Cutting fluid for processing eyeglass lenses

By preparing a cutting fluid containing specific components, the problems of insufficient lubricity and poor powder settlement of existing water-based glass cutting fluids are solved, efficient lubrication and cooling effects are achieved, and the processing quality and service life of spectacle lenses are improved. , suitable for cutting and grinding processes of glass and resin.

CN117343783BActive Publication Date: 2024-10-29HUNAN BOYIDI OPTICAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311288688.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-08
Publication Date
2024-10-29
Estimated Expiration
2043-10-08

AI Technical Summary

Technical Problem

The existing water-based glass cutting fluid has insufficient lubricity in the processing of spectacle lenses, which leads to problems such as staining, edge chipping, and cracking of the processing tools. It is also unable to effectively remove glass powder and grinding powder, affecting the smoothness and processing quality of the lens surface.

Method used

A cutting fluid containing deionized water, white carbon black, cellulose acetate, sodium carboxymethylcellulose, capric acid, ceria and sodium antimonate is prepared through specific stirring and dilution methods. During the cutting and polishing process of spectacle lenses, cutting fluid is sprayed out from the nozzle to improve lubricity and cooling, and cerium dioxide and sodium antimonate are used to assist silica and cellulose acetate as the main lubrication body to enhance the powder settling performance.

Benefits of technology

This cutting fluid significantly improves the lubricity and cooling of eyeglass lens processing, reduces the amount of cutting fluid, improves surface finish, extends service life, and simplifies waste liquid treatment. It is suitable for cutting and grinding processes of glass and resin. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a cutting fluid for processing eyeglass lenses, which is prepared by using deionized water, white carbon black, cellulose acetate, sodium carboxymethyl cellulose, capric acid, cerium dioxide, sodium antimonate, lauroyl amide propyl betaine, and polyacrylamide as raw materials. When preparing the cutting fluid, deionized water is first divided into two parts; one part is dissolved by adding capric acid, and then cellulose acetate, sodium carboxymethyl cellulose, and lauroyl amide propyl betaine are added, and the mixture is stirred evenly to obtain a combined liquid I; the other part is stirred evenly, and then cerium dioxide and sodium antimonate are added and stirred twice, and the combined liquid II is obtained after stirring evenly; and then the combined liquid I is mixed with the combined liquid II to obtain a finished cutting fluid. The invention has good cooling and lubricity, and is easy to store at the same time, has better processing efficiency and processing effect for processing eyeglass lenses, and can effectively reduce the amount of cutting fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of processing eyeglass lenses, in particular to a cutting fluid for processing eyeglass lenses. Background Art

[0002] Eyeglass lenses are transparent materials with one or more curved surfaces made of optical materials such as glass or resin. After polishing, they are often assembled with eyeglass frames to form glasses. They are used to correct the user's vision and obtain a clear field of vision. Because the degree of each person's eyes is different, each lens needs to be precisely polished to ensure that it is suitable for personal use.

[0003] When processing eyeglass lenses in the optical field, the cutting and grinding are carried out separately. Generally, a lens cutting machine is used to cut the lenses into the same size and shape as the sample, and then they are precisely ground. The cutting and grinding processes will directly affect the assembly and use of the eyeglass lenses.

[0004] At present, glass cutting fluid is mainly used as the cutting medium in the processing of eyeglass lenses, which is mainly used for lubrication, cleaning and cooling in the process of lens cutting and grinding. There are many kinds of glass cutting fluids in the prior art, and the common water-based glass cutting fluids generally have applicability defects. For processing tools, they generally have the defect of poor lubricity, which leads to problems such as contamination, edge collapse, and cracking when processing eyeglass lenses, which directly affects the processing effect of eyeglass lenses. At the same time, the glass powder and grinding powder and other dirt powders generated in the process of eyeglass lens processing cannot be removed in time, and these dirt powders will adhere to the glass surface and affect the processing effect. They will wear the mirror surface during the processing of the eyeglass lens, causing scratches and damage to the mirror surface. Frequent maintenance is required to ensure the processing quality of the eyeglass lenses.

[0005] Based on the above reasons, a cutting fluid specially used for glasses processing has been developed, which has excellent lubricity, good cooling performance, fast glass powder settling speed and good cleaning performance and has better application value. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a cutting fluid for processing eyeglass lenses, which can solve the defects in the above technical background.

