrasiloxane, and diethylaminomethyltriethoxysilane.
5. The preparation method according to claim 1, characterized in that: The grafted EVA resin has a VA content of 12-34 wt%.
6. The preparation method according to claim 1, characterized in that: The peroxide is composed of one or more of tert-butyl peroxycarbonate isopropyl ester, 2,5-dimethyl 2,5-bis(tert-butylperoxy)hexane, 1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxycarbonate-2-ethylhexyl ester, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, and tert-butyl peroxy 3,3,5-trimethylhexanoate, mixed in any proportion.
7. A high-transmittance and corrosion-resistant photovoltaic encapsulation film obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The super-hydrophobic modified porous silicon nano-composite oxide antacid of the high-transmittance and corrosion-resistant photovoltaic encapsulation film has a mass percentage of 0.2-1% and a light transmittance of greater than 92%; and The acid value after aging is less than 50ppm.
Citation Information
Patent Citations
Pillared layered silicon aluminum composite oxide and preparation method thereof
CN107398263A
High-viscosity and high-water-resistance packaging adhesive film, preparation method thereof and heterojunction battery assembly
CN116769425A