Preparation technology of neutral borosilicate vials
By adopting the process flow of upper tube, two-bottle integrated molding, separation and single-bottle molding on the horizontal vial-forming equipment, the bottle-making efficiency of vials is improved and the problem of low bottle-making yield in the existing technology is solved. Efficient production of neutral borosilicate vials was achieved.
Patent Information
- Application Number
- CN202311293611.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-10-08
AI Technical Summary
The existing vial preparation process has the problem of low output efficiency of finished products.
The preparation process of neutral borosilicate vials based on horizontal vial forming equipment is adopted, including the process of upper tube, two-bottle integrated molding, two-bottle integrated separation and single-bottle molding. The horizontal glass tube is combined with the equipment by fusing. The upper tube rhythm and stepping speed increase the bottle making capacity.
The bottle-making capacity is increased from 22 bottles/minute in the traditional process to about hundreds/minute, which solves the problem of low bottle-making productivity in the existing technology.
Smart Images

Figure CN117383815B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vial production, and in particular to a preparation process of a neutral borosilicate vial. Background Art
[0002] Vials, also known as borosilicate glass or soda-lime glass controlled injection bottles, are small bottles sealed with rubber stoppers and aluminum-plastic combination caps. With the development of the times, neutral borosilicate vials are increasingly used in the fields of biology, vaccines, powder injections, health care, cosmetics, and wine, and their application volume will increase in the future.
[0003] However, in the current industry, the production equipment for controlled vials is generally still a vertical bottle making machine that can only process one glass bottle at each station. Although the process is relatively mature, the production efficiency is limited. Therefore, there is a need for equipment and production processes that can meet both quantity and quality requirements for the preparation of controlled vials. Summary of the invention
[0004] A technical problem to be solved by the present invention is that the existing preparation process of vials has the problem of low finished product output efficiency.
[0005] In order to solve the above technical problems, the embodiment of the present invention provides a neutral borosilicate vial preparation process. The process is based on a vial horizontal molding device, and the process flow specifically includes: tube loading, two vials integrally molded, two vials integrally separated, single vial molding, and annealing;
[0006] The said upper tube refers to placing the glass tube into the process flow in a horizontal manner;
[0007] The two-bottle-in-one molding means: according to the cutting length and loss ratio of the two-bottle-in-one, the glass tube entering the process is simultaneously melted into multiple two-bottle-in-one; wherein, the two-bottle-in-one refers to a glass body with a length sufficient to be divided into two glass bottles and the bottoms of both ends are sealed;
[0008] The two-bottle-in-one separation refers to: dividing the two-bottle-in-one;
[0009] The single bottle forming refers to: preheating, gasification and stress elimination of the divided single bottle body, modifying the divided mouth, and making the bottle mouth.
[0010] In some embodiments, the steps of forming the two bottles into one piece include:
[0011] Positioning and preheating of the whole tube;
[0012] According to the cutting length and loss ratio of the two-bottle-in-one, the preheated glass tube is melt-cut to obtain the two-bottle-in-one;
[0013] The two bottles are subjected to stress relief, sorted in multiple columns, and transmitted to the two bottles separation process.
[0014] In some embodiments, the whole tube preheating operation includes: preheating the glass tube to 700-850° C. by a preheating device during the displacement gap during the whole tube transfer process; wherein the preheating device is arranged at a position 30-45 mm below the glass tube.
[0015] In some embodiments, the specific operation of the fuse cutting includes: determining the length of the two bottles as a whole according to the sum of the cutting length of the two bottles as a whole and the loss ratio, heating the glass tube by a first heating device 5-10 mm away from the glass tube, and performing multi-point cutting and separation by a separation and cutting device; wherein the first heating temperature is controlled at 1500-1650°C.
[0016] In some embodiments, the specific operation of stress relief includes: controlling the temperature of the two bottles in one body at 600-700° C. by a stress relief device 30-45 mm away from the two bottles in one body to relieve the stress.
