Two-component varnish composition and its preparation and use

By using a two-component varnish composition in automotive coatings, including hydroxyl (meth)acrylic resin, melamine resin and polyol ester, combined with polyisocyanate, the problem of insufficient resistance of the coating to corrosion by petroleum products is solved, and high performance is achieved. Hardness and water resistance, and maintains good performance under low temperature baking conditions.

CN117402541BActive Publication Date: 2024-10-11BASF COATINGS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311057101.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-21
Publication Date
2024-10-11
Estimated Expiration
2043-08-21

AI Technical Summary

Technical Problem

Existing automotive coatings show insufficient resistance when faced with corrosion by petroleum products and have poor reactivity, resulting in poor coating hardness and cross-linking density, making it difficult to meet the needs for high hardness and water resistance.

Method used

A two-component varnish composition is used, including hydroxyl (meth)acrylic resin, melamine resin and polyol ester. Through specific component proportions and structural design, a coating with a cross-linking point molecular weight of 300-700g/mol is formed. Polyisocyanate acts as a cross-linking agent to adjust the hardening speed and cross-linking density.

Benefits of technology

It achieves high hardness, petroleum product resistance and water resistance of the coating, while maintaining excellent finished product appearance, and is suitable for use under low-temperature baking conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_14
    Figure SMS_14
  • Figure SMS_15
    Figure SMS_15
  • Figure SMS_16
    Figure SMS_16
Patent Text Reader

Abstract

The present invention relates to a two-component varnish composition and its preparation and use. The present invention provides a two-component varnish composition, which comprises: component IA) a (meth) acrylic resin containing a hydroxyl group, B) a melamine resin, C) a polyol ester, wherein the polyol ester is a reaction product of one or more of castor oil, castor oil monoglyceride, and castor oil diglyceride with a polyol containing a primary hydroxyl group, an optional polyacid or anhydride; component II D) a polyisocyanate, wherein the varnish coating formed by the two-component varnish composition has a molecular weight between crosslinking points of 300 to 700 g / mol. The two-component varnish composition based on the present invention can form a paint film having excellent finished product appearance, high hardness, resistance to petroleum products, and water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of automobile coatings, and in particular to a two-component varnish composition and a preparation method and application thereof. Background Art

[0002] Car paint is applied in several layers, where the clearcoat is a transparent coating sprayed on the basecoat (such as basecoat), mainly used to protect the basecoat from the external environment and enhance the gloss and appearance of the car surface.

[0003] Clearcoats can be either one-component (1K) or two-component (2K) systems. For 2K systems, the clearcoat product is packaged separately in two drums and the formulations of the two drums are mixed before application on the primer. Most two-component clearcoat coatings are based on polyurethane chemistry, which is derived from the use of hydroxy-functional polyacrylate or polyester resins or polyols and isocyanate-based hardeners.

[0004] Patent Document 1 discloses a two-reagent package type clear coating composition, which comprises a specific hydroxy acrylate resin, a trifunctional HMDI isocyanurate compound and a polyester polyol, and forms a cured coating film that is excellent in scratch resistance, acid resistance, stain resistance and final appearance. However, the hardness and crosslinking density are still to be improved.

[0005] During the use of cars, it is inevitable that they will adhere to petroleum products such as asphalt on the road, leaked gasoline, lubricating oil, grease and brake fluid, which have a certain dissolving and corrosive effect on the car body coating. The varnish layer needs to have high resistance to petroleum products. Patent document 2 discloses a cross-linked varnish coating containing hydroxyl groups of acrylic resin, castor oil and melamine resin. Although the coating has good finished product appearance and hardness, the overall reactivity is poor, the product cures slowly, is easy to shrink, and has problems such as insufficient resistance to petroleum products and water resistance.

[0006] Therefore, it is necessary to provide a novel two-component varnish composition, which can form a paint film having excellent finished appearance and high hardness, resistance to petroleum products and water resistance.

[0007] References:

[0008] Patent document 1: CN101157814 B

[0009] Patent document 2: JP7200444 B1 Brief description of the invention

[0010] In one aspect, the present invention provides a two-component varnish composition comprising:

[0011] Component I

[0012] A) a (meth)acrylic resin containing a hydroxyl group,

[0013] B) melamine resin,

[0014] C) a polyol ester, which is a reaction product of one or more of castor oil, castor oil monoglyceride, castor oil diglyceride, a primary hydroxyl group-containing polyol, and optionally a polyacid or anhydride;

[0015] Component II

[0016] D) polyisocyanates,

[0017] The varnish coating formed by the two-component varnish composition has a molecular weight between crosslinking points of 300 to 700 g / mol, preferably 350 to 500 g / mol.

[0018] In another aspect, the present invention provides an article coated with the two-component clearcoat composition of the present invention.

[0019] In another aspect, the present invention provides a method for forming a multilayer coating film, comprising:

[0020] 1) optionally producing a cured first coating on a substrate;

[0021] 2) producing at least one primer coating on the coating obtained in step 1) by applying one or more identical or different primer materials;

[0022] 3) producing at least one clearcoat coating on the uppermost basecoat coating by applying one or more clearcoat materials which may be the same or different;

[0023] At least one of the varnish materials is a two-component varnish composition according to the present invention;

[0024] The primer coating and the clear coating are cured by baking separately or by combined baking. Preferably, the primer coating and the clear coating are cured by combined baking after step 3).

[0025] In another aspect, the present invention provides a multi-layer coating film prepared by the method for forming a multi-layer coating film according to the present invention.

[0026] Surprisingly, it is found that the two-component varnish composition based on the present invention can form a paint film with excellent finished product appearance, high hardness, resistance to petroleum products and water resistance. The polyol ester of the present invention adopts a specific structure with a relatively high hydroxyl value and reactivity, which has good compatibility with the hydroxyl-containing (meth) acrylic resin of the present invention and is not easy to precipitate from the system. The present invention uses melamine resin in the main agent (i.e., component I) to effectively adjust the curing speed. The components of the present invention are coordinated to obtain a varnish coating with a suitable cross-linking density, achieving a balance of various properties of the paint film. In some preferred embodiments of the present invention, through the selection of component types and physical property parameters, the two-component varnish composition of the present invention is also unexpectedly suitable for low-temperature baking. For example, the two-component varnish composition of the present invention is dried at 110°C, and the obtained multi-layer coating film can also show good appearance and high hardness, resistance to petroleum products and water resistance.

[0027] It should be noted that the above description does not disclose all embodiments of the present invention and all advantages of the present invention. DETAILED DESCRIPTION

[0028] The embodiments of the present invention are described below, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope of the invention claim, and the embodiments and embodiments obtained by appropriately combining the technical means disclosed in different embodiments and embodiments are also included in the technical scope of the present invention. In addition, all the documents recorded in this specification are cited in this specification as references.

[0029] Unless otherwise defined, technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0030] In the context of describing this specification (especially in the context of the following claims), the terms "a", "an", and "the" and similar language are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context.

[0031] In this specification, the numerical range expressed using "numerical value A to numerical value B" or "numerical value A-numerical value B" means a range including the endpoints numerical values ​​A and B.

[0032] In this specification, the meaning of "may" includes both the meaning of performing a certain process and the meaning of not performing a certain process. In this specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes the situation where the event occurs and the situation where the event does not occur.

[0033] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "some specific / preferred technical solutions", "other specific / preferred technical solutions", etc. refer to the specific elements (e.g., features, structures, properties and / or characteristics) related to the embodiments described herein being included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0034] In this specification, the term "comprises" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units that are not listed, or may optionally include other steps or units that are inherent to these processes, methods, products or devices.

[0035] In the present specification, the term "polyol ester" refers to a compound having two or more hydroxyl groups, wherein at least one of the hydroxyl groups is in the form of an ester.

[0036] In this specification, the term "2K" or "two-component" refers to a composition comprising two components, wherein each component can also be a mixture of several compounds. If necessary, the two components can be mixed together. The two components can also be two separate packages, which can be mixed on site for application.

[0037] In this specification, the term "acid value" refers to the mass of potassium hydroxide (KOH) in milligrams required to neutralize 1 gram of a chemical substance, which is a measure of the number of carboxylic acid groups in a compound or a mixture of compounds.

