A non-invasive electroencephalogram signal acquisition electrode, preparation method and application thereof

By adding Sn annealed ITO powder and sodium alginate hydrogel to In2O3 colloid, an elastic spherical EEG signal acquisition electrode was prepared, which solved the high cost and adhesion problems of conductive paste and achieved high efficiency. Convenient EEG signal acquisition improves the comfort and conductivity of the test.

CN117430830BActive Publication Date: 2024-11-26NANJING UNIV OF POSTS & TELECOMM
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311333825.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-11-26
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

In the existing EEG signal acquisition technology, the preparation method of conductive paste has problems such as high cost, complex equipment, unecottonous and easy adhesion after use, and it is difficult to find a balance between conductivity and comfort, and lacks alternative solutions.

Method used

By adding Sn annealed ITO powder into In2O3 colloids, combined with sodium alginate hydrogel, an elastic spherical non-invasive EEG signal acquisition electrode was prepared, and the electrode was deformed by the solidification process of calcium chloride solution. Ability to avoid adhesions and improve conductivity.

Benefits of technology

It realizes low-cost, environmentally friendly, non-adhesive EEG signal acquisition electrodes, simplifies the testing process, improves patient comfort and operation convenience, and ensures the excellent conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117430830B_ABST
    Figure CN117430830B_ABST
Patent Text Reader

Abstract

The invention discloses a non-invasive electroencephalogram (EEG) signal acquisition electrode, a preparation method and application thereof, and belongs to the field of EEG signal acquisition. Acetylacetone is used as a complexing agent to prepare an indium nitrate sol, and an ethanol solution of tin tetrachloride is used to perform a sol-gel reaction to prepare a precursor indium tin oxide sol with a Tyndall effect. The precursor sol is annealed and ground to obtain a high-concentration semiconductor indium tin oxide powder. The powder is mixed with sodium alginate gel to prepare a hydrogel precursor solution, which is injected into a mold, and a curing liquid solution is added to solidify to obtain a collection electrode with good formability. It can be directly placed in the hole of the electrode sheet before EEG measurement, and can be taken out and discarded after use. There is no need for the filling step of the traditional conductive paste and the instrument cleaning step after information acquisition, and there is no sticky feeling, which improves the comfort of the patient and the convenience of operation of medical staff. The electrode preparation process is simple, safe, low cost, and has a wide source of raw materials. It is simple to operate and has good and stable conductive properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electroencephalogram signal acquisition, and specifically relates to a method for preparing a non-invasive electroencephalogram signal acquisition electrode. Background Art

[0002] Electroencephalogram (EEG) is a neuroimaging electrophysiological monitoring technology that records brain electrical activity non-invasively. It records the brain's electrical activity signals by placing multiple electrodes on the scalp and can measure the brain's neural electrical activity state. The preparation method of the collection electrodes used in this test is one of the important research contents of EEG testing.

[0003] Indium tin oxide (ITO) is an N-type oxide semiconductor. There are various methods for preparing indium tin oxide, such as magnetron sputtering, vacuum evaporation, chemical vapor deposition, sol-gel method, etc. However, other preparation methods require complex equipment, high material costs, uncontrollable, and environmentally unfriendly. ITO prepared by the sol-gel method of inorganic salts can prepare semiconductor materials with excellent conductive effects without these.

[0004] The most commonly used conductive material in EEG experiments is conductive paste. Conductive paste is water-based and contains a small amount of salt. The salt concentration can affect the conductivity of the gel, where a higher salt concentration can produce a better quality signal. However, too high a salt concentration may also cause discomfort to the subject, so it is difficult for conductive paste to achieve the best of both worlds in terms of conductivity and comfort. In addition, conductive paste is easy to adhere to the subject's scalp, hair and test equipment before and after use, and the subject needs to clean the head and test equipment after each test.