[0017] In some embodiments, in the operation step of separating the two bottles, the separation operation uses a second heating device 5-10 mm away from the two bottles for heating; wherein the second heating temperature is controlled at 1500-1650°C.
[0018] In some embodiments, during the preheating, gasification and stress relief operations, the temperature is controlled at 400-550°C.
[0019] In some embodiments, the split mouth modification operation includes: performing separation plane penetration on two single bottle bodies and heating up the mouth for trimming.
[0020] In some embodiments, the operation of making the bottle mouth includes: making the bottle mouth by cooperating a linear mold and a mold core.
[0021] In some embodiments, in the tube loading process, the tube loading rhythm is controlled at 4-6.5s according to the milliliters of bottle production; in the two-bottle integral molding process, the stepping speed is controlled at 7-10 seconds to complete one displacement.
[0022] The neutral borosilicate vial preparation process provided by the present invention is based on a horizontal vial forming device, and its specific process flow includes: tube loading, two vials integrally formed, two vials integrally separated, single vial forming, and annealing. The present invention is based on a horizontal vial forming device, and the vial production capacity can be increased to about hundreds per minute by fusing a horizontal glass tube combined with the tube loading beat and stepping speed of the device, thereby solving the technical problem of low bottle production yield in the prior art.
[0023] In addition, the neutral borosilicate vial preparation process provided by the present invention ensures the production of neutral borosilicate vials on a horizontal machine, filling the technical gap in this industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 A process control flow chart of a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown;
[0026] Figure 2 A schematic diagram of the equipment layout of a horizontal vial forming equipment disclosed in an embodiment of the present invention is shown;
[0027] Figure 3 A flame process layout diagram of a horizontal vial in a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown;
[0028] Figure 4 A schematic diagram of a vial molding process of a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0029] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to exemplarily illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0030] The present invention provides these embodiments to make the present invention thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.
[0031] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0032] In addition, the words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" is not strictly perpendicular, but is within the tolerance range. "Parallel" is not strictly parallel, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.
[0033] All terms used in the present invention have the same meanings as those understood by ordinary technicians in the field to which the present invention belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, such as general dictionaries, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.
[0034] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.
[0035] The embodiment of the present invention provides a neutral borosilicate vial preparation process. The process is based on a vial horizontal molding device, and the process flow specifically includes: tube loading, two-bottle integral molding, two-bottle integral separation, single-bottle molding, and annealing.
[0036] Tube-raising refers to placing the glass tube into the process in a horizontal position.
[0037] Two-bottle-in-one molding means that the glass tube entering the process is simultaneously melted into multiple two-bottle-in-one according to the cutting length and loss ratio of the two-bottle-in-one. Among them, the two-bottle-in-one refers to a glass body that is long enough to be divided into two glass bottles and the bottoms of both ends are sealed.
[0038] Separating the two bottles as one body refers to dividing the two bottles as one body.
[0039] Single bottle molding refers to: preheating, gasification and stress elimination of the divided single bottle body, segmentation mouth modification and bottle mouth production.
[0040] In this embodiment, the entire process is carried out on a horizontal vial forming device, which includes a tube loading machine, a two-bottle integrated forming machine, and a two-bottle integrated separation, single product forming, and annealing integrated machine.
[0041] In specific implementation, the glass tube is placed in a horizontal manner in the two-bottle-in-one forming machine by a tube loading machine according to a certain tube loading rhythm, and the glass tube is pushed forward in the two-bottle-in-one forming machine according to the stepping speed of the two-bottle-in-one forming machine. The heating device in the two-bottle-in-one forming machine heats the entire glass tube during the pushing process and performs fusing and cutting. It should be pointed out that since the glass tube moves in a horizontal manner and the heating device is located under the glass tube to heat the entire glass tube, it is possible to simultaneously cut multiple parts of the glass tube during fusing and cutting to obtain multiple sections of two-bottle-in-one (for details, please refer to Figure 3 ).
