A method for preparing and using a high compressive strength, swelling-resistant cellulose hydrogel

By employing a synergistic approach of salting out and ion coordination, high compressive strength hydrogels were prepared using cellulose as a raw material. This approach solved the problems of hydrogels being easily damaged and having poor mechanical properties, and enabled the preparation of hydrogels with high strength and good stability, which are suitable for flexible sensors and wearable devices.

CN117402377BActive Publication Date: 2026-11-17INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311534213.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2026-11-17
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Existing hydrogels are easily damaged during use, have poor mechanical properties, and their preparation process relies on petrochemical raw materials, resulting in high costs and making them difficult to promote.

Method used

By utilizing the synergistic effect of salting out and ion coordination, a transparent cellulose solution was prepared using cellulose as a raw material through a lithium hydroxide/urea/water dissolution system. The solution was then immersed in a polytetrafluoroethylene mold to form a cellulose hydrogel with high compressive strength.

Benefits of technology

The prepared cellulose hydrogel has excellent mechanical properties, high compressive strength, is not easily damaged, has good stability, long life cycle, and is widely available from raw materials. It is also simple to operate and suitable for widespread application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117402377B_ABST
    Figure CN117402377B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing and using a high compressive strength, swelling-resistant cellulose hydrogel. The invention utilizes the salting-out effect and the synergistic effect of ion coordination to prepare a high compressive strength cellulose hydrogel, and the introduction of nano-silver (AgNW) can endow it with sensing properties. The cellulose hydrogel prepared by this invention exhibits swelling resistance in different solutions and can degrade rapidly in soil, while also possessing excellent compressive strength. After introducing AgNW, the cellulose hydrogel can be assembled into a strain sensor that can be used for human motion monitoring. The raw materials are widely available and renewable, and the preparation method is simple and easy to promote.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing and using a cellulose hydrogel with high compressive strength, anti-swelling properties, and biodegradability, belonging to the technical field of cellulose hydrogel materials. Background Technology

[0002] Hydrogels are soft polymer materials with a three-dimensional cross-linked network structure. Due to their abundant hydroxyl groups, high water content, and flexibility, they have attracted considerable attention as carriers or frameworks for functional soft materials. However, hydrogels are prone to internal and external damage during use, reducing material stability, shortening their lifespan, and lacking energy dissipation mechanisms, resulting in poor mechanical properties. This makes them susceptible to breakage or fracture in practical applications, limiting their practical applications and functional development.

[0003] In recent years, scholars both domestically and internationally have conducted extensive research to improve the mechanical properties of hydrogels, developing a series of novel hydrogel systems that combine high strength and high toughness. Among these, utilizing the salting-out effect to improve the mechanical properties of polymer hydrogels such as polyvinyl alcohol chitosan and gelatin is a simple and efficient preparation method. However, it relies on petrochemical raw materials, requires a large amount of raw materials, involves complex processes, and is costly. Furthermore, it suffers from defects such as low compressive strength and poor swelling properties, which seriously hinder its practical application and make it difficult to promote.

[0004] Cellulose is characterized by its natural and green nature, wide availability, low cost, renewability, and non-toxicity. To date, there are no reports of using natural cellulose salting-out to prepare high compressive strength hydrogels. Summary of the Invention

[0005] This invention provides a method for preparing and using a high compressive strength, anti-swelling cellulose hydrogel. The cellulose hydrogel prepared by this invention exhibits excellent mechanical properties. Specifically, the cellulose hydrogel treated with aluminum sulfate achieves tensile and compressive stresses of 1.84 MPa and 16.99 MPa, respectively, and can degrade rapidly in soil. The hydrogel also demonstrates excellent anti-swelling properties in different pH solutions and solvents. With the addition of AgNW, it can be used as a sensor to detect minute deformations of human skin.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a high compressive strength, swelling-resistant cellulose hydrogel includes the following steps:

[0008] A. Add cellulose to a cellulose dissolving system of lithium hydroxide / urea / water to react and obtain a transparent cellulose solution;

[0009] B. The cellulose solution is loaded into a polytetrafluoroethylene mold and immersed in a salt solution to obtain a cellulose hydrogel.