[0038] In this specification, the term "hydroxyl value" refers to the mass in milligrams of potassium hydroxide (KOH) required to neutralize acetic acid absorbed when 1 gram of a chemical substance containing free hydroxyl groups is acetylated, and is a measure of the free hydroxyl content in the chemical substance.

[0039] In this specification, the term "solid content" refers to the proportion of non-volatile matter contained in a paint, lacquer or other suspension, wherein the non-volatile matter is the material left after the volatile solvent evaporates.

[0040] In the present specification, the term "(meth)acrylic resin" refers to a product obtained by polymerizing a monomer composition containing at least one monomer selected from acrylic acid and its esters, methacrylic acid and its esters.

[0041] Two-component clearcoat composition

[0042] The present invention provides a two-component varnish composition, comprising:

[0043] Component I

[0044] A) a (meth)acrylic resin containing a hydroxyl group,

[0045] B) melamine resin,

[0046] C) a polyol ester, which is a reaction product of one or more of castor oil, castor oil monoglyceride, castor oil diglyceride, a primary hydroxyl group-containing polyol, and optionally a polyacid or anhydride;

[0047] Component II

[0048] D) polyisocyanates,

[0049] In the present invention, each component of the two-pack varnish composition may be used alone or in combination of two or more at a desired ratio.

[0050] In some embodiments of the present invention, the reactive material containing hydroxyl groups in the two-component varnish composition consists of component A and component C.

[0051] The varnish coating formed by the two-component varnish composition of the present invention has a molecular weight between crosslinking points of 300 to 700 g / mol, preferably 350 to 500 g / mol. The varnish coating formed by component I and component II has excellent hardness, resistance to petroleum products, water resistance and final appearance.

[0052] <Hydryl-containing (meth)acrylic resin>

[0053] Component A of the present invention is a hydroxyl-containing (meth) acrylic resin, which is the main film-forming resin in the two-component varnish composition. In some embodiments of the present invention, the glass transition temperature (i.e., T g ) is -50°C to 50°C, preferably, the glass transition temperature is -45°C to 25°C. In order to better balance the required properties, the present invention preferably uses a hydroxyl-containing (meth) acrylic resin with a low glass transition temperature, such as -45°C to -2°C. Compared with a hydroxyl-containing (meth) acrylic resin with a glass transition temperature above 0°C, the coating film obtained by combining it with other components of the present invention has good crosslinking density, hardness, water resistance, and resistance to petroleum products, while also having a better appearance.

[0054] In the present invention, the glass transition temperature of the hydroxyl group-containing (meth)acrylic resin is a value calculated using the following formula:

[0055] 1 / T g (K)=Σ(m i / T gi )

[0056] T g (℃)=T g (K)-273

[0057] T g : Glass transition temperature of hydroxyl-containing (meth) acrylic resin

[0058] m i : mole fraction of monomer component i

[0059] T gi : Glass transition temperature (K) of the homopolymer of monomer component i.

[0060] In addition, the glass transition temperature (K) of the homopolymer of the monomer component i can use the value described in the Polymer Handbook 2nd Edition (J. Brandup et al., ed.), etc. For a homopolymer of a monomer not described in the book, the glass transition temperature can be determined by synthesizing a homopolymer of a monomer having a weight average molecular weight of about 50,000 and measuring the glass transition temperature by differential scanning calorimetry.

[0061] In some embodiments of the present invention, one or more (meth) acrylic resins containing hydroxyl groups with a glass transition temperature within the aforementioned range can be directly prepared and / or selected as component A. In other embodiments of the present invention, two or more (meth) acrylic resins containing hydroxyl groups with different glass transition temperatures can be mixed as component A, as long as the glass transition temperature of the mixed component A meets the aforementioned range requirements. In a preferred embodiment of the present invention, component A is obtained by mixing a (meth) acrylic resin containing hydroxyl groups with a glass transition temperature of 12 to 40°C and a (meth) acrylic resin containing hydroxyl groups with a glass transition temperature of -40 to 0°C.

[0062] The present invention has no particular restrictions on the types of hydroxyl groups in the (meth) acrylic resin containing hydroxyl groups, such as secondary hydroxyl groups, primary hydroxyl groups, etc. In some embodiments of the present invention, the hydroxyl value of the (meth) acrylic resin containing hydroxyl groups is 130 to 220 mg KOH / g. When the hydroxyl value is within this range, a good crosslinking density can be given to the varnish coating film. If the hydroxyl value is too low, there is a tendency for the hardness, petroleum product resistance, and water resistance of the coating film to decrease. If the hydroxyl value is too high, it may have an adverse effect on the appearance. In some preferred embodiments of the present invention, the hydroxyl value of the (meth) acrylic resin containing hydroxyl groups is 150 to 200 mg KOH / g, more preferably 155 to 180 mg KOH / g, which is conducive to obtaining a coating film with good crosslinking density, hardness, petroleum product resistance, water resistance and appearance.

[0063] In some embodiments of the present invention, the weight average molecular weight (M) of the (meth) acrylic resin containing a hydroxyl group isw ) is 2000 to 10000 g / mol, preferably 2000 to 8000 g / mol, more preferably 3000 to 6500 g / mol. When the weight average molecular weight is within this range, the varnish coating film can have both advantages of appearance and durability.

[0064] The hydroxyl-containing (meth) acrylic resin of the present invention can be obtained, for example, by copolymerizing a hydroxyl-containing polymerizable unsaturated monomer with other copolymerizable monomers. A hydroxyl-containing polymerizable unsaturated monomer refers to a compound having at least one hydroxyl group and at least one polymerizable unsaturated bond per molecule. In some embodiments of the present invention, examples of hydroxyl-containing polymerizable unsaturated monomers include hydroxyalkyl esters of acrylic acid or methacrylic acid, and non-limiting examples include hydroxyalkyl (meth) acrylic acid esters with an alkyl carbon number of C1-C10 (preferably C2-C8), such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, hydroxypentyl (meth) acrylate, hydroxyhexyl (meth) acrylate, hydroxyheptyl (meth) acrylate, and one or more of hydroxyoctyl (meth) acrylate. In other embodiments of the present invention, hydroxyl-containing polymerizable unsaturated monomers also include one or more of N-hydroxymethyl (meth) acrylamide, allyl alcohol, and (meth) acrylates with hydroxyl-terminated polyoxyethylene chains. Preferably, the hydroxyl-containing polymerizable unsaturated monomer includes 2-hydroxyethyl acrylate (2-HEA), 2-hydroxyethyl methacrylate (2-HEMA), 3-hydroxypropyl acrylate (3-HPA), 3-hydroxypropyl methacrylate (3-HPMA), 4-hydroxybutyl acrylate (4-HBA), 4-hydroxybutyl methacrylate (4-HBMA), 1-hydroxyethyl acrylate (1-HEA), 1-hydroxyethyl methacrylate (1-HEMA), 1- or 2-hydroxypropyl acrylate (1- or 2-HPA), 1- or 2-hydroxypropyl methacrylate (1- or 2-HPA). The hydroxyl-containing polymerizable unsaturated monomer may be selected from the group consisting of 4-hydroxybutyl acrylate (4-HBA), 2-hydroxyethyl acrylate (2-HEA), 2-hydroxyethyl methacrylate (2-HEMA), 1-hydroxyethyl methacrylate (1-HEMA) and 2-hydroxypropyl methacrylate (2-HPMA).

