A laser cladding repair process for spiral shafts in the food industry

Laser cladding technology is used to repair two base layers and one wear-resistant layer on the spiral shaft, which solves the problems of insufficient hardness and poor repair quality caused by wear and corrosion of the spiral shaft, achieving a higher service life and Increased hardness.

CN117448811BActive Publication Date: 2024-10-18SHANDONG LAIYAN LASER TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311478352.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2024-10-18
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

Spiral shafts in the food industry are seriously damaged due to long-term extrusion, wear and corrosion during operation. The existing repair process is complex and difficult to effectively repair the damaged parts, which affects the service life.

Method used

Using laser cladding technology, the parts to be repaired on the spiral shaft are first pre-processed, and the spiral shaft is clamped for laser cladding repair with two layers of base layer and one layer of wear-resistant layer. The size and hardness are ensured through initial processing and final processing of the grinder.

Benefits of technology

The service life of the spiral shaft is increased, the hardness is significantly improved after repair, the operation is simple, the uneven size is filled and the wear resistance is high, avoiding waste of resources and complex mechanical processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117448811B_ABST
    Figure CN117448811B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of laser cladding technology, and specifically to a laser cladding repair process for a spiral shaft in the food industry, comprising the following steps: S1, pre-treating the part of the spiral shaft to be repaired; S2, clamping the spiral shaft in a way of two ends facing each other, and laser cladding two layers of primer layers on the part of the spiral shaft to be repaired; S3, pre-processing the end surface of the primer layer of the spiral shaft; S4, laser cladding a layer of wear-resistant layer on the surface of the primer layer; S5, final processing of the end surface of the wear-resistant layer of the spiral shaft. The present invention is simple to operate to repair the damaged part of the spiral shaft, and the damaged part has a strong hardness after repair, thereby increasing the service life of the spiral shaft.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser cladding, and in particular to a laser cladding repair process for a spiral shaft in the food industry. Background Art

[0002] The screw shaft is a part of the screw conveyor. The screw shaft is made of steel pipe, which has high strength, light weight and is easy to connect. The steel pipe is provided with main rotation blades and counter-rotation blades. A gap section is provided between the main rotation blades and the counter-rotation blades. The position of the gap section is opposite to the position of the discharge port of the screw conveyor; the transmission shaft is connected to the gear motor of the screw conveyor through a coupling. Its main function is to push the material to achieve the purpose of transportation. The screw shaft can help the screw conveyor to transport various materials horizontally, inclined or vertically.

[0003] During the operation of the spiral shaft in the food industry, the end face of the spiral shaft and the slurry-facing surface are squeezed, worn and corroded for a long time, and the machine body is seriously damaged. When the machine body is seriously worn and corroded, it cannot continue to operate. Replacing the entire spiral shaft with a new one will waste resources and be time-consuming.

[0004] CN202210439563.5 discloses a screw helical surface repair process, which includes placing the screw on a support device, using a spray welding device to melt and spray alloy on the surface of the screw helical surface, and after spraying, checking the size of the helical surface. When the size of the helical surface is larger than the original design size, the screw is removed and taken to a grinder for size restoration. After the size restoration is completed, the helical surface of the screw is polished. After the polishing is completed and the repair is completed, a rust inhibitor is applied to the screw helical surface. This patent uses mechanical treatments such as grinding and polishing, and the operation is relatively complicated.

[0005] CN201711491364.4 discloses a laser cladding process for a wear-resistant layer of a spiral shaft, and the specific steps are as follows: S1: removal of the wear-resistant layer, S2: surface cleaning, S3: end processing, S4: clamping cladding, S5: inspection, S6: surface processing. The present invention performs four layers of cladding on the blades of the spiral shaft, and increases the service life of the spiral shaft by using a layer of base layer and three layers of wear-resistant layers, thereby increasing practical performance. This patent uses a layer of base layer + three layers of wear-resistant layers for laser cladding repair, and it is difficult to fully transition between the base layer and the wear-resistant layer, which affects the repair hardness. Summary of the invention

[0006] In view of the technical problems that damaged parts of the spiral shaft are difficult to repair and the repair quality is poor, the present invention provides a laser cladding repair process for spiral shafts in the food industry. The repair operation is simple, and the damaged parts have greater hardness after repair, thereby increasing the service life of the spiral shaft.

[0007] The present invention provides a food industry spiral shaft laser cladding repair process, comprising the following steps:

[0008] S1. Pre-treat the part of the spiral shaft to be repaired;

[0009] S2. Clamp the spiral shaft with both ends facing each other, and laser clad two layers of base layer on the part to be repaired of the spiral shaft;

[0010] S3. Preliminary processing of the end surface of the bottom layer of the spiral shaft;

[0011] S4, laser cladding a wear-resistant layer on the surface of the base layer;

[0012] S5. Final processing of the end surface of the wear-resistant layer of the spiral shaft.

