A catalytic material for producing hydrogen by electrolysis of water and its preparation method and application

By developing the electrolytic water reaction of ABxOOH catalytic material and glucose, the problem of low hydrogen production efficiency of direct decomposition of water in solar cells is solved, and the production of high-efficiency hydrogen production and high-value-added product formic acid is achieved, which reduces the cost of hydrogen production.

CN117403262BActive Publication Date: 2024-11-01CHINA AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311312119.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2024-11-01
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

The current solar cells have low efficiency in direct decomposition of water to produce hydrogen, and the economic value of oxygen is not high. At present, the research mainly focuses on the selectivity of oxidation products, but no in-depth analysis of hydrogen production efficiency has been made, resulting in the need to improve the hydrogen production efficiency. .

Method used

Developed a catalytic material chemical composition ABxOOH, A is any one of Fe, Co and Ni, and B is any one of Mn, Fe, Ni, Cu and Zn, and prepared by electrochemical deposition reaction and oxidation treatment. Combined with the biomass-based raw material such as glucose as an oxidation substrate and the catalytic material is carried out to undergo an electrolytic reaction.

Benefits of technology

The efficient hydrogen production of electrolytic water is achieved, the solar hydrogen production efficiency exceeds 30%, and glucose is efficiently converted into a high value-added product formic acid, with a yield of more than 80%, reducing the cost per kilogram of hydrogen produced by solar cells to decompose water to produce hydrogen by about 4.6. Dollar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117403262B_ABST
    Figure CN117403262B_ABST
Patent Text Reader

Abstract

The present invention discloses a catalytic material for producing hydrogen by electrolysis of water, and a preparation method and application thereof, which belongs to the field of solar hydrogen production. The present invention provides a catalytic material for producing hydrogen by electrolysis of water, and its chemical composition is AB x OOH; 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar hydrogen production, and particularly relates to a catalytic material for electrolytic water hydrogen production, a preparation method thereof, and an application thereof. Background Art

[0002] Solar hydrogen production is a very promising technical solution to solve energy and environmental problems. Currently, the main ways of solar hydrogen production include photocatalytic water splitting for hydrogen production, photoelectrochemical water splitting for hydrogen production, and direct water splitting for hydrogen production by solar cells, etc. Among them, direct water splitting for hydrogen production by solar cells relatively has a higher conversion efficiency of solar hydrogen production, which can exceed 20%. However, the overpotential of the oxidation reaction of water splitting is relatively high, resulting in a low efficiency of solar hydrogen production, and the economic value of the generated oxygen is not high. In view of this problem, a hydrogen production scheme of coupling glycerol, chitosan, 5-methylfurfural oxidation with water reduction has been proposed in the prior art to improve the hydrogen production efficiency. However, the current research mainly focuses on the selectivity problem of oxidation products, and no systematic and in-depth analysis has been carried out on the hydrogen production efficiency. Therefore, the hydrogen production efficiency still needs to be improved. Therefore, it is very necessary to find a suitable oxidation substrate and develop a high-efficiency catalytic material matching it. Summary of the Invention

[0003] The present invention provides a catalytic material for electrolytic water hydrogen production, a preparation method thereof, and an application thereof.

[0004] The present invention first provides a catalytic material for electrolytic water hydrogen production, and its chemical composition is AB x OOH; 0 < x < 0.1. Wherein, A is any one of Fe, Co, and Ni, and B is any one of Mn, Fe, Ni, Cu, and Zn.

[0005] In the above catalytic material, 0.03 ≤ x ≤ 0.09, preferably, x = 0.05;

[0006] A is Co, and B is Cu, Fe, or Ni; preferably, B is Cu.

[0007] The present invention also provides a preparation method of the above catalytic material, including the following steps: weighing A source and B source according to the stoichiometric ratio and dissolving them in water to obtain an electrolyte solution; then carrying out an electrochemical deposition reaction, and oxidizing the anode after the reaction to obtain the catalytic material.

[0008] In the above preparation method, the A source is a nitrate and / or sulfate of the corresponding metal element; specifically, it can be cobalt nitrate;

[0009] The B source is a nitrate of the corresponding metal element; specifically, it can be copper nitrate, manganese nitrate, iron nitrate, nickel nitrate, or zinc nitrate;

[0010] In the electrolyte, the concentration of A is 0.05-0.3 mol / L, and can be specifically 0.1 mol / L.