[0065] The present invention does not particularly limit other copolymerizable monomers that can be polymerized with the hydroxyl-containing polymerizable unsaturated monomer. Examples of other copolymerizable monomers include C1-C20 alkyl (meth)acrylates, preferably C1-C10 alkyl (meth)acrylates, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl methacrylate (CHMA);

[0066] Aromatic ring-containing polymerizable unsaturated monomers such as styrene, α-methylstyrene, vinyltoluene, benzyl (meth)acrylate, etc.; carboxyl-containing polymerizable unsaturated monomers such as (meth)acrylic acid, maleic acid, crotonic acid, β-carboxyethyl acrylate, etc.; polymerizable unsaturated monomers having alkoxysilyl groups such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, etc.; vinyl compounds such as N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, vinyl acetate, etc.; nitrogen-containing polymerizable unsaturated monomers such as aminoalkyl (meth)acrylate, (meth)acrylamide or its derivatives; polymerizable unsaturated monomer compounds having carbonyl groups such as acrolein, acetoacetyl Oxyethyl methacrylate, formyl styrene, vinyl alkyl ketone with 4 to 7 carbon atoms, etc.; epoxy-containing polymerizable unsaturated monomers such as (meth) glycidyl acrylate, (meth) acrylate β-methyl glycidyl ester, 3,4-epoxycyclohexyl methyl (meth) acrylate, allyl glycidyl ether, etc.; (meth) acrylates with polyoxyethylene chains at the molecular end being alkoxy groups; polymerizable unsaturated monomers with phosphate groups such as 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 2-acryloyloxypropyl acid phosphate, 2-methacryloyloxypropyl acid phosphate, etc.; polymerizable unsaturated monomers with fluoroalkyl groups such as perfluoroalkyl (meth) acrylates and fluoroolefins, etc. Other copolymerizable monomers can be used alone or in combination of two or more monomers to react with the hydroxyl-containing polymerizable unsaturated monomers in the polymerization. Preferably, other copolymerizable monomers are selected from monomers having α,β-unsaturated double bonds, such as one or more of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, (meth)acrylic acid, and styrene.

[0067] The (meth) acrylic resin containing hydroxyl groups of the present invention can be prepared and synthesized by known methods such as free radical polymerization. As free radical polymerization initiators, azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, etc. can be cited; organic peroxides such as methyl ethyl ketone peroxide, cyclohexanone peroxide, 3,5,5-trimethylhexanone peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, tert-butyl peroxy-2-ethylhexanoate (TBPEH), tert-butyl peroxyneodecanoate, tert-butyl peroxylaurate, tert-butyl peroxybenzoate, tert-butyl peroxycarbonate, etc. can be used alone or in combination of two or more. There is no particular restriction on the amount of the free radical polymerization initiator.

[0068] Suitable organic solvents for polymerization include: aliphatic hydrocarbon solvents such as cyclohexane and ethylcyclohexane; aromatic hydrocarbon solvents such as toluene, xylene, ethylbenzene, and aromatic naphtha; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as ethyl acetate, n-butyl acetate, isobutyl acetate, and ethyl 3-ethoxypropionate; ether solvents such as dibutyl ether and tetrahydrofuran; and nitrogen-containing solvents such as acetonitrile, valeronitrile, and N,N-dimethylformamide. The organic solvent may be one kind or a mixed solvent of two or more kinds.

[0069] In some embodiments of the present invention, based on 100 parts by weight of the total solid content of component I, the content of the hydroxyl-containing (meth) acrylic resin (in terms of solid content) is 30 to 80 parts by weight, preferably 32 to 75 parts by weight, and more preferably 45 to 60 parts by weight.

[0070] <Melamine resin>

[0071] Component B of the present invention is a melamine resin, which refers to a partial methylol melamine resin and / or a complete methylol melamine resin obtained by the reaction of melamine with aldehydes. Non-limiting examples of aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, benzaldehyde, etc. In addition, the methylol of the above-mentioned methylol melamine resin partially or completely etherified by appropriate alcohol can also be used. Non-limiting examples of the alcohol used for etherification include one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, etc. Using melamine resin in combination with other components in the present invention can not only improve the hardness of the coating and increase the crosslinking density, but also surprisingly achieve system hardening rate regulation, solve the problems of petroleum product resistance and appearance control of the coating.

[0072] Melamine resins are well known to those skilled in the art and are supplied as commercial products by many companies. Examples of suitable low molecular weight, fully etherified melamine resins are CYTEC® from Cytec. 301 and 303, from BASF 066. From Solutia and MF. Examples of suitable, relatively low molecular weight, highly etherified melamine resins containing free imino groups are MF from Cytec. 325 and 327, 202 and 203, 062, 018 and 014; from BASF MF 927 and 3950, VMF 3611 and 3615 and 580, 717 and 718; 9539 from Solutia and 9539 from Akzo Resins US 138 and US 146. Examples of suitable relatively low molecular weight, partially etherified melamine resins are melamine resins from BASF 012, 016, 015, 018 and 010, from Solutia MF 590 and 600 and from Akzo Resins US 132 and 134. In the present invention, preference is given to using lower alcohols, in particular melamine resins etherified with methanol and / or ethanol and / or butanol, as crosslinking agents.

[0073] In some embodiments of the present invention, based on 100 parts by weight of the total solid content of component I, the content of melamine resin (in terms of solid content) is 1 to 35 parts by weight, preferably 3 to 30 parts by weight, and more preferably 5 to 20 parts by weight.

[0074] <Polyol Ester>

[0075] Component C of the present invention is a polyol ester, which is a reaction product of one or more of castor oil, castor oil monoglyceride, castor oil diglyceride and a polyol containing a primary hydroxyl group, an optional polyacid or anhydride. The present invention uses such a polyol ester, which has a higher hydroxyl value and reactivity than castor oil. In some embodiments of the present invention, the polyol ester of the present invention has excellent compatibility with the (meth) acrylic resin containing a hydroxyl group, and small molecules are not easy to precipitate from the system. In combination with other components of the present invention, the coating obtained has high water resistance, resistance to petroleum products, hardness and good appearance.

[0076] Castor oil is a vegetable oil obtained from the seeds of the Euphorbiaceae castor oil plant, which mainly includes triglycerides of unsaturated fatty acids (mainly ricinoleic acid: CH3(CH2)5CH(OH)=CH(CH2)7COOH, accounting for about 90%) and a small amount of saturated fatty acids (palmitic acid, stearic acid, etc.). The chemical structure of the main components of castor oil is shown in formula (I),

[0077]

[0078] Castor oil can be processed into castor oil monoglyceride and castor oil diglyceride by alcoholysis of glycerol. Castor oil monoglyceride is also called monoricinoleic acid glyceride, with molecular formula: C 21 H 40 O5; Castor oil diglyceride is also called glyceryl diricinoleate, molecular formula: C 39 H 72 O7.

[0079] In some embodiments of the present invention, one or more of castor oil, castor oil monoglyceride and castor oil diglyceride are reacted with the polyol containing primary hydroxyl to obtain polyol ester of the present invention, and the reaction is transesterification reaction.Through the transesterification reaction, the polyol ester with primary hydroxyl and based on ricinoleic acid and the polyol containing primary hydroxyl of the present invention is obtained.Primary hydroxyl refers to the hydroxyl connected with primary carbon atom.Primary carbon atom refers to the carbon atom directly connected to only one carbon atom and the carbon atom in methane.The non-limiting examples of the polyol containing primary hydroxyl in the present invention include one or more of ethylene glycol, propylene glycol, glycerol, trimethylolpropane, bis (trimethylolpropane), triethylolpropane, bis (triethylolpropane), pentaerythritol, bis (pentaerythritol), diglycerol, xylitol, sorbitol, galactitol, sucrose, polypropylene glycol, polyethylene glycol. In some embodiments of the present invention, the polyol containing primary hydroxyl groups preferably has more than 4 carbon atoms and contains more than two primary hydroxyl groups. Further preferably, in order to obtain better reaction activity and taking into account the compatibility with other components of the system, the polyol containing primary hydroxyl groups is selected from one or more of pentaerythritol, trimethylolpropane, and sorbitol. In some specific embodiments, a small amount of polypropylene glycol and polyethylene glycol can also be included at the same time. The conditions of the transesterification reaction can adopt conventional reaction conditions in the art, and preferably a catalyst is used to promote the reaction. The catalyst includes one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium methoxide, lead oxide, zinc oxide, and tetrabutyl titanate. Preferably, the catalyst is selected from tetrabutyl titanate. In some specific embodiments of the present invention, the transesterification reaction can be reacted for 2-5 hours at a reaction temperature of 140-250°C under the protection of an inert gas.