[0042] In specific implementation, before entering the two-bottle-in-one separation process, the two-bottle-in-one can be stress-relieved first to ensure that the bottle body structure is not affected by stress and improve the subsequent single bottle molding quality.
[0043] The neutral borosilicate vial preparation process provided in the embodiment of the present invention is implemented based on the horizontal vial forming equipment. By fusing the horizontal glass tube combined with the tube upper beat and stepping speed, the bottle production capacity can be increased from 22 per minute in the traditional process to about hundreds per minute, thereby solving the technical problem of low bottle production yield in the prior art.
[0044] In some embodiments, the steps of forming two bottles in one piece include:
[0045] Positioning and preheating of the whole tube;
[0046] According to the cutting length and loss ratio of the two-bottle-in-one, the preheated glass tube is melt-cut to obtain multiple two-bottle-in-one;
[0047] Each two-bottle-in-one is subjected to stress relief, sorted in multiple columns, and transmitted to the subsequent two-bottle-in-one separation process.
[0048] When implementing it, Figure 1-3 As shown, after the tube is loaded by the tube loading machine, when the first photoelectric switch of the two-bottle-in-one forming machine senses the glass tube, the fixed-length cylinder cooperates with the mechanical structure plate to align and position the glass tube, and then preheats it; then, according to the cutting length and loss ratio of the two-bottle-in-one, the preheated glass tube is melt-cut to obtain multiple two-bottle-in-one; and each two-bottle-in-one is stress-eliminated through temperature reduction control, and then the multiple two-bottle-in-one are sorted in multiple columns through the transmission device of the two-bottle-in-one machine and transmitted to the two-bottle-in-one separation process.
[0049] The fuse cutting in this embodiment is to cut multiple locations of the glass tube at the same time to improve the yield of neutral borosilicate vials.
[0050] Based on the horizontal vial forming equipment, the two-bottle-in-one separation process in this embodiment is two identical processes performed simultaneously to improve work efficiency.
[0051] In some embodiments, the whole tube preheating operation includes: during the displacement gap during the whole tube transfer process, the preheating device preheats the glass tube to 700-850° C. The preheating device is arranged at a position 30-45 mm below the glass tube.
[0052] In specific implementation, the preheating device uses a wide handle lamp holder, and the glass tube is transferred through the stepping wheel, and the stepping speed is controlled to complete a displacement in 7-10 seconds. Figure 3 As shown, in the displacement gap, wide-handled lamps with a hole diameter of 0.45-0.6mm and 20 holes are arranged in a row of 10 at a distance of 30-45mm below the glass tube as needed, and two wide-handled lamp heads are arranged to uniformly preheat the glass tube to 700-850℃. The arrangement direction of the wide-handled lamp heads is consistent with the horizontal direction of the glass tube.
[0053] In this embodiment, a row of wide-handled lamp holders are fixed on the same horizontal axis by professional brackets, integrated at different distances and angles, and the wide-handled lamp holders are universal products.
[0054] In this embodiment, a wide-handled lamp holder with an aperture of 0.45-0.6 mm and 20 holes is used as a preheating device, which can keep the flame temperature more stable, better reflect the mixing ratio of oxygen and natural gas, and the flame intensity is centered. The glass can be preheated without being over-softened to affect the next step. The wide-handled lamp is placed 30-45 mm below the glass tube, so that the glass tube can be well preheated within the step speed, which is conducive to the subsequent fuse cutting.
[0055] In some embodiments, the specific operation of fuse cutting includes: determining the length of the two bottles as a whole according to the sum of the cutting length of the two bottles as a whole and the loss ratio, heating the glass tube by a first heating device 5-10 mm away from the glass tube, and performing multi-point cutting and separation by a separation and cutting device; wherein the first heating temperature is controlled at 1500-1650°C.
[0056] In specific implementation, the length requirement is accurately determined based on the cutting length of two bottles in one plus the loss ratio. The heating device is composed of 10 fishtail lights with a hole diameter of 0.4-0.5mm and a hole number of 9 in a row. The arrangement direction of the fishtail lights is consistent with the horizontal direction of the glass tube. The first heating device is set at a position 5-10mm below the glass tube to control the melting temperature of the glass tube, and the melting temperature is controlled within 1500-1650℃. The servo motor controls the pressing tube separation wheel to assist in the cutting and separation of the glass tube.