[0005] At present, there has been no detailed research on the preparation method of the collection electrode specifically used to replace the conductive paste. Therefore, it is necessary to develop a simple, efficient and low-cost preparation method for the EEG signal collection electrode and use this electrode in the field of EEG signal collection. Summary of the invention

[0006] In view of the technical problems existing in the prior art, the present invention provides a non-invasive EEG signal acquisition electrode, a preparation method and application thereof. ITO powder formed by adding Sn to In2O3 colloid after annealing can effectively play the role of a semiconductor, increase the carrier concentration in sodium alginate, improve the electrical properties of the material, and obtain better electrical transport performance. The curing process of the calcium chloride solution ensures that the prepared electrode can be elastically deformed within a certain range, and ensures that the electrode can adaptively change its shape, so as to fit the tested part of the head more closely. The conductive paste that can replace the traditional EEG signal test is soft and elastic, can be formed independently, and will not adhere to the human body or the test instrument. While ensuring excellent conductivity, it reduces the subsequent processing work of the test, making the overall test process convenient and fast.

[0007] The technical solution adopted by the present invention is:

[0008] A non-invasive EEG signal collection electrode, which is in the shape of an elastic sphere or other shapes suitable for filling an EEG signal collection electrode sheet, is about 7.5 cm in size, and is an ITO-conductive hydrogel obtained by curing a sodium alginate hydrogel doped with indium tin oxide powder.

[0009] The present invention also provides the use of the non-invasive electroencephalogram signal acquisition electrode as a spherical electrode in an electroencephalogram signal acquisition system.

[0010] The preparation method of the above non-invasive EEG signal acquisition electrode comprises the following steps:

[0011] (1) Using acetylacetone as a solvent and a complexing agent, adding a trivalent indium source under heating conditions, and stirring until the reactant presents a brown-yellow colloid with no obvious impurities, thereby obtaining a trivalent indium source sol;

[0012] The indium source is indium nitrate; the heating temperature is 70-80° C., and the stirring time is 3 hours.

[0013] (2) Add a tetravalent tin source into ethanol, stir evenly to obtain a solution, and set aside; the tetravalent tin source is tin tetrachloride.

[0014] (3) slowly dripping the solution obtained in step (2) into the trivalent indium source sol obtained in step (1), and generating a sol-gel reaction under heating and stirring conditions to obtain a precursor indium tin oxide sol, annealing the sol to obtain a high-concentration semiconductor indium tin oxide powder, grinding the powder for later use;

[0015] Heat the temperature to 50-60°C, control the dropping time within 10 minutes, and continue stirring for 20 minutes after the dropping process is completed until the system is uniform;

[0016] The annealing treatment is carried out in an argon atmosphere, with the temperature being raised to a maximum temperature of 500° C. within 35 minutes and maintained for 2 hours.

[0017] The "high concentration" of the high concentration semiconductor indium tin oxide powder is 5-3 times the conventional concentration, and the "conventional concentration" is recorded in ([1] Song Weiming et al. "Sol-gel synthesis of indium tin oxide nanocrystals." Journal of Ningxia University: Natural Science Edition 21.4 (2000): 3.).

[0018] (4) adding a sodium alginate hydrogel to the indium tin oxide powder obtained in step (3) under heating and stirring conditions to obtain a mixed hydrogel doped with ITO powder;

[0019] The doping ratio of ITO powder is 1%-8%, preferably 2%-4%, and more preferably 2%.

[0020] (5) After the hydrogel obtained in step (4) is initially cooled and formed, it is poured into a spherical mold, and a calcium ion aqueous solution is added to solidify it to obtain a gel electrode with a certain shape;

[0021] The solid-to-liquid ratio of the calcium ion aqueous solution is 1:15-1:25, preferably 1:20.