[0080] In other specific embodiments of the present invention, the polyol ester of the present invention is the reaction product of one or more of castor oil, castor oil monoglyceride and castor oil diglyceride with a polyol, polyacid or anhydride containing a primary hydroxyl group. By adding a polyacid or anhydride as a modifier, the reaction system includes both the esterification of a polyacid or anhydride and a polyol containing a primary hydroxyl group, and also includes the esterification reaction of castor oil monoglyceride, castor oil diglyceride and a polyacid or anhydride and the transesterification reaction of a polyol containing a primary hydroxyl group with castor oil. The polyol ester synthesized by this method is a polyester polyol based on ricinoleic acid, which contains a hydroxyl group, an ester group and a long-chain alkyl group, and can have good compatibility with the hydroxyl-containing (meth) acrylic resin of the present invention. In order to obtain better reactivity, preferably, the polyol ester of the present invention has a primary hydroxyl group. The polyacid or anhydride is preferably a polyacid or anhydride having a carbon atom of C4-C12. The non-limiting examples of the polyacid include one or more of glutaric acid, adipic acid, phthalic acid, and isophthalic acid. In some preferred embodiments of the present invention, the acid anhydride is an acid anhydride with a cyclic structure, such as one or more of phthalic anhydride, hexahydrophthalic anhydride, and phthalic anhydride. In some embodiments of the present invention, polyacids or anhydrides can be added to the reaction system together with one or more of castor oil, castor oil glycerol monoester, castor oil diglycerol, and a polyol containing primary hydroxyl group to carry out polycondensation reaction. In other embodiments of the present invention, one or more of castor oil, castor oil monoglyceride, and castor oil diglyceride are first subjected to transesterification reaction with a polyol containing primary hydroxyl group to obtain a castor oil alcoholysis product, and then polyacids or anhydrides are added to carry out polycondensation reaction. The transesterification reaction is the same as described above. The conditions of the polycondensation reaction can also adopt conventional reaction conditions in the art, preferably using a catalyst to promote the reaction, the catalyst includes one or more of tetrabutyl titanate, tetraisopropyl titanate, tetraisobutyl titanate, tin tetrachloride, and diethylamine, and the catalyst is preferably selected from tetrabutyl titanate. In some specific embodiments of the present invention, the polycondensation reaction can be carried out under the protection of an inert gas at a reaction temperature of 140 to 250° C. for 2 to 5 hours.

[0081] In some embodiments of the present invention, the hydroxyl value of the polyol ester of the present invention is 180 to 500 mg KOH / g. If the hydroxyl value is too low, the reaction activity is low, the coating cures slowly and is easy to shrink; if the hydroxyl value is too high, it is easy to cause insufficient hydroxyl reaction, which has an adverse effect on the water resistance of the coating and may also cause cracking of the coating. In order to obtain a coating with excellent properties, the hydroxyl value of the polyol ester is further preferably 200 to 450 mg KOH / g. In order to make the coating obtain higher hardness, resistance to petroleum products, water resistance and better appearance, the hydroxyl value of the polyol ester is more preferably 240 to 400 mg KOH / g.

[0082] In some embodiments of the present invention, the weight average molecular weight of the polyol ester of the present invention is 1000 to 3000 g / mol, and more preferably 1200 to 2800 g / mol.

[0083] In some embodiments of the present invention, in order to improve compatibility with other components of the present invention, the molecular weight distribution PDI of the polyol ester of the present invention is above 1.5, more preferably above 1.8, and more preferably above 2.0.

[0084] In some embodiments of the present invention, based on 100 parts by weight of the total solid content of component I, the content of polyol ester is 5 to 35 parts by weight. In some specific embodiments of the present invention, in order to make the coating have better resistance to petroleum products, water resistance and / or appearance, it is preferably 8 to 20 parts by weight.

[0085] <Polyisocyanate>

[0086] Component D of the present invention is a polyisocyanate, which acts as a crosslinking agent. Polyisocyanates are a general term for compounds containing two or more isocyanate groups in the molecule (those skilled in the art understand that it refers to free isocyanate groups with a general structure of -N=C=O), including monomeric polyisocyanates and / or oligomeric polyisocyanates. The simplest and most important representative of these polyisocyanates is diisocyanate. They have a general structure of O=C=NRN=C=O, where R usually represents an aliphatic, alicyclic and / or aromatic group. Examples of polyisocyanates of the present invention include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic aliphatic polyisocyanates, aromatic polyisocyanates and derivatives of these polyisocyanates, etc. They can be used alone or in combination of two or more. Examples of the polyisocyanates of the present invention include propylene diisocyanate, butylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, 1,8-diisocyanato-4-(isocyanatomethyl)octane, dimer fatty acid diisocyanate, methyl 2,6-diisocyanohexanoate, 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, isocyanate, In one preferred embodiment, the polyisocyanate is an aliphatic polyisocyanate and / or an alicyclic polyisocyanate, such as hexamethylene diisocyanate (HDI) and / or isophorone diisocyanate. In a preferred embodiment, polyisocyanate is an oligomeric isocyanate compound, such as isocyanate dimer, isocyanate trimer, etc. In a specific embodiment, polyisocyanate is a trimer of HDI. Polyisocyanate can be obtained by reacting excessive isocyanate with water or polyol (such as ethylene glycol, propylene glycol, 1,3-butylene glycol, hexylene glycol, etc.), or by reacting isocyanate with itself. Polyisocyanate for the present invention can be purchased commercially. Commercial suppliers include Bayer, BASF, Asahi Chemical Co., Ltd., and suitable polyisocyanates are sold under trade names such as Desmodur, Duranate, Tolonate, Basonate.

[0087] In some embodiments of the present invention, the NCO content of the polyisocyanate is preferably 10%-30%, and more preferably 15%-25%.

[0088] In some preferred embodiments of the present invention, the polyisocyanate of the present invention is an unblocked polyisocyanate. Compared with blocked polyisocyanates, the use of the unblocked polyisocyanate of the present invention is conducive to achieving low-temperature baking.

[0089] The content of polyisocyanate is not particularly limited. From the perspective of better promoting the curing reaction, the molar equivalent ratio NCO / OH of the isocyanate group of the polyisocyanate and the total hydroxyl group of component A and component C of the present invention is 0.8 to 1.5:1, preferably 0.9 to 1.3:1.

[0090] <Other components>

[0091] The two-component varnish composition of the present invention also includes a solvent and other components optionally used in combination as needed, such as a curing catalyst, a rheology control agent, an ultraviolet absorber, a light stabilizer, a pigment, a defoamer, a leveling agent, an antioxidant, a film former, a surface conditioner, etc.

[0092] The two-component varnish composition of the present invention can be water-based or organic solvent-based. As the organic solvent, one or more of acetone, toluene, xylene, ethyl acetate, butyl acetate, isopropyl alcohol, n-butyl alcohol, 2-ethylhexyl alcohol, and ethyl 3-ethoxypropionic acid ester can be exemplified. Water and organic solvents can be used in combination. There is no particular restriction on water, which can be ion-exchanged water. In some specific embodiments of the present invention, the two-component varnish composition is organic solvent-based.

[0093] In some embodiments of the present invention, the two-component varnish composition of the present invention may optionally include a curing catalyst. The curing catalyst includes carboxylates of tin, zinc, titanium, lead, iron, bismuth, barium and zirconium; non-metallic catalysts such as tertiary amines, 1,4-diazabicyclo[2.2.2]octane (DABCO), diazabicycloundecene, phosphorus-containing catalysts such as substituted phosphonic acid monoesters, phosphonic acid diesters, diphosphonic acid diesters (preferably selected from acyclic phosphonic acid diesters, cyclic phosphonic acid diesters, acyclic diphosphonic acid diesters, and cyclic diphosphonic acid diesters) and / or amine adducts thereof (preferably amine-blocked ethylhexyl phosphonate and amine-blocked phenyl phosphonate), sulfonic acid catalysts such as dodecylbenzenesulfonic acid (DDBSA), dinonylnaphthalene disulfonic acid (DNNSA), p-toluenesulfonic acid (p-TSA) and blocked sulfonic acid catalysts such as blocked DDBSA, blocked DNNSA or blocked p-TSA. It is preferred to use sulfonic acid catalysts and phosphorus-containing catalysts to ensure the stability and durability of the coating system. In some preferred embodiments of the present invention, amine-blocked phosphoric acid catalysts are preferred, which have high catalytic efficiency and a stable and controllable effect on the appearance and performance of the paint film. Based on 100 parts by weight of the total solid content of component I, the amount of the curing catalyst is 0.01 to 2 parts by weight, preferably 0.05 to 1 part by weight.