[0011] In the above preparation method, the electrochemical deposition reaction adopts a three-electrode system, the cathode is a platinum sheet, platinum carbon or carbon paper; the anode is foamed nickel, foamed iron or carbon cloth; the reference electrode is Ag / AgCl or a saturated calomel electrode.

[0012] In the above preparation method, the electrochemical deposition reaction adopts a constant voltage mode; a voltage of -0.8 to -1.2 V relative to the reference electrode is applied to the anode; specifically, it can be -1.0 V; the electrodeposition time is 1 to 10 minutes; specifically, it can be 5 minutes.

[0013] In the above-mentioned preparation method, the oxidation is carried out by using the anode electrode after the electrochemical deposition reaction as the anode, potassium hydroxide solution as the electrolyte, and applying a constant voltage to the anode to carry out the oxidation reaction;

[0014] Preferably, the oxidation adopts a three-electrode system; a voltage of 0.1 to 0.5 V relative to the reference electrode is applied to the anode, specifically 0.3 V; the oxidation time is 1 to 10 min, specifically 5 min.

[0015] The concentration of the potassium hydroxide solution is 0.1-2 mol / L, specifically 1 mol / L.

[0016] Finally, the present invention also provides the use of the above catalytic material in any of the following:

[0017] (1) Application in hydrogen production by water electrolysis;

[0018] (2) Application of oxidation of alcohols, sugars or aldehydes in the production of hydrogen by combined electrolysis of water.

[0019] In the above application, the sugar is glucose;

[0020] The oxidation of alcohols, sugars or aldehydes produces formic acid.

[0021] In the above applications, the power source used is solar power;

[0022] Preferably, the power source is a solar cell.

[0023] The present invention utilizes biomass-based raw materials, such as glucose, as an oxidation substrate, and couples with the reduced water reaction and cooperates with high-efficiency catalytic materials. The efficiency of water electrolysis is as high as 94.2%, and the efficiency of solar hydrogen production exceeds 30%. At the same time, glucose can be efficiently converted into a high-value-added product, formic acid, with a yield of more than 80%. The technical solution of the present invention can reduce the cost of solar cells to decompose water to produce hydrogen by about US$4.6 per kilogram. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Preparation of electrocatalytic material CoCu for electrochemical deposition x Physical pictures before and after electrochemical oxidation during OOH (x = 0.05); Figure 1 In the figure, a is the physical picture before electrochemical oxidation, and b is the physical picture after electrochemical oxidation.

[0025] Figure 2 The electrocatalytic material CoCu prepared in Example 1 x X-ray diffraction patterns of OOH (x=0.05) and CoOOH; the blue dotted line is the diffraction peak of the base nickel foam.

[0026] Figure 3 The electrocatalytic material CoCu prepared in Example 1 x Field emission scanning electron microscopy of OOH (x=0.05).

[0027] Figure 4 The electrocatalytic material CoCu prepared in Example 1 x Composition analysis of OOH (x = 0.05); Figure 4 a is the X-ray selected area energy spectrum analysis; b is the Co element distribution; c is the Cu element analysis; d is the EDX spectrum; and e is the element composition ratio.

[0028] Figure 5 The electrocatalytic material CoCu prepared in Example 1 x X-ray surface photoelectron spectroscopy of OOH (x=0.05).

[0029] Figure 6 Diagram of the apparatus for glucose oxidation testing.

[0030] Figure 7 This is the voltage-current curve of glucose oxidation.

[0031] Figure 8 This is the current-time curve of the oxidation of 20 mmol / L glucose in 1 mol / L KOH aqueous solution at 0.3 V.

[0032] Fig. 9 This is the NMR 1H spectrum of the product obtained by oxidation of 20 mmol / L glucose in 1 mol / L KOH aqueous solution at 0.3V.

[0033] Fig.10 The effect of Cu doping concentration on formate yield.

[0034] Fig.11 Schematic diagram of the setup for driving a single electrolytic cell to oxidize glucose and produce hydrogen for a solar cell.