[0022] Beneficial effects: Compared with the prior art, the advantages of the present invention are:

[0023] (1) The present invention uses acetylacetone as a solvent and a complexing agent to prepare an indium nitrate sol, and performs a sol-gel reaction with an ethanol solution of tin tetrachloride to prepare a precursor indium tin oxide sol with a Tyndall effect using an inorganic salt as a substrate. The preparation method is low-cost and easy to operate. After annealing and grinding the precursor sol, a high-concentration semiconductor indium tin oxide powder is obtained. The powder is mixed with sodium alginate gel to prepare a hydrogel precursor solution, which is injected into a mold and solidified by adding a solidifying liquid solution to obtain a collection electrode with good formability. When used, it can be directly placed in the hole of the electrode sheet and can be taken out and discarded after use. There is no need for the traditional conductive paste filling step and the instrument cleaning step after information collection, and there is no sticky feeling, which improves the comfort of patients and the convenience of operation of medical staff.

[0024] (2) In the reaction system, acetylacetone, as a solvent for indium nitrate and a complexing agent for the reaction, can fully promote the sol-gel reaction; tin tetrachloride uses ethanol as a solvent, which makes tin tetrachloride easily soluble in acetylacetone and can promote ion exchange reactions between substances. The prepared indium tin oxide material is used as a semiconductor conductive material to ensure the stable conductivity of the EEG signal collection electrode and has good conductive properties. The preparation process is simple, safe, low-cost, and has a wide range of raw material sources, making it suitable for expanded production.

[0025] (3) Adding sodium alginate hydrogel to indium tin oxide powder can make the EEG signal collection electrode softer and easier to deform, and easier to fit tightly to the subject's head without contaminating the subject and the instrument, so as to obtain more accurate EEG signals. At the same time, it ensures good biocompatibility and is safe and environmentally friendly during the test process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope (SEM) image of the ITO powder of Example 1 of the present invention. It can be seen from the image that the size and distribution of the ground ITO powder are very uniform, which is convenient for subsequent mixing with the hydrogel;

[0027] Figure 2This is a scanning electron microscope (SEM) image of sodium alginate doped with 2% high-concentration ITO powder according to Example 1 of the present invention. It can be seen from the image that the powder is evenly distributed in the hydrogel, and the uniform incorporation of homogeneous powder can make the conductivity of the sodium alginate electrode more stable; the black holes seen in the image are caused by the drying of the mixed hydrogel, and the pores caused by the drying are visible through the glass slide under the sample, resulting in a black shadow;

[0028] Figure 3 The XRD patterns of the high-concentration and normal-concentration ITO powders after annealing in Example 1 of the present invention show that the high-concentration ITO powder has high crystallinity, large particle size, and high content of effective semiconductor components, and is more suitable for being incorporated into electrodes as a semiconductor material than the low-concentration powder.

[0029] Figure 4 The X-ray diffraction XRD patterns of sodium alginate doped with 2% high-concentration ITO powder in Example 1 and sodium alginate doped with 4% high-concentration ITO powder in Example 2 of the present invention are shown in Table 1. Generally, the diffraction peaks of ITO are as follows: Figure 3 As shown, sodium alginate has diffraction peaks at 14.0° and 23.0°, but no corresponding diffraction peaks are observed in the XRD spectrum of the mixed hydrogel, which may further prove that the uniform mixing of ITO and sodium alginate during the gel mixing process prevents the crystallization behavior of ITO and sodium alginate, thereby forming a mixed hydrogel;

[0030] Figure 5 This is a graph of the electrode RI test of Example 1 of the present invention. It can be seen from the graph that while the test current I is constantly changing, the resistance of the electrode remains stable, which ensures the stability and accuracy of the brain waves collected during the test;

[0031] FIG6 is an EEG test electroencephalogram of the hydrogel electrode mixed with different concentrations of ITO powder in Example 1 of the present invention. It can be seen from the figure that its waveform and amplitude are Figure 7 The waveform of the conductive paste test is very similar, which ensures its substitutability for conductive paste in the test;

[0032] (a) The curing liquid concentration is 1:20, and 2% ITO powder is added;

[0033] (b) The curing liquid concentration is 1:20, and 4% ITO powder is added;

[0034] (c) The curing liquid concentration is 1:25, and 2% ITO powder is added;

[0035] Figure 7 This is an EEG test brain wave diagram of the comparative example of the present invention;

[0036] Figure 8It is a statistical diagram of the conduction points and lines of electrodes with different doping concentrations in Example 1 of the present invention;

[0037] Fig. 9 It is a statistical diagram of conduction points and lines of electrodes after being cured with different curing liquid concentrations according to Example 2 of the present invention. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the examples of the present invention, rather than all other embodiments of the present invention. All other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.