[0094] In some embodiments of the present invention, the two-component varnish composition of the present invention may optionally include a rheology control agent. Conventionally known rheology control agents may be used, for example, clay minerals (e.g., metal silicates, montmorillonite), (meth) acrylic acid, polyolefins (e.g., polyethylene, polypropylene, etc.), amides (higher fatty acid amides, polyamides, etc.), polycarboxylates, celluloses (including various derivatives such as nitrocellulose, acetylcellulose, cellulose ethers, etc.), carbamates (polymers and / or oligomers containing carbamate structures in the molecule, etc.), ureas (polymers and / or oligomers containing urea structures in the molecule). Based on 100 parts by weight of the total solid content of component I, the amount of the rheology control agent (in terms of solid content) is 8 to 35 parts by weight, preferably 10 to 30 parts by weight.

[0095] In some embodiments of the present invention, the two-component varnish composition of the present invention may also optionally include conventionally known ultraviolet absorbers, such as benzotriazole absorbers, triazine absorbers, salicylic acid absorbers, benzophenone absorbers, etc. These can be used alone or in combination of two or more.

[0096] In some embodiments of the present invention, the two-component varnish composition of the present invention may also optionally include a conventionally known light stabilizer such as a hindered amine light stabilizer, etc. Examples of hindered amine light stabilizers include acylated hindered amines, amino ether hindered amines, and the like.

[0097] In some embodiments of the present invention, the two-component clear coating composition of the present invention may further optionally include a pigment such as a colorant, an anti-rust pigment, etc., which may be contained in an amount that does not substantially impair the transparency of the formed coating film.

[0098] Those skilled in the art may choose to add other additives such as defoamers, leveling agents, antioxidants, film-forming agents, surface conditioners, etc. as needed, and the amount used may also be determined according to actual applications.

[0099] In some embodiments of the present invention, the weight ratio (based on solid content) of component I to component II of the two-component varnish composition of the present invention is 1 to 5:1, preferably 1.5 to 3.5:1.

[0100] Articles coated with two-component clearcoat composition

[0101] The two-component varnish composition of the present invention can be applied by any method in the prior art, such as air sprayer, electrostatic air sprayer, roller coater, flow coater or dip coater or brush coater or rod coater, or applicator, etc. The present invention preferably adopts the spraying method.

[0102] There is no restriction on the thickness of the varnish coating obtained by applying the two-component varnish composition of the present invention, but the thickness of the paint film after drying is preferably in the range of 10 μm to 150 μm, more preferably in the range of 30 μm to 60 μm. The varnish coating formed by the two-component varnish composition of the present invention has a molecular weight between crosslinking points of 300 to 700 g / mol. The molecular weight (MC) between crosslinking points refers to the average molecular weight of the segment between two adjacent crosslinking points. The smaller the average molecular weight between two adjacent crosslinking points, the more crosslinking points there are and the greater the crosslinking density. In the present invention, if the molecular weight between the crosslinking points is too low, it will affect the mechanical properties of the coating such as tensile properties, and cracking will easily occur during the hardening process, resulting in poor appearance of the coating; if the molecular weight between the crosslinking points is too high, the crosslinking density is insufficient, which will also lead to a decrease in hardness, resistance to petroleum products and water resistance. In some embodiments of the present invention, in order to balance the various properties required for the coating, the molecular weight between the crosslinking points is preferably 310 to 500 g / mol, and further preferably 350 to 500 g / mol.

[0103] Examples of substrates for coating the two-component clearcoat composition of the present invention include inorganic and organic materials, such as metal, wood, glass, cloth, plastic, foam, elastomer, paper, ceramic, concrete, gypsum board, etc., and preferably metal substrates. These base materials may or may not be pretreated.

[0104] The present invention also provides articles coated with the two-component varnish composition of the present invention. Examples of the obtained or obtainable coated articles include metal products, structural materials, wood products, plastic products, rubber products, paper products, ceramic products, glass products, etc., more specifically, they include automobiles and automobile parts (e.g., bodies made of various materials, bumpers, spoilers, mirrors, wheels, interior decoration parts, etc.), metal plates such as steel plates, bicycles, bicycle parts, materials used on roads (e.g., guardrails, traffic signs, soundproof walls, etc.), tunnels (e.g., sidewall panels, etc.), ships, railway locomotives, aircraft, furniture, musical instruments, household appliances, building materials, containers, office accessories, sports accessories, toys, etc. Preferred coated articles of the present invention are automobiles and automobile parts.

[0105] Method for forming multilayer coating film

[0106] The present invention also provides a method for forming a multilayer coating film, comprising:

[0107] 1) optionally producing a cured first coating on a substrate;

[0108] 2) producing at least one primer coating on the coating obtained in step 1) by applying one or more identical or different primer materials;

[0109] 3) producing at least one clearcoat coating on the uppermost basecoat coating by applying one or more clearcoat materials which may be the same or different;

[0110] At least one of the varnish materials is a two-component varnish composition of the present invention;

[0111] The primer coating and the clear coating are cured by baking separately or by combined baking. Preferably, the primer coating and the clear coating are cured by combined baking after step 3).

[0112] In this method, a multilayer coating system is constructed on a substrate. Preferably according to the present invention, the substrate is selected from metal substrates, plastics, glass and ceramics, more particularly selected from metal substrates. The metal substrate mainly includes a substrate comprising or consisting of, for example, iron, aluminum, copper, zinc, magnesium and alloys thereof and steel, which is in any of a variety of forms and compositions. Particularly preferred substrates are steel substrates, especially typical steel substrates used in the automotive industry. Before step 1 of the method of the present invention, the metal substrate can be pretreated in a conventional manner, i.e., for example, cleaned. Suitable plastic substrates are, in principle, substrates comprising or consisting of: (i) polar plastics, such as polycarbonate, polyamide, polystyrene, styrene copolymers, polyesters, polyphenylene oxides and blends of these plastics, (ii) reactive plastics, such as PUR-RIM, SMC, BMC, and (iii) polyolefin substrates of polyethylene and polypropylene types with high rubber content, such as PP-EPDM, and surface-activated polyolefin substrates. Plastics can also be fiber-reinforced, more specifically using carbon fibers and / or metal fibers. Prior to step 1) of the method according to the invention, the plastic substrate can also be pretreated, more particularly by cleaning, to improve the adhesion of the first coating. In addition, substrates containing metal and plastic parts can also be used. Such substrates are, for example, car bodies containing plastic parts.

[0113] Step 1)

[0114] In step 1) of the method, a cured first coating can be produced on the substrate by applying the coating material to the substrate and optionally subsequently curing it.

[0115] The coating of step 1) may be an electrophoretic coating. The first coating is preferably a cured electrocoating with a thickness in the range of 8 μm to 20 μm.

[0116] Step 2)

[0117] The primer material of step 2) is preferably a water-based colored primer material. Suitable water-based colored primer materials can be commercially available, such as from BASF N-3000N6. The primer materials corresponding to each layer of the primer coating can be the same or different. Two or more layers of primer coating can be prepared with the same primer material, and one or more layers of primer coating can be prepared with one or more other primer materials. The primer coating can be cured alone or baked and cured in combination with the varnish coating. In some embodiments of the present invention, the primer coating is cured alone, and the baking temperature (or curing temperature) is 100 to 250°C, preferably 110°C to 160°C, for 10 to 45 minutes; in other embodiments of the present invention, the primer coating is baked and cured in combination with the varnish coating. In step 2), the primer coating is preferably not exposed to a temperature higher than 100°C for more than 1 minute, and it is particularly preferred that it is not exposed to a temperature higher than 100°C at all in step 2). In a specific embodiment of the present invention, a low temperature such as 60 to 80°C flash-drying primer material is used. Each primer coating layer after curing has a layer thickness of more than 4 μm. Preferably, the primer coating layer after curing has a thickness in the range of 12 μm to 18 μm.