[0013] Furthermore, in step S1, the method for pre-treating the part of the spiral shaft to be repaired comprises the following steps:

[0014] S11. Use a handheld grinder and polisher to remove the rusted area of ​​the spiral shaft to be repaired;

[0015] S12. Remove oil stains from the surface of the part of the spiral shaft to be repaired;

[0016] S13. Use laser to ablate the corroded area to make it smooth.

[0017] Furthermore, in step S13, the process parameters for laser ablating the corroded area to be smooth are: laser power of 1300 W, spot size of 3 mm, robot running fitting speed of 120 cm / min, protective gas of Ar, gas flow rate of 8 L / min, program running trajectory along the spiral direction, and the laser head at an angle of 75° to the end face.

[0018] Furthermore, in step S2, the method of laser cladding two layers of primer layers is to first laser clad the first iron-based alloy powder to the part to be repaired of the spiral shaft to form a first primer layer, and then laser clad the second iron-based alloy powder to the surface of the first primer layer to form a second primer layer.

[0019] Furthermore, in step S2, the first iron-based alloy powder includes the following chemical components in weight percentage: Cr18.4%, Ni11.49%, Nb1.03%, Mo2.42%, and the balance is Fe and unavoidable impurities; the powder particle size of the first iron-based alloy is 270-400 mesh, and the average hardness is 25-35HRC.

[0020] Furthermore, in step S2, the second iron-based alloy powder includes the following chemical components in weight percentage: Cr14.59%, Ni 0.48%, Mn 0.72%, Mo 0.036%, W 4.51%, and the remainder is Fe and inevitable impurities; the particle size of the second iron-based alloy powder is 270-400 mesh, and the average hardness is 40-50HRC.

[0021] Furthermore, in step S2, the laser cladding process parameters of the two layers of base layer are: laser power of 2800 W, spot size of 3 mm, robot running fitting speed of 90 cm / min, protective gas of Ar, gas flow rate of 8 L / min, program running trajectory along the spiral direction, the laser head and the end face are at an angle of 75°, and the powder feeding rate is 2.0 r / min.

[0022] Furthermore, in step S3, the method for initially processing the end surface of the bottom layer of the spiral shaft is to grind the end surface of the spiral shaft flat by a grinder and measure the size to ensure that it is qualified.

[0023] Further, in step S4, a wear-resistant layer is laser-clad on the surface of the base layer by laser cladding the mixed powder to the surface of the base layer to form a wear-resistant layer, the mixed powder includes a third iron-based alloy powder and WC powder, the third iron-based alloy powder includes the following components in weight percentage: Cr 14.6%, Ni 0.48%, Mo 0.034%, Mn 0.73%, W5.61%, and the balance is Fe and inevitable impurities; the third iron-based alloy powder has a particle size of 270-400 meshes and an average hardness of 55-60HRC; the amount of WC powder is 6.5% of the weight of the third iron-based alloy powder; the process parameters of the laser cladding of the wear-resistant layer are: laser power of 3200W, spot size of 3mm, robot running fitting speed of 90cm / min, protective gas of Ar, gas flow rate of 8L / min, program running trajectory along the spiral direction, the laser head and the end face are at an angle of 75°, and the powder feeding rate is 2.5r / min.

[0024] Furthermore, in step S4, the method for final processing of the end surface is to grind the wear-resistant layer of the end surface of the spiral shaft flat by a grinder and measure the size of the finished product.

[0025] The beneficial effects of the present invention are as follows: the present invention sequentially laser-clads two layers of primer and one layer of wear-resistant layer on the part to be repaired of the spiral shaft. The first primer is mainly used to fill the size of the severely corroded part of the spiral shaft. Since the filling part is uneven and has a large slope, the material of the first primer is selected from powders with low hardness and easy fusion to achieve the purpose of large-size repair; the second primer is mainly used for the transition between the first primer and the surface wear-resistant layer, so a material with relatively high hardness and slightly wear-resistant components is used. The ratio of the wear-resistant components can meet both the wear-resistant performance and the difficulty of grinding by the grinder, so that the middle transition layer can fill a certain size and have a certain wear-resistant effect without cracking. The hardness of the cladding layer increases successively, the cladding thickness is relatively consistent, and it has a strong hardness after repair, which increases the service life of the spiral shaft. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 It is a process flow chart of a specific implementation mode of the present invention.