[0039] Comparative test of EEG signal acquisition application using traditional conductive paste

[0040] (1) After the test system is turned on, select Weishi Medical, then select "New Medical Record", "Regular Sampling", then enter the sampler's information and click Confirm to enter the EEG acquisition page.

[0041] (2) Adjust the initial parameters of EEG acquisition: select 19 leads for "Leads" and select None for "High and low pass filters";

[0042] (3) Put the test EEG cap on the subject, adjust the electrode to the center, and fill the conductive paste between the EEG cap and the subject's scalp through the holes on the electrode sheet to ensure that the electrode resistance at the test interface is all reduced to below 30k0hms.

[0043] (4) After the test, rinse the conductive paste stuck to the EEG cap with clean water for 20 minutes. After washing, squeeze out the water and store it in a ventilated place. Clean the conductive paste on the subject's head in time to avoid air drying and difficulty in cleaning or allergic reaction.

[0044] (5) After filtering and ICA preprocessing, the EEG signals detected above are preliminarily processed to obtain effective EEG signals. Figure 7 .

[0045] Example 1 Effect of adding different amounts of ITO powder on the preparation of non-invasive gel electrodes

[0046] In this embodiment, non-invasive EEG signal acquisition electrodes with different concentration ratios of ITO powder to sodium alginate hydrogel were prepared, and the effect of adding different amounts of ITO powder on the preparation of non-invasive gel electrodes was investigated, specifically 1%, 2%, 4%, and 8%.

[0047] 1. Preparation of non-invasive EEG signal acquisition electrodes, the steps are as follows:

[0048] (1) Weigh 5.523 g of indium nitrate and add it to 27 ml of acetylacetone. Place the mixture in a round-bottom flask in an oil bath at 70-80°C and heat with stirring for 3 h. After sufficient stirring, the sol becomes brown-yellow and has no obvious impurities.

[0049] (2) Weigh 1.43 g of tin tetrachloride and add it to 3 ml of ethanol. Stir magnetically at room temperature for 1 h. After thorough stirring, the solution becomes transparent and colorless with no obvious impurities.

[0050] (3) Use a dropper to slowly drip the tin tetrachloride solution into the indium nitrate sol. The solution needs to be completely dripped in within 10 minutes. At the same time, the temperature is kept at 50℃-60℃ with magnetic stirring for 20 minutes. The precursor indium tin oxide sol is successfully prepared and has a Tyndall effect.

[0051] (4) The stirred sol is aged for 1-2 days, and a dropper is used to fill more than half of a 50mm*15mm*7.5mm quartz boat. The sol is annealed in an argon atmosphere for 35 minutes at a maximum temperature of 500°C for 2 hours to obtain a high-concentration semiconductor indium tin oxide powder. The X-ray diffraction (XRD) spectrum of the high-concentration semiconductor indium tin oxide powder and the normal concentration indium tin oxide powder is shown in FIG. Figure 3 The indium tin oxide powder obtained by annealing was ground, and the degree of grinding uniformity was determined by scanning electron microscope SEM images. Figure 1 The "high concentration" of the high concentration semiconductor indium tin oxide powder is 5-3 times the conventional concentration. "Conventional concentration semiconductor indium tin oxide powder" is recorded in ([1] Song Weiming et al. "Sol-gel synthesis of indium tin oxide nanocrystals." Journal of Ningxia University: Natural Science Edition 21.4 (2000): 3.).