[0118] Step 3)

[0119] At least one of the varnish materials in step 3) is a two-component varnish composition of the present invention. In some embodiments of the present invention, the varnish material may also include other different varnish materials, but in order to ensure the performance of the coating, it is preferred to use the two-component varnish composition of the present invention as the top varnish material. Further preferably, the varnish coating of the present invention only includes applying the two-component varnish composition of the present invention to obtain a coating. The varnish coating can be cured alone or baked and cured in combination with the primer coating. In some embodiments of the present invention, the varnish coating is cured alone, and the baking temperature (or curing temperature) is 80°C to 160°C, preferably 110°C to 130°C, for 10 to 45 minutes; in other embodiments of the present invention, the primer coating and the varnish coating are jointly baked and cured, and the baking temperature (or curing temperature) is 110°C to 160°C, for 10 to 45 minutes. In some preferred embodiments of the present invention, the present invention can also achieve low-temperature baking, whether for a single curing or a combined baking and curing process, the baking temperature is preferably 110°C to 130°C. Even if the curing temperature is low, the multilayer coating obtained by the present invention can still have good comprehensive properties.

[0120] After curing, each clearcoat layer has a layer thickness of 15 μm to 80 μm, preferably 20 μm to 65 μm, particularly preferably 30 μm to 60 μm.

[0121] The two-component varnish composition of the present invention can be applied to different coating processes and has wide applicability.

[0122] In another aspect, the present invention also provides a multilayer coating film prepared by the method for forming a multilayer coating film according to the present invention, wherein the obtained multilayer coating film has excellent finished product appearance and high hardness, resistance to petroleum products and water resistance. In some preferred embodiments of the present invention, the multilayer coating film comprises one or two primer coating layers and only one clear coat layer.

[0123] Implementation

[0124] The following embodiments are used to illustrate the present invention in more detail.

[0125] Implementation 1:

[0126] A two-component varnish composition comprising:

[0127] Component I

[0128] A) a (meth)acrylic resin containing a hydroxyl group,

[0129] B) melamine resin,

[0130] C) a polyol ester, which is a reaction product of one or more of castor oil, castor oil monoglyceride, castor oil diglyceride, a primary hydroxyl group-containing polyol, and optionally a polyacid or anhydride;

[0131] Component II

[0132] D) polyisocyanates,

[0133] The varnish coating formed by the two-component varnish composition has a molecular weight between crosslinking points of 300 to 700 g / mol, preferably 350 to 500 g / mol.

[0134] Second implementation scheme:

[0135] A two-component varnish composition according to the first embodiment, wherein:

[0136] The glass transition temperature of the component A is -50°C to 50°C, preferably -45°C to 25°C, and more preferably -40°C to -2°C.

[0137] Implementation 3:

[0138] The two-component varnish composition according to the first or second embodiment, wherein

[0139] The hydroxyl value of the component A is 130 to 220 mg KOH / g, preferably 150 to 200 mg KOH / g.

[0140] Implementation 4:

[0141] A two-component varnish composition according to any one of the first to third embodiments, wherein:

[0142] The hydroxyl value of the component C is 180 to 500 mg KOH / g, preferably 200 to 450 mg KOH / g, and more preferably 240 to 400 mg KOH / g.

[0143] The fifth implementation scheme:

[0144] A two-component varnish composition according to any one of the first to fourth embodiments, wherein

[0145] The weight average molecular weight of the component C is 1000 to 3000 g / mol.

[0146] The sixth implementation scheme:

[0147] A two-component varnish composition according to any one of the first to fifth embodiments, wherein

[0148] The molecular weight distribution PDI of the component C is above 1.5.

[0149] The seventh implementation scheme:

[0150] A two-component varnish composition according to any one of the first to sixth embodiments, wherein

[0151] The primary hydroxyl group-containing polyol is a polyol having 4 or more carbon atoms and containing two or more primary hydroxyl groups.

[0152] The eighth implementation plan:

[0153] A two-component varnish composition according to any one of the first to seventh embodiments, wherein

[0154] The molar equivalent ratio NCO / OH of the isocyanate group of the component D to the total hydroxyl group of the components A and C is 0.8 to 1.5:1, preferably 0.9 to 1.3:1.

[0155] Implementation No. 9:

[0156] A two-component varnish composition according to any one of the first to eighth embodiments, wherein

[0157] Based on 100 parts by weight of the total solid content of the component I, the component C is 5 to 35 parts by weight, and preferably, the component C is 8 to 20 parts by weight.

[0158] The tenth implementation plan:

[0159] A two-component varnish composition according to any one of the first to ninth embodiments, wherein

[0160] Based on 100 parts by weight of the total solid content of the component I, the component B is 1 to 35 parts by weight, preferably, the component B is 5 to 20 parts by weight.

[0161] Implementation 11:

[0162] An article coated with the two-component varnish composition according to any one of the first to tenth embodiments.

[0163] Implementation 12:

[0164] A method for forming a multilayer coating film, comprising:

[0165] 1) optionally producing a cured first coating on a substrate;

[0166] 2) producing at least one primer coating on the coating obtained in step 1) by applying one or more identical or different primer materials;

[0167] 3) producing at least one clearcoat coating on the uppermost basecoat coating by applying one or more clearcoat materials which may be the same or different;

[0168] At least one of the varnish materials is a two-component varnish composition as described in any one of embodiments 1 to 10;

[0169] The primer coating and the clear coating are cured by baking separately or by combined baking. Preferably, the primer coating and the clear coating are cured by combined baking after step 3).

[0170] Implementation 13:

[0171] The method for forming a multilayer coating film according to the twelfth embodiment, wherein

[0172] The baking temperature of the varnish coating is 80°C to 160°C, preferably, the baking temperature of the varnish coating is 110°C to 130°C.

[0173] Implementation 14:

[0174] The method for forming a multilayer coating film according to the eleventh or twelfth embodiment, wherein

[0175] The primer material is a water-based colored primer material.

[0176] Implementation 15:

[0177] A multi-layer coating film produced by the method for forming a multi-layer coating film according to any one of the 11th to 14th embodiments.

[0178] Example

[0179] The present invention will be explained more specifically below with reference to Examples, but it should be understood that the present invention is not limited to these Examples.

[0180] The coating film thickness (coating thickness) in the examples refers to the cured dry film thickness.

[0181] Test method:

[0182] Solid content (%)

[0183] The solids content is determined in accordance with DIN EN ISO 3251 (date: June 2008).

[0184] 1 g of sample is weighed into pre-dried aluminum foil, dried in a drying oven at 125°C for 60 minutes, cooled in a desiccator and then reweighed. The residue relative to the total amount of sample used corresponds to the solid content or non-volatile fraction.

[0185] Solid mass = sample mass × solid content (%).

[0186] Dry film thickness

[0187] The dry film thickness was determined in accordance with DIN EN ISO 2808:2007-05 (date: May 2007), method 12A - magnetic induction meter, using an FMP20 instrument from Helmut-Fischer.

[0188] Acid value and hydroxyl value

[0189] The acid value is determined in accordance with DIN EN ISO 2114 (date: June 2002). The hydroxyl value is determined in accordance with DIN 532402 (date: November 2007).

[0190] Molecular weight

[0191] The number average molecular weight, weight average molecular weight, PDI are determined and calculated according to DIN 556721 (date: August 2007).

[0192] Glass transition temperature (T g )

[0193] The calculation is performed using the method described above in the specification of the present invention.

[0194] Preparation and Synthesis Example of (Meth) Acrylic Resin (A) Containing Hydroxyl Group:

[0195] Synthesis Example 1-6

[0196] Add 60 parts by weight of solvent (Ac-1) to a four-necked flask equipped with a stirring device, a thermometer, a cooling tube and a nitrogen inlet under nitrogen, and heat to 155°C. When the temperature reaches 155°C, add monomer (Am) and 3 parts by weight of polymerization initiator (Ab) dropwise to the flask over 2 hours, wherein the composition and proportion of monomer (Am) are shown in Table 1. Thereafter, the product is aged at 155°C for 3 hours under nitrogen, cooled to room temperature, and diluted with solvent (Ac-2), thereby obtaining an acrylic resin (A) having a solid content of 60%. The characteristic parameters of the obtained acrylic resin (A) are also shown in Table 1.