[0007] A cutting fluid for processing eyeglass lenses, specifically comprising the following components in parts by weight:

[0008] 60-100 parts of deionized water, 30-40 parts of white carbon black, 15-20 parts of cellulose acetate, 7-15 parts of sodium carboxymethyl cellulose, 3-5 parts of capric acid, 3-5 parts of cerium dioxide, 2-3 parts of sodium antimonate, 0.5-1.2 parts of lauramidopropyl betaine, 0.03-0.05 parts of polyacrylamide, and other additives for improving performance;

[0009] In the above raw material components: the white carbon black is fumed white carbon black; the sodium antimonate and the cerium dioxide are both nano-powders with a purity of more than 99.5%; the capric acid is one or a combination of n-decanoic acid, sebacic acid, and decanoic acid;

[0010] Cutting fluid is prepared by:

[0011] Divide the deionized water into two equal parts using a container;

[0012] Adding capric acid to a portion of deionized water, stirring thoroughly to dissolve it, then adding cellulose acetate, sodium carboxymethyl cellulose, and lauroylamidopropyl betaine, stirring thoroughly to obtain a combined solution I;

[0013] Add polyacrylamide to another portion of deionized water, stir thoroughly, then add cerium dioxide and sodium antimonate and stir again, and stir evenly to obtain a combined solution II;

[0014] The combined liquid I and the combined liquid II are mixed, and after mixing, white carbon black is continuously added and stirred, and a finished cutting fluid is obtained after stirring evenly.

[0015] As a further limitation, the preferred components of the cutting fluid for processing eyeglass lenses are:

[0016] 100 parts of deionized water, 40 parts of white carbon black, 18 parts of cellulose acetate, 10 parts of sodium carboxymethyl cellulose, 4 parts of capric acid, 4 parts of cerium dioxide, 2 parts of sodium antimonate, 1 part of lauroamidopropyl betaine, and 0.05 parts of polyacrylamide.

[0017] As a further limitation, the auxiliary agent is one or a combination of a surfactant, a dispersant, and an extreme pressure agent;

[0018] The surfactant is a nonionic surfactant or an anionic surfactant, and the added amount is 1-3% of the total mass of the cutting fluid. The nonionic surfactant is polysorbate 60 or polysorbate 80; the anionic surfactant is lignin sulfonate or dodecylbenzene sulfonate.

[0019] The dispersant is preferably an anionic dispersant, and the amount added is 0.7-1.5% of the total mass of the cutting fluid;

[0020] The extreme pressure agent is preferably a phosphate extreme pressure agent, and the added amount is 2.5-3.5% of the total mass of the cutting fluid.

[0021] As a further limitation, the particle size range of the sodium antimonate and the cerium dioxide is 200-800 nm, and the proportion of particles with a particle size range below 500 nm is ≥55%.

[0022] As a further limitation, when the cutting fluid is used during the cutting process, it is sprayed through a nozzle arranged on the side of the cutter, and the direction of the nozzle is such that the cutting fluid is sprayed directly from the front to the feed of the cutter.

[0023] As a further limitation, when the cutting fluid is used during the grinding process, it is sprayed through a nozzle arranged on the side of the grinding wheel. The nozzle is a flat-head fan-shaped nozzle, and the spraying plane of the flat-head fan-shaped nozzle corresponds to the normal plane of the grinding wheel, and the center position of the flat-head fan-shaped nozzle corresponds to the grinding contact position between the grinding wheel and the eyeglass lens.

[0024] As a further limitation, when the cutting fluid is used in the grinding process, it is diluted with 5 to 8 times the mass of deionized water to obtain a treatment liquid, and the treatment liquid is sprayed through a nozzle arranged on the side of the grinding wheel and covers the entire grinding area.

[0025] Beneficial effects: The cutting fluid for processing eyeglass lenses of the present invention is a water-soluble synthetic cutting fluid product, which overcomes the problem that optical lens cutting fluids in the past are not very versatile. It has a wide range of applications and can be simultaneously applied to the cutting and grinding processes of eyeglass lenses, especially suitable for fine grinding processes. The cutting fluid product has excellent cooling and powder sedimentation properties, can provide very high surface finish support, greatly improves the processing quality of eyeglass lenses, and can effectively reduce the amount of cutting fluid used in the cutting and grinding of various optical lenses, especially in the fine grinding process. DETAILED DESCRIPTION

[0026] In order to make the technical means, creative features, objectives and effects of the present invention easier to understand, the present invention is further described below in conjunction with specific embodiments. The described embodiments are only part of the embodiments of the present invention, not all of them.