[0052] (5) Weigh 38 ml of pure water and heat it in an oil bath to 50°C-55°C. Weigh 2 g of sodium alginate and slowly add it. Stir continuously while adding to ensure that the hydrogel is uniform and free of large lumps. Continue to heat the oil bath at the above temperature while magnetically stirring for 7 hours. After obtaining a uniform hydrogel, let it stand for 5 hours.

[0053] (6) Weigh 0.5 g of calcium chloride and add it to 9.5 ml of deionized water (solidification solution concentration 1:20). Stir magnetically at room temperature for 3 h. After sufficient stirring, the solution becomes transparent and colorless with no obvious impurities.

[0054] (7) 0.06g, 0.12g, 0.24g, and 0.48g of the ground indium tin oxide powder in step (4) were mixed with an equal amount of 6g of sodium alginate gel in step (5) by magnetic stirring for 6h to obtain mixed hydrogel precursor solutions with doping concentrations of 1%, 2%, 4%, and 8%, respectively. The uniformity of the representative sample, i.e., the mixed hydrogel with a doping ratio of 2%, was obtained by scanning electron microscopy (SEM) images. Figure 2; Then observe the composition of 2% and 4% gel by X-ray diffraction XRD pattern, see Figure 4 Sample 1 and Sample 2 were mixed evenly and placed in a refrigerator for cooling and standing for 8 hours. They were then taken out and injected into a spherical silicone mold with a diameter of 7 mm using a dropper to shape the sample. The above is the method for making hydrogel electrodes with different doping concentrations.

[0055] (8) Use the mold to fill more than 24 spherical electrodes, put them into the refrigerator to cool and set for 20 minutes, take them out and put them into the calcium chloride solution in (6) to solidify for 20 minutes. The non-invasive gel electrodes with different doping concentrations are completed. The RI curve of the electrode with a doping concentration of 2% is shown in Figure 5 .

[0056] 2. Conduct EEG signal acquisition application test on the above gel electrodes:

[0057] The application test of EEG signal acquisition is the same as that of the control example, except that in step (3), the spherical electrodes need to be filled in the holes of the electrode sheet before the EEG cap is put on, and the process of injecting conductive paste is cancelled; and the two-step cleaning process in step (4) is cancelled. It is only necessary to discard the used spherical electrodes and ventilate the EEG cap. The EEG signals after preprocessing are collected by electrodes with concentrations of 2% and 4%, as shown in Figures 6 (a) and (b). The resistance conduction of electrodes with different doping concentrations is obtained by Weiss Medical Software, and a statistical chart is drawn, as shown in Figure 6 (b). Figure 8 As can be seen from the figure, 2% and 4% ITO powder incorporation concentrations can ensure that the resistance of the test interface is completely reduced to below 30k0hms, and all test electrodes are turned on; 1% and 8% ITO powder incorporation concentrations are too low or too high, and cannot play the role of semiconductor conductivity in the hydrogel, and the test electrodes cannot all be reduced to below 30k0hms, and the brain wave collection test cannot be performed. Therefore, the collection electrode of the present invention has good formability, does not require a filling step and a cleaning step after information collection, does not produce a sticky feeling, improves the adaptability of patients and the convenience of operation of medical staff, and has good material electrical properties.

[0058] Example 2 Effect of different curing liquid concentrations on the preparation of non-invasive gel electrodes

[0059] The case where the doping concentration in Example 1 is 2% was selected to investigate the effect of curing with different concentrations of curing liquid on the performance of the non-invasive gel electrode. The preparation method is the same as that in Example 1, except that:

[0060] In step (6), 0.5 g of calcium chloride was weighed and added to 7 ml, 9.5 ml and 12 ml of deionized water respectively, and magnetic stirring was carried out at room temperature for 3 h. After sufficient stirring, the solution was transparent and colorless without obvious impurities, and three different concentrations of solidified liquids with mass ratios of 1:15, 1:20 and 1:25 were obtained. Different solidified electrodes were obtained through the same process as in Example 1.