[0197] Table 1

[0198]

[0199] in,

[0200] St:Styrene

[0201] 2-EHA: 2-ethylhexyl acrylate

[0202] CHMA: Cyclohexyl methacrylate

[0203] MMA: Methyl Methacrylate

[0204] AA: Acrylic acid

[0205] HEMA: Hydroxyethyl Methacrylate

[0206] 4-HBA: Hydroxybutyl acrylate

[0207] Solvent (Ac-1): Butyl acetate

[0208] Solvent (Ac-2): Ethyl 3-ethoxypropionate

[0209] Polymerization initiator (Ab): tert-butyl peroxy(2-ethylhexanoate)

[0210] Preparation Synthesis Example of Polyol Ester (C):

[0211] Synthesis Example 7-8

[0212] Castor oil (C1), a polyol containing a primary hydroxyl group (C2), and a catalyst tetrabutyl titanate (the amount added is 0.5 wt % of the mass of castor oil) in the molar ratio shown in Table 2 are added to a four-necked flask equipped with a heater, a stirrer, a thermometer, a reflux condenser, and a water separator. The mixture is poured into the four-necked flask, heated to 220° C. under nitrogen, kept warm for 3 hours, and then gradually cooled to 150° C. to obtain polyol esters (C-1 to C-2) of the present invention.

[0213] Synthesis Example 9-11

[0214] Castor oil (C1) and a polyol (C2) containing a primary hydroxyl group in the molar ratio shown in Table 2 are added to a four-necked flask equipped with a heater, a stirrer, a thermometer, a reflux condenser and a water separator, and a polyacid or anhydride (C3) in a molar ratio of 2:1 between alcohol and acid is added. The temperature is raised to 220° C. at a rate of 20° C. / hour. After being kept warm for 3 hours, when the acid value is about 10 mg KOH / g, the temperature is lowered to 180° C. and vacuumed. When the acid value is less than or equal to 1.5 mg KOH / g, the polyol esters (C-3 to C-5) of the present invention are obtained.

[0215] Synthesis example 12

[0216] Castor oil (C1) was used as a comparative example (C-6).

[0217] Table 2 also shows the parameters of the obtained polyol esters (C-1 to C-5) and castor oil (C-6).

[0218] Table 2

[0219]

[0220] in,

[0221] Castor oil (C1): manufactured by Ito Oil Chemical Co., Ltd., refined castor oil, weight average molecular weight: 1510 g / mol

[0222] Polyols containing primary hydroxyl groups (C2):

[0223] Polyol containing primary hydroxyl group (C2-1): pentaerythritol, weight average molecular weight: 136 g / mol

[0224] Polyol containing primary hydroxyl group (C2-2): trimethylolpropane, weight average molecular weight: 134 g / mol

[0225] Polyol containing primary hydroxyl group (C2-3): glycerol, weight average molecular weight: 92 g / mol

[0226] Polyol containing primary hydroxyl group (C2-4): sorbitol, weight average molecular weight: 182 g / mol

[0227] Polyacid or anhydride (C3):

[0228] Polyacid or anhydride (C3-1): Phthalic anhydride, weight average molecular weight: 148 g / mol

[0229] Polyacid or anhydride (C3-2): Hexahydrophthalic anhydride, weight average molecular weight: 154 g / mol

[0230] Preparation of two-component clearcoat compositions

[0231] Examples 1-11, Comparative Examples 1-4

[0232] The hydroxyl-containing (meth) acrylic resin (A) (solid content of 60%) and polyol ester (C) obtained in the above-mentioned preparation synthesis examples 1-12 and other raw materials (melamine (B), curing catalyst (E), rheology control agent (F)) given in Table 3 were mixed using a rotary blade stirrer according to the mixing ratio given in Table 3 to obtain component I; polyisocyanate (D) was prepared according to the amount given in Table 3 to obtain component II, thereby obtaining a two-component varnish composition (CC-1 to CC-15).

[0233] Component I and component II of each of CC-1 to CC-15 were mixed and the mixture was stirred uniformly, the viscosity of the mixture was adjusted to 25 seconds using Ford cup No. 4 at 20°C by adding ethyl acetate, and then various test plates were prepared according to the following conditions.

[0234] Preparation of PP board with molecular weight (MC) between crosslinking points

[0235] A test piece with a width of 10 mm and a length of 70 mm was prepared and the dynamic viscoelasticity measurement (storage elastic modulus E) was carried out under the following conditions. MC was measured by formula (II):

[0236] Equipment: Dynamic viscoelasticity measurement equipment RSA3;

[0237] Measurement mode: Non-resonance forced vibration method

[0238] Heating rate: 3.0℃ / min

[0239] Measuring interval: 12 / min

[0240] Frequency: 1.0Hz

[0241] Temperature range: -50~200℃

[0242] Formula (II): MC = (293 × 1.05) / (log ((E / 3), 10) -7 )

[0243] The evaluation criteria are as follows:

[0244] 〇: 350~500g / mol

[0245] △: 300~349 or 500~700g / mol

[0246] ×: 299 or less or 701 or more

[0247] Preparation of test panels for performance and appearance

[0248] A cationic electrodeposition coating (product name "CathoGuard 800", produced by BASF Coatings) was applied to a zinc phosphate treated mild steel plate by electrostatic deposition and baked at 175°C for 25 minutes to obtain an electrodeposition coated plate (abbreviated as "electrodeposition plate") having a dry film thickness of 20 μm.

[0249] Then, a first primer material (aqueous gray intermediate coating, produced by BASF Coatings) was applied to the electrodeposited plate at a temperature of 25° C. and a relative humidity of 75% using a rotary atomization type cup coater (product name “Metal Cup G1-COPES Cup”, produced by ABB) in such a manner that the dry film thickness was 15 μm. Then, the resulting plate was allowed to stand at room temperature for 5 minutes. Thereafter, a second primer material (lava red water-based glitter base paint, produced by BASF Coatings) was applied in such a manner that the dry film thickness was 12 μm. Then, the plate was allowed to stand at room temperature for 5 minutes and flashed at 80° C. for 10 minutes. After cooling to 25° C., a clear coating (one of CC-1 to CC-15 was selected, respectively) was applied to provide a dry film thickness of 45 μm. After this coating, the plate was allowed to stand at room temperature for 10 minutes and then horizontally baked at 140° C. for 30 minutes to obtain a test plate having a multilayer coating film (Examples 1-11, Comparative Examples 1-4).

[0250] Change the primer material, spraying process and baking temperature:

[0251] A cationic electrodeposition coating (product name "CathoGuard 800", produced by BASF Coatings) was applied to a zinc phosphate treated mild steel plate by electrostatic deposition and baked at 175°C for 25 minutes to obtain an electrodeposition coated plate (abbreviated as "electrodeposition plate") having a dry film thickness of 20 μm.

[0252] A rotary atomizing cup coater (product name "Metal Cup G1-COPES Cup", produced by ABB) was used to apply the first primer material (aqueous white mid-coat, produced by BASF Coatings) to the electrodeposited plate at a temperature of 25°C and a relative humidity of 75% in a manner such that the dry film thickness was 15 μm. Then, the resulting plate was allowed to stand at room temperature for 10 minutes and then horizontally baked at 140°C for 30 minutes. Thereafter, a second primer material (bright white water-based monochromatic primer, produced by BASF Coatings) was applied in a manner such that the dry film thickness was 12 μm. Then, the plate was allowed to stand for 10 minutes and then horizontally baked at 140°C for 30 minutes. After cooling to 25°C, a clear coat (one of CC-1, CC-7, CC-13 or CC-15, respectively) was applied to provide a dry film thickness of 45 μm. After the coating, the plate was left to stand at room temperature for 10 minutes and then horizontally baked at 110° C. for 30 minutes, thereby obtaining test plates of the multilayer coating films corresponding to Examples 12 and 13 and Comparative Examples 5 and 6.

[0253] The obtained test plates were subjected to the following coating film performance tests. The results are shown in Table 3.

[0254] hardness:

[0255] The hardness is evaluated according to the pencil hardness, and the hardness refers to the GB / T 6739-2006 standard.