[0027] In the following embodiments, those skilled in the art will understand that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of ordinary technicians in the field to which this application belongs. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In Example 1, the embodiment specifically includes the following raw materials in parts by weight:

[0029] 600kg deionized water, 300kg white carbon black, 200kg cellulose acetate, 80kg sodium carboxymethyl cellulose, 50kg capric acid, 50kg cerium dioxide, 30kg sodium antimonate, 10kg lauroamidopropyl betaine, and 500g polyacrylamide.

[0030] Among them, white carbon black is fumed white carbon black; sodium antimonate and cerium dioxide are both nano-powders with a purity of more than 99.5%, and the particle size range of the powder particles is 200~800nm, and the proportion of particles with a particle size range of less than 500nm in the sodium antimonate and cerium dioxide particles is 55~60%; capric acid is sebacic acid.

[0031] At the same time, the following are added: 2% of the total mass of the raw materials as polysorbate 80 as a surfactant; 0.8% of the total mass of the raw materials as sodium polyacrylate as an anionic dispersant; and 3% of the total mass of the raw materials as a phosphate extreme pressure agent.

[0032] During preparation, first divide the deionized water into two equal portions using a container, each portion is 300 kg;

[0033] Adding capric acid to one portion of the deionized water, stirring thoroughly to dissolve it, then sequentially adding cellulose acetate, sodium carboxymethyl cellulose, and lauroylamidopropyl betaine, stirring thoroughly to obtain a combined solution I;

[0034] Add polyacrylamide to another portion of deionized water, stir thoroughly, then add cerium dioxide and sodium antimonate powder and stir for a second time, and stir evenly to obtain a combined solution II;

[0035] The combined liquid I, the combined liquid II, and the auxiliary agents of polysorbate 80, sodium polyacrylate, and phosphate extreme pressure agent are mixed, and after mixing evenly, white carbon black is continuously added and stirred continuously, and after stirring evenly, a finished cutting fluid is obtained.

[0036] The external performance of the corresponding cutting fluid is as follows: specific gravity is 1.09±0.02g / ml; pH value (5% dilution) is 7.8; physical stability is good; there is no stratification or crystallization at 5±2℃ (72h), and no stratification at 65±2℃ (72h); the maximum non-seizure in the four-ball machine test is 74Pb / kg; the cutting efficiency is 0.82mm / min.

[0037] In Example 2, the embodiment specifically includes the following raw materials in parts by weight:

[0038] 1000kg deionized water, 400kg white carbon black, 160kg cellulose acetate, 14kg sodium carboxymethyl cellulose, 40kg capric acid, 30kg cerium dioxide, 25kg sodium antimonate, 8kg lauroamidopropyl betaine, and 400g polyacrylamide.

[0039] Among them, white carbon black is fumed white carbon black; sodium antimonate and cerium dioxide are both nano-powders with a purity of more than 99.5%, and the particle size range of the powder particles is 400-600nm, and the proportion of particles with a particle size range of less than 500nm in the sodium antimonate and cerium dioxide particles is 58-65%; capric acid is a mixture of n-decanoic acid and sebacic acid in a mass ratio of 1:1.

[0040] At the same time, the following are added: 1% of the total mass of the raw materials as polysorbate 60 as a surfactant; 1.2% of the total mass of the raw materials as ammonium polyacrylate as an anionic dispersant; and 3.5% of the total mass of the raw materials as a phosphate extreme pressure agent.

[0041] During preparation, first divide the deionized water into two equal portions using a container, each portion is 500 kg;

[0042] Adding capric acid to one portion of the deionized water, stirring thoroughly to dissolve it, then sequentially adding cellulose acetate, sodium carboxymethyl cellulose, and lauroylamidopropyl betaine, stirring thoroughly to obtain a combined solution I;

[0043] Add polyacrylamide to another portion of deionized water, stir thoroughly, then add cerium dioxide and sodium antimonate powder and stir for a second time, and stir evenly to obtain a combined solution II;

[0044] The combined liquid I, the combined liquid II, and the auxiliary agents polysorbate 60, ammonium polyacrylate, and the phosphate extreme pressure agent are mixed, and after mixing evenly, white carbon black is continuously added and stirred continuously, and after stirring evenly, a finished cutting fluid is obtained.