[0057] In this embodiment, a plurality of fishtail lamp holders are fixed on the same horizontal axis by professional brackets, integrated at different distances and angles, and the fishtail lamp holder is a universal product.
[0058] In this embodiment, the arrangement position and number of the fishtail lamp holders are conducive to controlling the required fusing temperature of the glass tube at the current stepping speed within 1500-1650°C.
[0059] In some embodiments, the specific operation of stress relief includes: controlling the temperature of the two-bottle-in-one body at 600-700° C. by a stress relief device 30-45 mm away from the two-bottle-in-one body to relieve the stress.
[0060] In this embodiment, by controlling the temperature of the two bottles in one body within the range of 600-700°C, it is beneficial to improve the yield of subsequent single bottles. Among them, the stress relief device is composed of 10 watt lamp heads with 0.45-0.6mm holes and 40 holes. The arrangement direction of the watt lamp heads is consistent with the horizontal direction of the glass tube.
[0061] In this embodiment, rows of tile lamp heads are fixed on the same horizontal axis by professional brackets, arranged and integrated at equal distances as required, and the tile lamp heads are universal products.
[0062] In some embodiments, in the operation step of separating the two bottles, the separation operation uses a second heating device 5-10 mm away from the two bottles for heating; wherein the second heating temperature is controlled at 1500-1650°C.
[0063] In specific implementation, the second heating device is composed of 6 segmented lamps with a hole diameter of 0.4-0.5 mm and a hole number of 7. The arrangement direction of the segmented lamps is consistent with the horizontal direction of the glass tube. The stepping wheel in this embodiment can have 7 lanes, and the specific number can be determined according to actual conditions.
[0064] In this embodiment, the logarithmic split lamp nozzles are fixed on the same horizontal axis through a professional bracket, arranged and integrated at equal distances as required, and the split lamp nozzles are universal products.
[0065] In this embodiment, the two bottles are transported into the post-processing area for positioning, and then step into the segmentation area for equidistant segmentation. During segmentation, a segmentation flame is set below the two bottles, and the segmentation wheel presses down to the bottle body from above, and the two bodies are separated in the process of heating and pressing.
[0066] In this embodiment, the above-mentioned splitting operation can increase the number of finished products of a single bottle and reduce material loss while ensuring rapid splitting.
[0067] In some embodiments, during the preheating gasification and stress relief operations, the temperature is controlled at 400-550°C.
[0068] In specific implementation, the temperature of a single bottle body is controlled at 400-550°C by 4 stepping wheels, 3 wide-handled lamps with 0.45-0.6mm holes and 20 holes to complete preheating, gasification and stress elimination of a single bottle body.
[0069] The gasification in this embodiment is to prevent glass chips from entering the bottle body when blowing through in the next step of the split mouth modification operation. Specifically, the hot gas generated by preheating during gasification forms air pressure which is released at the moment of blowing through to form an air wall to prevent glass chips from entering.
[0070] In some embodiments, the split mouth modification operation includes: performing separation plane penetration on two single bottle bodies and performing temperature trimming.
[0071] In specific implementation, when a single bottle body enters, a double-sided blowing lamp hole with an aperture of 0.4mm is used to penetrate the separation plane at the dividing openings of the two single bottles, and the temperature is increased to trim the openings, so as to improve the quality of the finished product and reduce defective products.
[0072] In some embodiments, the operation of making the bottle mouth includes: making the bottle mouth by cooperating a linear mold with a mold core.
[0073] In the specific implementation, in order to facilitate the operation and improve the work efficiency, a drawing can be drawn according to the bottle mouth requirements to produce a linear mold and a mold core with corresponding requirements to complete the production of the bottle mouth.