[0256] The evaluation criteria are as follows:

[0257] 0:HB and above

[0258] △: B

[0259] ×: 2B and below

[0260] Appearance (LW, SW):

[0261] The appearance of dried and cured varnish is evaluated by its surface texture, which is measured by a BYK wave scanner. The surface texture is a mixture of various textures, ranging from very fine to very rough. BYK wave scans dually measure the surface texture at different scale levels, which are divided into six categories, identified by wavelength (Du, Wa, Wb, Wc, Wd, We). Based on these measurement data, the equipment calculates LW, SW, which represents the appearance grade of the paint. The lower the LW and SW, the better the appearance performance. LW is mainly determined by the varnish layer, while SW is determined not only by the varnish layer but also by the substrate and primer.

[0262] The LW evaluation criteria are as follows:

[0263] 0:0 <LW<5

[0264] △: 5≤LW<10

[0265] ×: LW≥10

[0266] The SW evaluation criteria are as follows:

[0267] 0:5≤SW<25

[0268] △: 3 <SW<5,25≤SW≤30

[0269] ×: SW≤3, SW>30

[0270] Resistance to petroleum products:

[0271] Preparation of E10 petroleum alcohol solution:

[0272] Mix No. 93 gasoline and ethanol in a mass ratio of 9 to 1, and the mixed solution is the E10 test solution.

[0273] Pour a sufficient amount of E10 solution into the glass tank and adjust the test temperature to 40℃±2℃. Immerse 2 / 3 of the test plate in E10. Use an appropriate support to immerse the test plate in a vertical position for 1 hour. The immersed test plate should be at least 30mm away from the inner wall of the tank, and the test plates should be 30mm apart. To reduce the evaporation of E10 solution, the container should be covered.

[0274] After reaching the specified immersion time, take out the test plate, wipe the surface with filter paper to remove the residual liquid, and immediately use a colorimeter to test the change in L of the test plate coating before and after immersion.

[0275] Evaluation criteria for resistance to petroleum products:

[0276] ○: ΔL≤0.3Good

[0277] △:0.3<ΔL≤0.8There is a slight discoloration, but it does not affect the use

[0278] ×: ΔL>0.8 has serious discoloration and cannot be used

[0279] Water resistance:

[0280] The test plate was immersed in warm water at 40°C for 240 hours and then taken out and dried at 20°C for 12 hours. The multilayer coating on the test plate was cut into a grid pattern with a cutter to reach the substrate, and 100 checkerboard holes of 2 mm x 2 mm in size were formed. Then, a scotch tape was attached to the surface, and the remaining state of the checkerboard coating after the tape was quickly peeled off at 20°C was examined.

[0281] Water resistance evaluation criteria:

[0282] 0: 100 checkerboard eye coatings remain, and no missing edges occur

[0283] △: 100 checkerboard eye coatings remain, but the edges are missing

[0284] ×: The number of remaining checkered paint films is less than 99

[0285]

[0286]

[0287] in:

[0288] Melamine resin (B): CYMEL manufactured by Allnex TM 202, solid content = 100%

[0289] Polyisocyanate (D-1): DURANATE manufactured by Asahikasei Co., Ltd. TM TPA-100, solid content = 100%, NCO% = 23.1

[0290] Polyisocyanate (D-2): DURANATE manufactured by Asahikasei Co., Ltd. TM TKA-100, solid content = 100%, NCO% = 21.7

[0291] Curing catalyst (E):

[0292] E-1: King Industries NACURE 5076

[0293] E-2: CYCAT 4045 made by allnex

[0294] E-3: King Industries NACURE 4167

[0295] E-4: DURAPHOS BAP made by Solvay

[0296] Rheology control agent (F):

[0297] In a four-necked flask equipped with a stirring device, a thermometer, a cooling tube and a nitrogen inlet, 60 parts by mass of a solvent (Ac-1) was added under nitrogen, and the temperature was raised to 155° C. When the temperature reached 155° C., 34 parts by mass of butyl acrylate, 21 parts by mass of hydroxyethyl acrylate, 39 parts by mass of styrene, 2 parts by mass of methacrylic acid, and 2 parts by mass of a polymerization initiator of di-tert-butyl hydroperoxide were dropwise added to the flask over 2 hours. Thereafter, the product was aged at 155° C. for 3 hours under nitrogen, cooled to room temperature, and diluted with a solvent to obtain a rheology control agent (F-1) having a solid content of 60%.

[0298] It can be seen from Table 3 that only the two-component varnish composition that meets the requirements of the present invention can form a paint film having excellent finished product appearance and high hardness, resistance to petroleum products and water resistance. In some preferred embodiments, even if low-temperature baking and curing are performed, the two-component varnish composition of the present invention can also obtain a paint film with good comprehensive properties.

Claims

1. A two-component varnish composition comprising: Component I A) a (meth)acrylic resin containing a hydroxyl group, B) melamine resin, C) a polyol ester, which is a reaction product of one or more of castor oil, castor oil monoglyceride, castor oil diglyceride, a primary hydroxyl group-containing polyol, and optionally a polyacid or anhydride; Component II D) polyisocyanates, The varnish coating formed by the two-component varnish composition has a molecular weight between crosslinking points of 300 to 700 g / mol. It is characterized in that The glass transition temperature of component A is -45°C to -2°C; the hydroxyl value of component C is 240 to 400 mg KOH / g; and based on 100 parts by weight of the total solid content of component I, component C is 5 to 35 parts by weight.

2. The two-component varnish composition according to claim 1, characterized in that The varnish coating formed by the two-component varnish composition has a molecular weight between crosslinking points of 350 to 500 g / mol.

3. The two-component varnish composition according to claim 1 or 2, characterized in that The glass transition temperature of the component A is -40°C to -2°C.

4. The two-component varnish composition according to claim 1 or 2, characterized in that The hydroxyl value of the component A is 130 to 220 mg KOH / g.

5. The two-component varnish composition according to claim 4, characterized in that The hydroxyl value of the component A is 150 to 200 mg KOH / g.

6. The two-component varnish composition according to claim 1 or 2, characterized in that: The weight average molecular weight of the component C is 1000 to 3000 g / mol.

7. The two-component varnish composition according to claim 1 or 2, characterized in that: The molecular weight distribution PDI of the component C is above 1.

5.

8. The two-component varnish composition according to claim 1 or 2, characterized in that: The primary hydroxyl group-containing polyol is a polyol having 4 or more carbon atoms and containing two or more primary hydroxyl groups.

9. The two-component varnish composition according to claim 1 or 2, characterized in that: The molar equivalent ratio NCO / OH of the isocyanate group of the component D to the total hydroxyl group of the components A and C is 0.8-1.5:

1.

10. The two-component varnish composition according to claim 9, characterized in that The molar equivalent ratio NCO / OH of the isocyanate group of the component D to the total hydroxyl group of the components A and C is 0.9-1.3:

1.

11. The two-component varnish composition according to claim 1 or 2, characterized in that: Based on 100 parts by weight of the total solid content of the component I, the component C is 8 to 20 parts by weight.

12. The two-component varnish composition according to claim 1 or 2, characterized in that: Based on 100 parts by weight of the total solid content of the component I, the component B is 1 to 35 parts by weight.

13. The two-component varnish composition according to claim 12, characterized in that Based on 100 parts by weight of the total solid content of the component I, the component B is 5 to 20 parts by weight.

14. Articles coated with a two-component clearcoat composition according to any one of claims 1 to 13.

15. A method for forming a multilayer coating film, comprising: 1) optionally producing a cured first coating on a substrate; 2) producing at least one primer coating on the coating obtained in step 1) by applying one or more identical or different primer materials; 3) producing at least one clearcoat coating on the uppermost basecoat coating by applying one or more clearcoat materials which may be the same or different; At least one of the varnish materials is a two-component varnish composition according to any one of claims 1 to 13; The primer coating and the clear coating are cured by baking separately or by combined baking.

16. The method for forming a multilayer coating film according to claim 15, characterized in that: The primer coating and the clear varnish coating are jointly baked and cured after step 3).

17. The method for forming a multilayer coating film according to claim 15 or 16, characterized in that: The baking temperature of the varnish coating is 80°C to 160°C.

18. The method for forming a multilayer coating film according to claim 17, characterized in that: The baking temperature of the varnish coating is 110°C to 130°C.

19. The method for forming a multilayer coating film according to claim 15 or 16, characterized in that: The primer material is a water-based colored primer material.

20. A multi-layer coating film obtained by the method for forming a multi-layer coating film according to any one of claims 15 to 19.