[0045] The corresponding cutting fluid has the following external properties: specific gravity is 1.11±0.03g / ml; pH value (5% dilution) is 7.9; physical stability is good; there is no stratification or crystallization at 5±2℃ (72h), and no stratification at 65±2℃ (72h); the maximum non-seizure value in the four-ball machine test is 73Pb / kg; and the cutting efficiency is 0.81mm / min.

[0046] In Example 3, the embodiment specifically includes the following raw materials in parts by weight:

[0047] 1000kg deionized water, 400kg white carbon black, 180kg cellulose acetate, 100kg sodium carboxymethyl cellulose, 40kg capric acid, 40kg cerium dioxide, 20kg sodium antimonate, 10kg lauroamidopropyl betaine, and 500g polyacrylamide.

[0048] Among them, white carbon black is fumed white carbon black; sodium antimonate and cerium dioxide are both nano-powders with a purity of more than 99.5%, and the particle size range of the powder particles is 300-600nm, and the proportion of particles with a particle size range of less than 500nm in the sodium antimonate and cerium dioxide particles is 65-70%; capric acid is a mixture of sebacic acid and decanedioic acid in a mass ratio of 1:1.

[0049] At the same time, the following are added: 1% of the total mass of the raw materials as polysorbate 60 as a surfactant; 1.2% of the total mass of the raw materials as sodium polyacrylate as an anionic dispersant; and 3.5% of the total mass of the raw materials as a phosphate extreme pressure agent.

[0050] During preparation, first divide the deionized water into two equal portions using a container, each portion is 500 kg;

[0051] Adding capric acid to one portion of the deionized water, stirring thoroughly to dissolve it, then sequentially adding cellulose acetate, sodium carboxymethyl cellulose, and lauroylamidopropyl betaine, stirring thoroughly to obtain a combined solution I;

[0052] Add polyacrylamide to another portion of deionized water, stir thoroughly, then add cerium dioxide and sodium antimonate powder and stir for a second time, and stir evenly to obtain a combined solution II;

[0053] The combined liquid I, the combined liquid II, and the auxiliary agents polysorbate 60, ammonium polyacrylate, and the phosphate extreme pressure agent are mixed, and after mixing evenly, white carbon black is continuously added and stirred continuously, and after stirring evenly, a finished cutting fluid is obtained.

[0054] The external performance of the corresponding cutting fluid is as follows: specific gravity is 1.11±0.02g / ml; pH value (5% dilution) is 7.9; physical stability is good; there is no stratification or crystallization at 5±2℃ (72h), and no stratification at 65±2℃ (72h); the maximum non-seizure in the four-ball machine test is 76Pb / kg; the cutting efficiency is 0.84mm / min.

[0055] The cutting fluids prepared in the above three groups of embodiments have relatively excellent lubricity and extreme pressure lubricity, good anti-foaming effect, the products are clear and transparent, easy to observe, and have high working efficiency.

[0056] It uses cerium dioxide and sodium antimonate to assist white carbon black and cellulose acetate as the main lubricating body, which can effectively meet the material processing requirements of optical glass and optical resin; at the same time, because the cutting fluid is an aqueous cutting fluid, it has better sedimentation properties on glass powder, so it has better cleaning properties after cutting, and due to the addition of capric acid, cellulose acetate and sodium carboxymethyl cellulose have better structural stability, which can extend the service life of the cutting fluid, so that it can usually be used for about 2 to 3 months (about 800 to 1200 processing cycles).

[0057] In addition, since this cutting fluid is superior to those that do not contain mineral oil, animal and vegetable oils, the product will not spoil and has a long storage and service life; it does not contain harmful substances such as S, P, Cl, phenol, etc., and the waste liquid treatment is simple, making it an environmentally friendly cutting fluid.

[0058] The combination of cellulose acetate and lauryl amide propyl betaine has good debris settling properties, can quickly settle and carry away glass debris, and can effectively improve the cleaning performance of the system cleaning and the surface finish of the side processing part of the eyeglass lens.

[0059] The above three groups of cutting fluids for eyeglass lens processing provided in the examples of this specific implementation manner can all be used for lubrication and cooling of the cutting, slicing and grinding processes of eyeglass lenses made of glass, resin glass and optical glass.

[0060] This cutting fluid can be used directly as the working fluid using the original liquid during the cutting and dicing process. When in use, it is sprayed through a nozzle arranged on the side of the cutter, and the direction of the nozzle is such that the cutting fluid is sprayed directly from the front to the feed of the cutter. In the corresponding processing process, the consumed working fluid is directly replenished with the original liquid.