[0035] Fig.12 The performance of commercial solar cells InGaP / GaAs / Ge (5mm×5mm, HGSC-A50B) at 1 sun (green line) and 14 suns (blue line) intensities, as well as the current-voltage curves of water electrolysis in 1 (orange line) and 2 (red) electrolytic cells.

[0036] Fig.13 Schematic diagram of a solar cell driving two electrolytic cells to oxidize glucose and reduce water to produce hydrogen under certain external voltage conditions.

[0037] Fig.14 is the hydrogen production efficiency at different temperatures. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.

[0039] The experimental methods in the following examples are all conventional methods unless otherwise specified.

[0040] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0041] Example 1: Electrocatalytic Material CoCu x Preparation of OOH (x = 0.05)

[0042] The electrocatalytic material CoCu of the present invention x OOH (x = 0.05) is synthesized by electrochemical deposition reaction at room temperature. The specific method is as follows: Take Co(NO3)2·6H2O as raw material and prepare 30mL of 0.1mol / L Co aqueous solution. After stirring evenly, add Cu(NO3)2·3H2O, the concentration of Cu is 5mol% of Co, and stir evenly to obtain the electrolyte required for electrochemical deposition. The electrochemical deposition adopts a three-electrode system, the anode is nickel foam (thickness 0.5mm, area 2cm×3cm), the cathode is a platinum sheet (area 1cm×2cm), and the reference electrode is Ag / AgCl. The electrodeposition adopts the constant voltage mode of the electrochemical workstation, and a voltage of -1.0V relative to the reference electrode Ag / AgCl is applied to the anode, and the electrodeposition time is 5 minutes. After the electrodeposition is completed, rinse with deionized water to obtain a green electrode, which can be seen Figure 1 a in.

[0043] The obtained electrode was oxidized in an electrolyte of 1 mol / L KOH, with the electrode as the anode, the platinum sheet as the cathode, and Ag / AgCl as the reference electrode. A voltage of 0.3 V relative to the reference electrode Ag / AgCl was applied to the anode in the constant voltage mode of the electrochemical workstation. The oxidation time was 5 minutes, and after the oxidation was completed, it was rinsed with deionized water to obtain a black electrode, which is the electrocatalytic material CoCu x OOH (x = 0.05), the figure is shown in Figure 1 b in.

[0044] The electrocatalytic material CoCu prepared by the present invention x OOH (x = 0.05) has the same crystal structure as oxyhydroxide CoOOH (see Figure 2 ), Cu doping does not change its phase composition. Electrocatalytic material CoCu x The morphology of OOH (x = 0.05) is a flake structure. Figure 3 The EDX spectrum shows that the Cu and Co elements are evenly distributed, and the ratio of Cu to Co measured by the spectrum is 5.32% (see Figure 4 ). After the sample was dissolved in hydrochloric acid, the ratio of Cu to Co in two repeated samples was measured by inductively coupled plasma spectroscopy to be 6.3% and 6.6%. Surface photoelectron spectroscopy proved the presence of hydroxyl groups in the material, the valence state of Co was a mixed state of +2 and +3, and Cu was +2 (see Figure 5 ).

[0045] Among them, the preparation method of CoOOH is as follows: Co(NO3)2·6H2O is used as a raw material, and 30mL of a 0.1mol / L Co aqueous solution is prepared. Stir evenly to obtain the electrolyte required for electrochemical deposition. The electrochemical deposition adopts a three-electrode system, the anode is nickel foam (thickness 0.5mm, area 2cm×3cm), the cathode is a platinum sheet (area 1cm×2cm), and the reference electrode is Ag / AgCl. The electrochemical deposition adopts the constant voltage mode of the electrochemical workstation, and a voltage of -1.0V relative to the reference electrode Ag / AgCl is applied to the anode, and the electroplating time is 5 minutes. After the electroplating is completed, rinse with deionized water.

[0046] The obtained electrode was oxidized in an electrolyte of 1 mol / L KOH, with the electrode as the anode, the platinum sheet as the cathode, and Ag / AgCl as the reference electrode. A voltage of 0.3 V relative to the reference electrode Ag / AgCl was applied to the anode through the constant voltage mode of the electrochemical workstation. The oxidation time was 5 minutes. After the oxidation was completed, it was rinsed with deionized water to obtain a black electrode, which was the electrocatalytic material CoOOH.