[0061] The application test of EEG signal acquisition is the same as in Example 1. The electrodes cured with the curing liquid concentration of 1:20 and 1:25 collect the pre-processed EEG signals. The resistance conduction of the electrodes with different curing liquid concentrations is obtained by Weisi Medical Software, and a statistical chart is drawn. Fig. 9 As can be seen from the figure, the solidified electrodes with solidifying liquid concentrations of 1:15, 1:20, and 1:25 can ensure that the resistance of the test interface is all reduced below 30k0hms, and all the test electrodes are turned on. However, the electrodes solidified at 1:15 and 1:25 are obviously less conductive than the electrodes solidified at 1:20. Because the concentration of the solidifying liquid is too low or too high, the hydrogel electrode has insufficient support or is over-hardened, and cannot fit the scalp at the test site well. The test electrode cannot exert its conductive properties to the best of its ability, and cannot perform more accurate EEG acquisition tests.

[0062] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a non-invasive electroencephalogram signal acquisition electrode, It is characterized in that Here are the steps: (1) Using acetylacetone as a solvent and a complexing agent, adding a trivalent indium source under heating conditions, and stirring until the reactant presents a brown-yellow colloid with no obvious impurities, thereby obtaining a trivalent indium source sol; (2) Add a tetravalent tin source to ethanol, stir evenly to obtain a solution, and set aside; (3) slowly dripping the solution obtained in step (2) into the trivalent indium source sol obtained in step (1), and generating a sol-gel reaction under heating and stirring conditions to obtain a precursor indium tin oxide sol, annealing the sol to obtain a high-concentration semiconductor indium tin oxide powder with a concentration 5-3 times that of conventional powder, grinding the powder for later use; (4) adding the indium tin oxide powder obtained in step (3) to the sodium alginate hydrogel under heating and stirring conditions to obtain a mixed hydrogel doped with ITO powder; the doping ratio of the ITO powder is 2%-4%; (5) After the hydrogel obtained in step (4) is initially cooled and formed, it is poured into a mold and solidified by adding a calcium ion aqueous solution to obtain a gel electrode with a certain shape; the solid-liquid ratio of the calcium ion aqueous solution is 1:15~1:

25.

2. A method for preparing a non-invasive electroencephalogram signal acquisition electrode according to claim 1, It is characterized in that In step (1), the indium source is indium nitrate; the heating temperature is 70-80° C., and the stirring time is 3 h. In step (2), the tetravalent tin source is tin tetrachloride.

3. A method for preparing a non-invasive electroencephalogram signal acquisition electrode according to claim 1, It is characterized in that In step (3), the heating temperature is 50°C-60°C, the dropping time is controlled within 10 minutes, and after the dropping process is completed, stirring is continued until the system is uniform; The annealing treatment is carried out in an argon atmosphere, with the temperature being raised to a maximum temperature of 500° C. within 35 minutes and maintained for 2 hours.

4. A method for preparing a non-invasive electroencephalogram signal acquisition electrode according to claim 1, It is characterized in that In step (5), the solid-to-liquid ratio of the calcium ion aqueous solution is 1:

20.

5. A method for preparing a non-invasive electroencephalogram signal acquisition electrode according to claim 1, It is characterized in that In step (4), the doping ratio of ITO powder is 2%.

6. A non-invasive EEG signal acquisition electrode prepared by the method for preparing a non-invasive EEG signal acquisition electrode according to claim 1.

7. Use of the non-invasive EEG signal acquisition electrode according to claim 6 as a spherical electrode in preparing an EEG signal acquisition system.

Citation Information

Patent Citations

  • Method for preparing ITO film with high conductivity

    CN101337773A

  • Preparation method of micro conductive hydrogel

    CN105153459A

  • Flexible strain sensor based on conductive hydrogel and preparation method and application thereof

    CN116183071A