[0061] When performing grinding, there are two ways to use it:

[0062] One way to use it is to use a flat fan-shaped nozzle to spray, the spray plane of the flat fan-shaped nozzle corresponds to the normal plane of the grinding wheel, and the center position of the flat fan-shaped nozzle corresponds to the grinding contact position between the grinding wheel and the eyeglass lens. In the corresponding processing process, the consumed working fluid is directly replenished with the original fluid.

[0063] Another method is to use 5-8 times the mass of deionized water as the working fluid. During the grinding process, the processing fluid is sprayed through a common nozzle set on the side of the grinding wheel and covers the entire grinding area. During the corresponding processing, the consumed working fluid can be replenished at a mass concentration of 20-30% of the original fluid.

[0064] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A cutting fluid for processing eyeglass lenses, characterized in that: The composition comprises the following components in parts by weight: 60-100 parts of deionized water, 30-40 parts of white carbon black, 15-20 parts of cellulose acetate, 7-15 parts of sodium carboxymethyl cellulose, 3-5 parts of capric acid, 3-5 parts of cerium dioxide, 2-3 parts of sodium antimonate, 0.5-1.2 parts of lauramidopropyl betaine, 0.03-0.05 parts of polyacrylamide, and other additives for improving performance; In the above raw material components: the white carbon black is fumed white carbon black; the sodium antimonate and the cerium dioxide are both nano-powders with a purity of more than 99.5%; the capric acid is one or a combination of n-decanoic acid, sebacic acid, and decanoic acid; The auxiliary agent is one or a combination of a surfactant, a dispersant, and an extreme pressure agent; The surfactant is a nonionic surfactant or an anionic surfactant, and the addition amount is 1-3% of the total mass of the cutting fluid. The nonionic surfactant is polysorbate 60 or polysorbate 80; the anionic surfactant is lignin sulfonate or dodecylbenzene sulfonate; Prepared by: Divide the deionized water into two equal parts using a container; Adding capric acid to a portion of deionized water, stirring thoroughly to dissolve it, then adding cellulose acetate, sodium carboxymethyl cellulose, and lauroylamidopropyl betaine, stirring thoroughly to obtain a combined solution I; Add polyacrylamide to another portion of deionized water, stir thoroughly, then add cerium dioxide and sodium antimonate and stir again, and stir evenly to obtain a combined solution II; The combined liquid I and the combined liquid II are mixed, and after mixing, white carbon black is continuously added and stirred, and a finished cutting fluid is obtained after stirring evenly.

2. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: The components of the cutting fluid for processing eyeglass lenses are: 100 parts of deionized water, 40 parts of white carbon black, 18 parts of cellulose acetate, 10 parts of sodium carboxymethyl cellulose, 4 parts of capric acid, 4 parts of cerium dioxide, 2 parts of sodium antimonate, 1 part of lauroamidopropyl betaine, and 0.05 parts of polyacrylamide.

3. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: The dispersant is an anionic dispersant, and the added amount is 0.7-1.5% of the total mass of the cutting fluid.

4. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: The extreme pressure agent is a phosphate extreme pressure agent, and the addition amount is 2.5-3.5% of the total mass of the cutting fluid.

5. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: The particle sizes of the sodium antimonate and the cerium dioxide are in the range of 200-800 nm, and the proportion of particles with a particle size below 500 nm is ≥55%.

6. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: When the cutting fluid is used in the cutting process, it is sprayed out through a nozzle arranged on the side of the cutter, and the direction of the nozzle is such that the cutting fluid is sprayed directly from the front to the feed of the cutter.

7. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: When the cutting fluid is used in the grinding process, it is sprayed through a nozzle arranged on the side of the grinding wheel. The nozzle is a flat-head fan-shaped nozzle, and the spraying plane of the flat-head fan-shaped nozzle corresponds to the normal plane of the grinding wheel, and the center position of the flat-head fan-shaped nozzle corresponds to the grinding contact position between the grinding wheel and the eyeglass lens.

8. The cutting fluid for eyeglass lens processing according to claim 1, characterized in that: When the cutting fluid is used in the grinding process, it is diluted with 5 to 8 times the mass of deionized water to obtain a treatment fluid, which is sprayed through a nozzle arranged on the side of the grinding wheel and covers the entire grinding area.

Citation Information

Patent Citations

  • Method for wafer dicing and composition useful thereof

    CN102311863A

  • Water-based cutting fluid used for glass processing

    CN105238536A