[0010] This application provides a simple and scalable preparation method through the synergistic effect of salting out and ion coordination. This method uses abundant and environmentally friendly cellulose as raw material, which can expand the applicability and functionality of hydrogels, and the resulting product is...

[0011] Cellulose-based hydrogels, as functional materials, need to withstand certain stresses in important applications such as electrical sensors and tissue engineering. The limited compressive strength of existing hydrogels restricts their use. This application obtains cellulose-based hydrogels with ultra-high compressive strength through a simple method. These hydrogels are not easily damaged, have good stability, long lifespan, and excellent anti-swelling properties. The raw materials are widely available, the operation is simple, and they are suitable for widespread application.

[0012] As another implementation, a method for preparing a high compressive strength, swelling-resistant cellulose hydrogel includes the following steps:

[0013] A. Add cellulose to a cellulose dissolution system of lithium hydroxide / urea / water to react and obtain a transparent cellulose solution. Then add nano silver (AgNW) aqueous solution and stir evenly to obtain a mixed solution.

[0014] B. The mixture is poured into a polytetrafluoroethylene mold and immersed in a salt solution to obtain a cellulose hydrogel.

[0015] The cellulose in step A above is prepared by crushing virgin wood pulp into cellulose using a pulverizer and then vacuum drying it at 70±5℃ for 4±1h. Commercially available cellulose can be purchased directly.

[0016] The aforementioned virgin wood pulp includes cotton pulp, softwood pulp, and hardwood pulp, among which softwood pulp includes Masson pine pulp and spruce pulp, and hardwood pulp includes eucalyptus pulp and birch pulp.

[0017] In step A above, the concentration of the nano-silver aqueous solution is 3-6 mg / mL, preferably 5 mg / mL; the mass ratio of nano-silver aqueous solution to cellulose is (0.02-0.12):1.

[0018] The diameter and length of the silver nanoparticles in the aqueous solution are approximately 30 nm and 20 μm, respectively.

[0019] In step A above, the mass ratio of lithium hydroxide: urea: water in the cellulose dissolution system is (4-4.5):(12-15):(80-83.8).

[0020] To balance compressive strength and preparation cost, in step A, the mass percentage of cellulose relative to the cellulose dissolution system is 3–5 wt%; the reaction temperature is -10 to -20°C; and the reaction time is 5–30 min.

[0021] In step B above, the salt used in the salt solution is a metal ion or an ammonium ion (NH4+). + Compounds that combine with acid radicals. Preferably, the salt used in the salt solution is aluminum sulfate, sodium sulfate, zinc sulfate, sodium chloride, or magnesium sulfate. Most preferably, the salt used in the salt solution is aluminum sulfate. Aluminum citrate has low solubility at room temperature; experiments have shown that aluminum sulfate is significantly more effective than aluminum citrate in soaking.

[0022] In step B above, the concentration of the salt solution is 0.5–2M (M represents mol / L), the salt solution soaking temperature is room temperature, and the soaking time is 24–48 hours.

[0023] The cellulose hydrogel prepared by the above method can be used as a carrier or skeleton for flexible sensors, wearable devices and smart textiles.

[0024] The cellulose hydrogel prepared by the above method can be used to prepare flexible strain sensors for structural health monitoring and early warning, medical diagnosis and rehabilitation.

[0025] Any techniques not mentioned in this invention are based on existing technologies.

[0026] The technical solution of this invention has the following advantages:

[0027] 1) This invention utilizes the salting-out effect to prepare cellulose hydrogels. The raw materials are widely available and renewable biomass materials. The preparation method is simple, and the resulting hydrogels have excellent properties.

[0028] 2) The cellulose hydrogel prepared by this invention has significant compressive strength, is not easily damaged or broken, has good stability, and a long lifespan.

[0029] 3) The cellulose hydrogel prepared by this invention has good anti-swelling properties in different pH solutions and solvents.

[0030] 4) The cellulose hydrogel prepared by this invention can be degraded in soil.

[0031] 5) The cellulose hydrogel prepared by this invention can be used as a strain sensor to detect minute deformations of human skin. Attached Figure Description

[0032] Figure 1 The images show the SEM images of the hydrogel in Example 1 after soaking in different 1.0M salt solutions for 24 hours. (a) and (b) show the effects of cations and anions on its morphology.