[0074] In some embodiments, in the tube loading process, the tube loading rhythm is controlled at 4-6.5s according to the milliliters of the bottle produced; in the two-bottle integrated molding process, the stepping speed is controlled at 7-10 seconds to complete one displacement.
[0075] In this embodiment, the upper tube beat is controlled at 4-6.5s, the stepping speed is controlled at 7-10 seconds / displacement, and the bottle making speed is increased from 22 bottles / minute (this speed is the maximum speed that a single machine of the original bottle making equipment can reach per minute) to about 150 bottles / minute.
[0076] In order to enable those skilled in the art to better understand the preparation process of the neutral borosilicate vial provided by the present invention, the applicant will explain it in conjunction with the following specific examples:
[0077] Figure 1 A process control flow chart of a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown; Figure 2 A schematic diagram of the equipment layout of a horizontal vial forming equipment disclosed in an embodiment of the present invention is shown; Figure 3 A flame process layout diagram of a horizontal vial in a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown; Figure 4 A schematic diagram of a vial molding process of a neutral borosilicate vial preparation process disclosed in an embodiment of the present invention is shown.
[0078] Combination Figure 1-4 The production process of the embodiment of the present invention is as follows:
[0079] 1. Place the glass tubes in the storage bin manually, unpack and align them.
[0080] 2. Press the start button of the tube loading machine, and the PLC in the tube loading machine will control the servo module built by the module and non-standard accessories through the program to work (the mobile loading module will grab, rise, transplant, drop, and open the storage bin to complete the tube loading needs). The tube loading beat is controlled within 4-6.5 seconds according to the milliliters of bottle production.
[0081] 3. After the tube is loaded, the stepper motor drives the intermediate chain (a closed loop is formed by the stepper motor through the combination of the bracket and the plate chain) to complete the connection between the tube loading machine and the molding machine (the tube loading machine puts the glass tube on the intermediate chain, and the intermediate chain transports the glass tube to the molding machine). The stepping speed is required to match the speed of the tube loading machine and the molding machine.
[0082] 4. Positioning of the entire tube (after the first photoelectric switch of the glass tube entering the forming machine senses the glass tube, the fixed-length cylinder cooperates with the mechanical structure plate to align and position the glass tube).
[0083] 5. The stepping speed will be controlled to complete one displacement in 7-10 seconds through the stepping wheel. In the displacement gap, wide handle lamps with an aperture of 0.45-0.6mm and 20 holes are arranged in a row at a distance of 30-45mm below the glass tube as needed, and two rows are arranged to preheat the glass tube evenly to 700-850℃.
[0084] 6. According to the cutting length of the two bottles plus the loss ratio, the length requirement is accurately determined, and the fishtail lamps with an aperture of 0.4-0.5mm and 9 holes are placed in a row of 10 at a distance of 5-10mm below the glass tube. The fusing temperature is controlled within 1500-1650℃, and the servo motor controls the tube separation wheel to assist in the separation of the glass tube.
[0085] 7. The two bottles rotate and step together to enter the watt lamp holder with an aperture of 0.4-0.5mm and 40 holes. Ten of them are arranged in a row at a distance of 30-45mm below the glass tube in two paths to control the temperature between 600-700℃ for stress elimination.
[0086] 8. The fourth stage of the molding machine divides the two-bottle-in-one object into two rows and sorts and transports them in two opposite directions.
[0087] 9. The conveyor transports the two-bottle body into the post-processing area for positioning and stepping into the segmentation area for equidistant segmentation (using 7 stepping wheels, 6 apertures with a diameter of 0.4-0.5mm and 7 apertures, and the temperature of the segmentation nozzles 5-10mm below the glass tube is controlled within 1500-1650℃ for fusing). The two bodies are separated with the cooperation of the separation wheel to obtain a single bottle body (i.e. Figure 4 The single bottle base shown in FIG.
[0088] 10. The temperature of the wide-handled lamp holder with 20 holes of 0.45-0.6mm at 3 locations on 4 stepping wheels is controlled at 400-550℃ to complete the preheating, gasification and stress elimination of a single bottle.