[0047] Table 1 CoCu measured by inductively coupled plasma emission spectroscopy x Content of Co and Cu in OOH (x = 0.05)

[0048]

[0049] Example 2, Glucose Oxidation Test

[0050] A three-electrode system was used, with the anode being the electrode material prepared in Example 1, the cathode being a platinum sheet (area 1 cm×2 cm), and the reference electrode being Ag / AgCl. The test device was an H-type electrochemical cell with an anion exchange membrane, the exchange membrane separating the cathode and anode cells, each containing 20 mL of a 1 mol / L KOH aqueous solution, and 72 mg of glucose added to the anode cell. The anode cell contained the prepared electrode material and reference electrode, and the cathode cell contained a platinum sheet electrode. The device was as follows: Figure 6 The voltage-current relationship test of glucose oxidation was carried out in the linear scanning mode of the electrochemical workstation with a scanning speed of 2mV / s ( Figure 7 The test of complete oxidation of glucose to formic acid was conducted in constant voltage mode, with a voltage of 0.3 V applied to the anode relative to the reference electrode until the current decayed to nearly 0 mA ( Figure 8 ). The product was determined by NMR to be formate (8.38 ppm) with a yield of 80.9% ( Fig. 9 The formate yield was quantitatively calculated by adding the internal standard pivalic acid, and its peak position was 1.03 ppm. Among them, the doping concentration of Cu has an important influence on the formate yield, and about 5% is the optimal ( Fig.10 , the preparation method of the anode used in the figure is the same as that in Example 1, except that the concentration of the added Cu is different, and the concentration of the added Cu is 1 mol%, 3 mol%, 5 mol%, 7 mol%, and 9 mol% respectively). In addition, doping other elements in CoOOH also has similar functions, but the yields are different, see Table 2. The preparation method of each electrocatalytic material used in Table 2 is the same as that in Example 1, except that the added elements are different, and the specific added substances are Mn(NO3)2·4H2O, Fe(NO3)3·9H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Zn(NO3)2·6H2O.

[0051] Table 2 Formate yields of electrocatalytic materials obtained by doping CoOOH with 5 mol% of different elements in 1 M KOH aqueous solution for oxidation of glucose

[0052] Doping elements Formate yield (%) none 50 Mn 58 Fe 63 Ni 60 Cu 80 Zn 32

[0053] Example 3: Testing of hydrogen production by solar cell driven glucose oxidation and water reduction

[0054] The solar cell is used to drive glucose oxidation and water reduction. The solar cell used in this embodiment is a commercial InGaP / GaAs / Ge solar cell (5mm×5mm, HGSC-A50B, Shenzhen Huashang.SuperiorIndustrial Co., Ltd), which has a solar cell efficiency of 29.8% under one sun. The material for reducing water to produce hydrogen at the cathode is Ni4Mo, and its preparation method is described in the literature (ChemElectroChem 1, 1138-1144 (2014)). The material for oxidizing glucose at the anode is CoCu x OOH (x = 0.05). The test device is a single electrolytic cell, and the electrolyte is an aqueous solution of 1 mol / L KOH and 0.02 mol / L glucose. Under the test conditions of one sun, when driving an electrolytic cell to reduce water and oxidize glucose, the solar cell is directly connected to the cathode and anode of the electrolytic cell, as shown in the schematic diagram. Fig.11 As shown, the hydrogen production efficiency is 16.7% ( Fig.12 ), the hydrogen production efficiency is 25.9% when driving two electrolytic cells ( Fig.12 When the condenser is used to concentrate light into 14 suns, the open circuit voltage and short circuit current of the solar cell are improved, and the cell efficiency is also increased to 34.9% ( Fig.12 ). At this time, the hydrogen production efficiency of driving an electrolytic cell is 17.2% ( Fig.12 ), and when driving two electrolytic cells, the voltage of the solar cell is not enough to support the large current after concentration, so the hydrogen production efficiency is only 10.6% ( Fig.12 ), resulting in the solar cell failing to achieve maximum efficiency. Therefore, during the experiment, an external voltage of 0.3 V was applied through an electrochemical workstation (which can also be replaced by other power sources), such as Fig.13 At this time, the hydrogen production efficiency can reach 30% at room temperature, and heating can further improve the hydrogen production efficiency, as shown in Fig.14 As shown. The hydrogen production efficiency at 80°C can reach 32.9%. In addition, multiple solar cells can be used to drive more electrolytic cells to fully utilize the efficiency of solar cells, or solar cells with required open circuit voltage can be customized as needed.