[0033] Figure 2 The mechanical properties of the hydrogel in Example 1 after immersion in different 1.0M salt solutions for 24 hours are tested. (a) cationic tensile stress-strain curve, (b) cationic compressive stress-strain curve, (c) anionic tensile stress-strain curve, and (d) anionic compressive stress-strain curve.

[0034] Figure 3 This is a SEM image of the cellulose solution in Example 1 that was not soaked in the salt solution;

[0035] Figure 4 The average pore size is given by (a) the hydrogels prepared with different cations (sulfates) and (b) the hydrogels prepared with different anions (sodium salts) in Example 1.

[0036] Figure 5 The mechanical properties of the cellulose solution obtained in Example 2 after immersion in 1.5M aluminum sulfate solution for 3h, 6h, 12h, 24h and 48h are tested, where (a) is the tensile stress-strain curve and (b) is the compressive stress-strain curve.

[0037] Figure 6 The mechanical properties of the hydrogels obtained by soaking in aluminum sulfate solutions of different concentrations (0.25M, 0.5M, 1.0M and 1.5M) for 24 hours in Example 2 are tested, where (a) is the tensile stress-strain curve and (b) is the compressive stress-strain curve.

[0038] Figure 7 The swelling properties of the cel-Al2(SO4)3-1.0 hydrogel obtained in Example 3 were tested, where (a) is the swelling kinetic curve in deionized water and physiological saline, and (b) is the swelling kinetic curve in solutions with different pH values.

[0039] Figure 8 The mechanical properties of the cel-Al2(SO4)3-1.0 hydrogel obtained in Example 3 were tested after swelling in two different solvents and seven different pH acid and alkaline solutions for 25 days. (a) shows the compressive stress-strain curves in water and physiological saline, and (b) shows the compressive stress-strain curves in acid and alkaline solutions.

[0040] Figure 9 The degradation experiment of the cel-Al2(SO4)3-1.0 hydrogel obtained in Example 5 in soil;

[0041] Figure 10 Mechanical properties of Ag-Al2(SO4)3-1.0 hydrogel were tested, where (a) is the tensile stress-strain curve and (b) is the compressive stress-strain curve.

[0042] Figure 11Conductivity tests of Ag-Al2(SO4)3-1.0 hydrogels with different AgNW contents;

[0043] Figure 12 The swelling kinetics curves of cel-Al2(SO4)3-1.0 and Ag-Al2(SO4)3-1.0 hydrogels in aqueous solution are shown.

[0044] Figure 13 The strain sensitivity factor (GF) of the Ag-Al2(SO4)3-1.0 hydrogel obtained in Example 2 under different strains;

[0045] Figure 14 The sensing performance of the Ag-Al2(SO4)3-1.0 hydrogel obtained in Example 2 was tested. (a) The relative resistance response signal of the hydrogel under small strain (2%, 4%, 6% and 8%), the relative resistance response signal of the hydrogel when the human body (b) fingers, (c) wrists, (d) elbows, (e) knees were active, and (f) The relative resistance response signal of the hydrogel after 130 cycles at 5% strain.

[0046] Figure 15 This is a schematic diagram illustrating the preparation process of a high compressive strength, swelling-resistant cellulose hydrogel.

[0047] Figure 16 This is a comparison chart of the compressive strength of existing cellulose-based hydrogels (including physically cross-linked, chemically cross-linked, and physicochemically double-cross-linked hydrogels) of the cel-Al2(SO4)3-1.5 hydrogel obtained in Example 2. Detailed Implementation

[0048] To better understand the present invention, the following embodiments further illustrate the content of the present invention, but the content of the present invention is not limited to the following embodiments.

[0049] Example 1 describes the preparation of cellulose hydrogels soaked in salt solutions with different anions and cations. Example 2 describes the preparation of cellulose hydrogels soaked in aluminum sulfate solutions of different concentrations. Example 3 describes the study of the anti-swelling properties of cellulose hydrogels.

[0050] Example 4 is a soil degradation experiment of cellulose hydrogel. Example 5 is a study on the sensing properties of cellulose hydrogel.

[0051] Unless otherwise specified, all examples were performed at room temperature (20-25°C).