[0089] 11. When the single body enters, use the double-sided blow-through lamp hole with an aperture of 0.4mm to separate the two single bottles, and use the auxiliary heat preservation lamp head to heat and trim the cut. The gas generation in the previous step is to prevent glass chips from entering the bottle body when blowing through. The hot air generated by preheating forms air pressure and is released at the moment of blowing through, forming an air wall to prevent glass chips from entering.
[0090] 12. The PLC controls the synchronous motor to drive the automatic rotating cam to make the mold core enter the bottle body, complete the rotation and step forward at the same time (the speed can be adjusted here according to needs).
[0091] 13. Draw the drawings according to the bottle mouth requirements and make the corresponding linear mold and mold core to complete the production of the bottle mouth.
[0092] 14. Enter the annealing stage. The bottle making process is now complete.
[0093] So far, various embodiments of the present invention have been described in detail. In order to avoid obscuring the concept of the present invention, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.
[0094] Although some specific embodiments of the present invention have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present invention. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.
Claims
1. A process for preparing neutral borosilicate vials, characterized in that: The process is based on a horizontal vial forming device, and the process flow specifically includes: tube loading, two-bottle integral forming, two-bottle integral separation, single-bottle forming, and annealing; The said upper tube refers to placing the glass tube into the process flow in a horizontal manner; The two-bottle-in-one molding means: according to the cutting length and loss ratio of the two-bottle-in-one, the glass tube entering the process is simultaneously melted into multiple two-bottle-in-one; wherein, the two-bottle-in-one refers to a glass body with a length sufficient to be divided into two glass bottles and the bottoms of both ends are sealed; The two-bottle-in-one separation refers to: dividing the two-bottle-in-one; The single bottle forming refers to: preheating, gasification and stress elimination of the split single bottle body, split mouth modification, and bottle mouth production; the split mouth modification operation includes: separating plane penetration of two single bottle bodies and heating and mouth trimming.
2. The process according to claim 1, characterized in that The operation steps of forming the two bottles into one piece include: Positioning and preheating of the whole tube; According to the cutting length and loss ratio of the two-bottle-in-one, the preheated glass tube is melt-cut to obtain multiple two-bottle-in-one; Each two-bottle-in-one is subjected to stress relief, sorted in multiple columns, and transmitted to the two-bottle-in-one separation process.
3. The process according to claim 2, characterized in that The whole tube preheating operation includes: preheating the glass tube to 700-850° C. by a preheating device during the displacement gap during the whole tube transfer process; wherein the preheating device is arranged at a position 30-45 mm below the glass tube.
4. The process according to claim 2, characterized in that The specific operation of the fuse cutting includes: determining the length of the two bottles in one according to the sum of the cutting length of the two bottles in one and the loss ratio, heating the glass tube by a first heating device 5-10mm away from the glass tube, and performing multi-point cutting and separation by a separation and cutting device; wherein the first heating temperature is controlled at 1500-1650°C.
5. The process according to claim 2, characterized in that The specific operation of stress elimination includes: controlling the temperature of the two-bottle-in-one body at 600-700° C. by a stress elimination device 30-45 mm away from the two-bottle-in-one body to eliminate the stress.
6. The process according to claim 1, characterized in that In the operation step of separating the two bottles, the separation operation is performed by heating with a second heating device 5-10 mm away from the two bottles; wherein the second heating temperature is controlled at 1500-1650°C.
7. The process according to claim 1, characterized in that During the preheating, gasification and stress relief operations, the temperature is controlled at 400-550°C.
8. The process according to claim 1, characterized in that The operation of making the bottle mouth includes: making the bottle mouth by cooperating a linear mold with a mold core.
9. The process according to claim 1, characterized in that In the tube loading process, the tube loading rhythm is controlled within 4-6.5s according to the milliliters of the bottles produced; in the two-bottle integral molding process, the stepping speed is controlled within 7-10 seconds to complete one displacement.