[0055] Example 4: Solar cell driven glucose oxidation and water reduction to produce hydrogen

[0056] According to the analysis of some recent studies, assuming an efficiency of 28% for converting solar energy to hydrogen, the levelized cost of green hydrogen production from traditional water electrolysis to produce hydrogen and oxygen can reach US$5.90 per kilogram or less (Sustainable Energy Fuels 5, 1085-1094 (2021)).

[0057]

[0058] According to formula (1), 49 kg of potassium formate can be produced for every 1 kg of H2 produced (calculated at an 80% yield). At the same time, 15 kg of glucose is consumed. According to the estimated market price of bulk chemicals in China in April 2023, the price of industrial glucose is about $0.45-0.65 / kg; the price of KOH is about $0.95-1.35 / kg; and the price of potassium formate is about $1.05-1.25 / kg. According to the average market prices of the above raw materials and products (glucose: $0.55 / kg, KOH: $1.15 / kg, potassium formate: $1.15 / kg, and the yield is 80%), it can be calculated according to formula (1) that the material of the present invention is used to oxidize glucose and produce hydrogen at the same time, and an additional profit of about $4.63 / kg can be obtained for every 1 kg of H2 produced. Therefore, the production cost of green hydrogen is expected to drop below $2.0 / kg, which is comparable to or even lower than the cost of traditional methane reforming hydrogen production.

Claims

1. A method for preparing a catalytic material for producing hydrogen by electrolysis of water, comprising the following steps: weighing a source A and a source B and dissolving them in water to obtain an electrolyte; then performing an electrochemical deposition reaction, and after the reaction, oxidizing the anode to obtain the catalytic material; The corresponding metal element of the A source is Co; The metal element corresponding to the B source is Mn, Fe, Ni or Cu; In the electrolyte, the concentration of A is 0.1 mol / L; when the metal element corresponding to the B source is Cu, the molar concentration of B is 3%, 5%, 7% or 9% of the molar concentration of A; when the metal element corresponding to the B source is Mn, Fe or Ni, the molar concentration of B is 5% of the molar concentration of A; The electrochemical deposition reaction adopts a three-electrode system, wherein the cathode is a platinum sheet, platinum carbon or carbon paper; the anode is foamed nickel, foamed iron or carbon cloth; and the reference electrode is Ag / AgCl or a saturated calomel electrode; The electrochemical deposition reaction adopts a constant voltage mode; a voltage of -0.8 to -1.2 V relative to the reference electrode is applied to the anode; The oxidation is carried out by using the anode electrode after the electrochemical deposition reaction as the anode and potassium hydroxide solution as the electrolyte, and applying a constant voltage to the anode to carry out the oxidation reaction; The oxidation adopts a three-electrode system; a voltage of 0.1 to 0.5 V relative to the reference electrode is applied to the anode.

2. The preparation method according to claim 1, characterized in that: The A source is a nitrate and / or sulfate of the corresponding metal element; The B source is the nitrate of the corresponding metal element.

3. The preparation method according to claim 1 or 2, characterized in that: The electrodeposition time is 1 to 10 minutes.

4. The preparation method according to claim 1 or 2, characterized in that: The oxidation time is 1 to 10 minutes.

5. The catalytic material prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the catalytic material according to claim 5 in any of the following; (1) Application in hydrogen production by water electrolysis; (2) Application of oxidation of alcohols, sugars or aldehydes in the production of hydrogen by combined electrolysis of water.

7. The use according to claim 6, characterized in that: The sugar is glucose; The oxidation of alcohols, sugars or aldehydes produces formic acid.

8. The use according to claim 6 or 7, characterized in that: The power source used in the application is solar-generated electricity.

9. The use according to claim 8, characterized in that: The power source used in the application is solar cells.