[0052] Example 1

[0053] Preparation of cellulose hydrogel: 20g of lithium hydroxide / urea / water (mass ratio 4.5:15:80.5) solution was cooled to -15℃, and then 1g of cellulose (coniferous wood pulp, Tianjin Wood Elf Biotechnology Co., Ltd.) was added. The solution was mechanically stirred at -15℃ (450rpm) for 20 minutes until the cellulose was completely dissolved, resulting in a transparent cellulose solution. The solution was then centrifuged at 10000rpm for 10 minutes to remove air bubbles and poured into a polytetrafluoroethylene mold. The solution was then immersed in 1.0M sodium salts (sodium citrate, sodium sulfate, sodium thiosulfate, sodium acetate, sodium chloride) and sulfates (aluminum sulfate, calcium sulfate, magnesium sulfate, zinc sulfate, potassium sulfate) at room temperature for 24h to obtain X-cel-OH hydrogel (X is the ion type). The cellulose solution without salt immersion was used as a blank test. Instructions: The PTFE mold is ring-shaped. After sealing the bottom of the mold with PTFE film, pour in the cellulose solution and then immerse it in the salt solution. The cellulose solution will solidify after one minute. Remove the PTFE film and continue soaking for the specified time.

[0054] SEM images of cellulose hydrogels are shown below. Figure 1 Its mechanical properties are shown in Figure 2 SEM images of cellulose solutions that were not soaked in salt solution are shown below. Figure 3 .Depend on Figure 2 From a and 2b, we can see that the order of mechanical strength of the cation series is: Al 3+ >Ca 2+ >Mg 2+ >Zn 2+ >K + Among them, Al-cel-OH exhibited the highest tensile strength (1.52 MPa) and superior compressive strength (11.11 MPa). This may be due to ionic coordination; higher valence cations are more conducive to crosslinking between cellulose molecules than lower valence cations, forming a tighter crosslinked network structure. The effects of different anions on the mechanical properties of the hydrogel were tested. Figure 2 c and 2d): Cit 3- SO4 2- >S2O3 2- >Ac - >Cl - The tensile strength of Cit-cel-OH reached 1.09 MPa when stretched to 132.32%. This may be due to the differences in the hydration capabilities of various anions, particularly Cit-cel-OH. 3- Due to its three carboxyl groups, it possesses strong hydration capabilities, resulting in hydrogels with denser cross-linked structures and maximizing mechanical properties. In this example, the salting-out effect is utilized to regulate the aggregation of cellulose chains at the molecular level, preparing hydrogels with different mechanical properties. Figure 1 and Figure 3Comparative analysis revealed that the hydrogels soaked in salt solutions possess a porous structure, resulting from ion-triggered polymer salting-out, which leads to the formation of pores in the hydrogel. Furthermore, it was found that hydrogels with higher mechanical properties have smaller pores; the average pore sizes of Al-cel-OH and Cit-cel-OH were 1.01 μm and 2.06 μm, respectively. Figure 4 In summary, cellulose hydrogels based on ion coordination and salting out exhibit excellent mechanical properties due to the enhanced cross-linking and densification of cellulose chains.

[0055] Example 2

[0056] A 20g lithium hydroxide / urea / water solution (mass ratio 4.5:15:80.5) was cooled to -15℃, and then 1g cellulose (coniferous wood pulp, Tianjin Wood Elf Biotechnology Co., Ltd.) was added. The solution was mechanically stirred at -15℃ (450rpm) for 20 minutes until the cellulose was completely dissolved, resulting in a transparent cellulose solution. The solution was then centrifuged at 10000rpm for 10 minutes to remove air bubbles, and finally poured into a polytetrafluoroethylene mold. The solution was then soaked in 0.25M, 0.5M, 1.0M, and 1.5M aluminum sulfate solutions at room temperature for 24 hours to obtain cel-Al2(SO4)3-0.25, cel-Al2(SO4)3-0.5, cel-Al2(SO4)3-1.0, and cel-Al2(SO4)3-1.5 hydrogels. Mechanical property testing was conducted using a barbell-shaped specimen measuring 4.5cm × 0.9cm × 0.3cm for tensile testing at a tensile rate of 20mm / min; and a cylindrical hydrogel specimen with a height of 1cm and a diameter of 0.7cm for uniaxial compression testing at a compression rate of 2mm / min. The mechanical properties of the hydrogel reaction solution after immersion in 1.5M aluminum sulfate solution at room temperature for 3h, 6h, 12h, 24h, and 48h were also investigated. Figure 5 The inventors discovered that the mechanical properties stabilized after immersion for 24 hours. The mechanical properties of the cel-Al2(SO4)3-0.25, cel-Al2(SO4)3-0.5, cel-Al2(SO4)3-1.0, and cel-Al2(SO4)3-1.5 hydrogels are shown below. Figure 6 (a) and (b) show that, due to the synergistic effect of salting out and ion coordination, the mechanical properties of the hydrogel are directly proportional to the concentration of the Al2(SO4)3 solution. When the concentration increases from 0.25M to 1.5M, the tensile and compressive strengths of the hydrogels increase from 0.95MPa to 1.84MPa and from 3.9MPa to 16.99MPa, respectively.

[0057] The cel-Al2(SO4)3-1.5 hydrogel prepared above (corresponding to...) Figure 16The compressive strength of the (five-pointed star) hydrogel was compared with that of existing cellulose-based hydrogels (including physically cross-linked hydrogels ref. 1, ref. 2 and ref. 3, chemically cross-linked hydrogels ref. 4, ref. 5 and ref. 6, and physicochemically dual-cross-linked hydrogels ref. 7, ref. 8 and ref. 9), and the results are as follows: Figure 16 As shown.

[0058] The hydrogels ref.1-9 were prepared according to the following references:

[0059] ref.1: Zhao, T., Zhang, S., Bi, Y., Sun, D., Kong, F., Yuan, Z., & Xin, X. (2020). Development and characterisation of multi-form composite materials based on silver nanoclusters and cellulose nanocrystals. Colloids and Surfaces A: Physicochemical and Engineering Aspects, 603, 125257.

[0060] ref.2: Kim, J., Jayaramudu, T., Zhai, LD, Kim, HC, & Agumba, DO (2020). Preparation of cellulose nanocrystal-reinforced physical hydrogels for actuator application. CurrComput-Aided Drug Des 10:969.

[0061] ref.3: Zhang, PX, Lin, H., Qu, C., Tang, YP, Li, NG, Kai, J., et al. (2015). Design, synthesis, and in vitro antiplatelet aggregation activities of ferulicacid derivatives. Journal of Chemistry, 2015.

[0062] ref.4: Ye, D., Zhong, Z., Xu, H., Chang, C., Yang, Z., Wang, Y., et al. (2016). Construction of cellulose / nanosilver sponge materials and their antibacterial activities for infected wounds healing. Cellulose, 23, 749-763.

[0063] ref.5: Ma, M., Yang, J., Ye, Z., Dong, A., Zhang, J., & Zhang, J. (2021). A simple strategy for synergistic integration of dynamic covalent bonds and hydrogen bonds to overcome the tradeoff between mechanical property and self-healing capacity of hydrogels. Macromolecular Materials and Engineering, 306(2), 2000577.

[0064] ref.6: Shao, C., Wang, M., Chang, H., Xu, F., & Yang, J. (2017). A self-healing cellulose nanocrystal-poly(ethylene glycol) nanocomposite hydrogel via Diels–Alder click reaction. ACS Sustainable Chemistry & Engineering, 5(7), 6167-6174.

[0065] ref.7:Ye,D.,Cheng,Q.,Zhang,Q.,Wang,Y.,Chang,C.,Li,L.,etal.(2017).Deformation drives alignment of nanofibers in framework for inducing anisotropic cellulose hydrogels with high toughness.ACS Applied Materials & Interfaces,9(49),43154-43162.

[0066] ref.8: Zhao, D., Huang, J., Zhong, Y., Li, K., Zhang, L., & Cai, J. (2016). High-strength and high-toughness double-cross-linked cellulose hydrogels: a new strategy using sequential chemical and physical cross-linking. Advanced Functional Materials, 26(34), 6279-6287.

[0067] ref.9: Rao, Z., Dong, Y., Liu, J., Zheng, X., Pei, Y., & Tang, K. (2022). Genipin-crosslinked gelatin-based composite hydrogels reinforced with amino-functionalized microfibrillated cellulose. International Journal of Biological Macromolecules, 222, 3155-3167.

[0068] Depend on Figure 16As can be seen, the cel-Al2(SO4)3-1.5 hydrogel of this application can withstand a compressive strength of 16.99 MPa. Compared with existing cellulose-based hydrogels (including physically cross-linked, chemically cross-linked, and physicochemically double-cross-linked cellulose-based hydrogels), this hydrogel exhibits superior mechanical properties, especially with a significant improvement in compressive strength.

[0069] Example 3

[0070] A cel-Al2(SO4)3-1.0 hydrogel was prepared according to the method in Example 2, and the following experiments were conducted:

[0071] Cylindrical cel-Al2(SO4)3-1.0 hydrogels were immersed at room temperature in 100 mL of deionized water, physiological saline (0.9 wt%), and acid / alkaline solutions of different pH values ​​for 25 days. The pH range of the acid / alkaline solutions was 2.0, 4.0, 6.0, 8.0, 10.0, 12.0, and 14.0. Their mass was measured at room temperature, and the swelling ratio (SR) was calculated using the following formula:

[0072] Among them, W t W0 represents the mass of the cel-Al2(SO4)3-1.0 hydrogel after immersion, and W0 represents the mass of the cel-Al2(SO4)3-1.0 hydrogel before immersion.

[0073] The swelling kinetics curves of the hydrogel in four different solvents are shown in the figure. Figure 7 Studies have shown that the hydrogel exhibits good anti-swelling properties during immersion at room temperature for up to 25 days, with equilibrium swelling rates of approximately -12.31% and -11.85% in deionized water and physiological saline (0.9% sodium chloride aqueous solution), respectively. The swelling kinetics curves of the hydrogel in solutions of different pH values ​​(NaOH or HCl) are shown below. Figure 7 b. After soaking at room temperature for 25 days, the hydrogel maintained good swelling properties. Within a pH range of 4-12, the absolute value of the equilibrium swelling rate was less than 14%. Furthermore, in solutions with pH values ​​of 2 and 14 (strong acid and alkaline conditions), the absolute values ​​of the equilibrium swelling rate were less than 3% and 6%, respectively. The mechanical strength of the hydrogel after 25 days of swelling was tested, and the results are as follows: Figure 8 (The horizontal axis represents the strain of the hydrogel, and the vertical axis represents the compressive strength that the hydrogel can withstand. The strain on the horizontal axis changes over time.) The mechanical property testing method is the same as in Example 2. The hydrogel still exhibits excellent mechanical properties after being soaked in other solvents and solutions of different pH values ​​at room temperature for 25 days, indicating their application potential in different environments. The anti-swelling property of cel-Al2(SO4)3-1.5 hydrogel was tested in the same manner, and all data improved by more than 8.2%.

[0074] Example 4

[0075] A 0.1 cm × 4 cm × 3 cm cel-Al2(SO4)3-1.5 hydrogel was prepared according to the method in Example 2 and buried at a depth of 5 cm in soil. Its biodegradability was determined by recording the morphological changes of the hydrogel in the soil over time. The geographical location was Nanjing (N: 32°04′N; E: 118°49′E), with a soil temperature of ~32℃. Figure 9 It can be seen that the morphology of the hydrogel began to change significantly after being buried in the soil for 10 days, which may be the result of the decomposition and metabolism of cellulose-degrading microorganisms in the natural environment. After 22 days of burial, the hydrogel was almost completely degraded. The degradation performance of cel-Al2(SO4)3-0.5 and cel-Al2(SO4)3-1.0 was tested using the same method, and the time to complete degradation was less than 20 days. This indicates that our hydrogel has good biodegradability and is beneficial to sustainable development.

[0076] As can be seen from the above, this hydrogel has high compressive strength, excellent degradability and anti-swelling properties, is simple to prepare and easy to promote, and has great application prospects in improving soil water retention capacity and fertility, as well as as a substrate material for flexible sensors and wearable devices.

[0077] Example 5

[0078] A 20g lithium hydroxide / urea / water solution (mass ratio 4.5:15:80.5) was cooled to -15℃, and then 1g cellulose (coniferous wood pulp, Tianjin Wood Elf Biotechnology Co., Ltd.) was added. The mixture was mechanically stirred at -15℃ (450rpm) for 20 minutes until the cellulose was completely dissolved. Then, 60μL of nano-silver aqueous solution (Xianfeng Nano, concentration 5mg / mL, diameter and length approximately 30nm and 20μm, respectively) was added dropwise. The mixture was stirred evenly for 20 minutes to obtain a hydrogel reaction solution. The solution was then centrifuged at 10000rpm for 10 minutes to remove air bubbles. Finally, the solution was poured into a polytetrafluoroethylene mold and soaked in 1.0M aluminum sulfate at room temperature for 24 hours to obtain Ag-Al2(SO4)3-1.0 hydrogel.

[0079] The Ag-Al2(SO4)3-1.0 hydrogel prepared above was subjected to the following experiments:

[0080] The mechanical properties of the Ag-Al2(SO4)3-1.0 hydrogel were tested, and the testing method was the same as in Example 2. Figure 10 It can be seen that the incorporation of AgNW has no significant effect on the mechanical properties of Ag-Al2(SO4)3-1.0 hydrogel. Furthermore, the electrical conductivity of hydrogels with different AgNW contents was tested, and the electrical conductivity of the hydrogel was directly proportional to the AgNW content. Figure 11The anti-swelling properties of the hydrogel were determined. Figure 12 It was found that the equilibrium swelling ratio of the hydrogel did not change significantly after the addition of AgNW. Hydrogel samples were prepared as 4cm × 1cm × 0.2cm specimens, and their sensitivity was shown in [the figure]. Figure 13 Tensile tests were conducted under different minute strains. The hydrogel sensor was able to capture the minute strains in the limb and exhibited stable changes in resistance signal. Figure 14 a) Test its force-sensing performance by attaching the hydrogel to fingers, wrists, elbows, and knees using 3M tape, such as... Figure 14 As shown in (b) to (e), the relative resistance response signal increases synchronously with limb flexion, and immediately returns to its initial state upon limb straightening. The hydrogel exhibits excellent force-sensitive sensing performance. Furthermore, the resistance change demonstrates good repeatability during cyclic limb flexion and straightening, such as... Figure 14 As shown in f, the hydrogel sensor exhibits excellent cycle performance over 130 consecutive cycles at 5% strain. Therefore, this hydrogel sensor can be applied to structural health monitoring and early warning, medical diagnosis and rehabilitation, and smart textiles, among other applications.

Claims

1. A method for preparing a high-compressive-strength, anti-swelling cellulose hydrogel, characterized by, Includes the following steps: A. Cellulose is added to a cellulose dissolution system of lithium hydroxide, urea and water to react and obtain a transparent cellulose solution. B. The cellulose solution is filled into a polytetrafluoroethylene mold and immersed in a salt solution to obtain a cellulose hydrogel; The cellulose in step A is obtained by vacuum drying the cellulose formed by crushing virgin wood pulp in a pulverizer at 70±5℃ for 4±1h. In step A, the mass ratio of lithium hydroxide:urea:water in the cellulose dissolution system is (4 ~ 4.5):(12 ~ 15):(80 ~ 83.8). In step B, the salt used in the salt solution is aluminum sulfate; the concentration of the salt solution is 0.5~2M, the soaking temperature of the salt solution is room temperature, and the soaking time is 24~48 h.

2. The production method according to claim 1, wherein Includes the following steps: A. Add cellulose to a cellulose dissolution system of lithium hydroxide, urea and water to react and obtain a transparent cellulose solution. Then add nano silver aqueous solution and stir evenly to obtain a mixed solution. B. The mixture is poured into a polytetrafluoroethylene mold and immersed in a salt solution to obtain a cellulose hydrogel.

3. The production method according to claim 2, characterized by: In step A, the concentration of the nano-silver aqueous solution is 3~6 mg / mL, and the mass ratio of the nano-silver aqueous solution to cellulose is (0.02~0.12):

1.

4. The production method according to any one of claims 1 to 3, characterized by: In step A, the mass of cellulose relative to the cellulose dissolution system is 3 to 5 wt%; the reaction temperature is -10 to -20℃; and the reaction time is 5 to 30 min.

5. Use of the cellulose hydrogel produced by the production process according to any one of claims 1 to 4, characterized in that: Carriers or frames used in flexible sensors, wearable devices, and smart textiles.