[0028] Figure 2 This is a physical picture of a damaged spiral shaft to be repaired according to a specific implementation method of the present invention.

[0029] Figure 3 This is a physical picture of the damaged spiral shaft after two layers of primer are applied according to a specific embodiment of the present invention.

[0030] Figure 4 This is a physical picture of the finished product of the repaired spiral shaft according to a specific implementation method of the present invention. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] Example 1

[0033] like Figure 1 As shown, the present invention provides a laser cladding repair process for spiral shafts in the food industry, and the specific process steps are as follows:

[0034] Step 1: Removal of rusted area: Use a handheld grinder to remove the rusted area of ​​the spiral shaft;

[0035] Step 2: Surface pretreatment before cladding: Remove the oil stains on the surface of the spiral shaft to be clad, and use laser to ablate the severely corroded area to make it smooth. The process parameters of laser treatment are: laser power is 1300W, spot size is 3mm, robot running speed is 120cm / min, protective gas is Ar, gas flow rate is 8L / min, program running trajectory is along the spiral direction, and the laser head is at an angle of 75° to the end face. Figure 2 , showing a damaged spiral shaft to be repaired;

[0036] Step 3: Clamping cladding: Tighten the spiral shaft by the method of two ends facing each other, calculate the parameters such as pitch, fitting speed, powder feeding amount and laser power, and perform two size bottom filling on the defective area of ​​the spiral shaft. The specific method is: first, the first iron-based alloy powder is laser clad to the part to be repaired of the spiral shaft to form a first bottom layer, and then the second iron-based alloy powder is laser clad to the surface of the first bottom layer to form a second bottom layer. The first iron-based alloy powder includes the following chemical compositions by weight percentage: Cr18.4%, Ni11.49%, Nb1.03%, Mo2.42%, and the remainder is Fe and unavoidable impurities; the powder particle size of the first iron-based alloy is 270-400 mesh, and the hardness of the first bottom layer is detected to be 34HRC; the second iron-based alloy powder includes the following chemical compositions by weight percentage: Cr14.59%, Ni0.48%, Mn0.72%, Mo0.036%, W 4.51%, the balance is Fe and unavoidable impurities; the particle size of the second iron-based alloy powder is 270-400 mesh, and the hardness of the second base layer is increased to 48HRC; the laser cladding process parameters of the two base layers are: laser power is 2800W, spot size is 3mm, robot running fitting speed is 90cm / min, protective gas is Ar, gas flow rate is 8L / min, program running trajectory is along the spiral direction, the laser head is at an angle of 75° to the end face, and the powder feeding rate is 2.0r / min, such as Figure 3 The figure shows the damaged spiral shaft after two layers of primer.

[0037] Step 4: Preliminary processing of the end surface: Grind the end surface of the bottom layer of the spiral shaft by a grinder and measure the size;

[0038] Step 5: Clamping cladding: According to the finished product size on the drawing, confirm the relevant laser cladding process parameters, complete the processing of the wear-resistant layer on the surface of the spiral shaft end surface, and reserve more than 50 wires on one side of the cladding wear-resistant layer to ensure grinding by a grinder. The laser cladding wear-resistant layer method is to laser clad the mixed powder to the surface of the base layer to form a wear-resistant layer. The mixed powder includes a third iron-based alloy powder and WC powder. The third iron-based alloy powder includes the following weight percentage components: Cr 14.6%, Ni 0.48%, Mo0.034%, Mn 0.73%, W 5.61%, the balance is Fe and unavoidable impurities; the particle size of the third iron-based alloy powder is 270-400 mesh, and the average hardness is 55-60HRC; the amount of WC powder is 6.5% of the weight of the third iron-based alloy powder; the process parameters of laser cladding of the wear-resistant layer are: laser power is 3200W, spot size is 3mm, robot running fitting speed is 90cm / min, protective gas is Ar, gas flow rate is 8L / min, program running trajectory is along the spiral direction, the laser head is at an angle of 75° with the end face, and the powder feeding rate is 2.5r / min;

[0039] Step 6: End surface final processing: Grind the wear-resistant layer of the end surface of the spiral shaft by a grinder, and measure the finished product size according to the drawing, such as Figure 4 , showing the actual picture of the finished product of the repaired spiral shaft;

[0040] Step 7: Inspection: Measure the hardness and size of the end face of the spiral shaft. After testing, the hardness of the end face of the repaired part is: the highest is 60.7HRC, the lowest is 55.5HRC, and the average hardness is 57.4HRC.

[0041] Comparative Example 1

[0042] Comparative Example 1: The composition of the second iron-based alloy powder in the second base layer of Example 1 is changed, as shown in Table 1, and the spiral shaft is repaired without changing the laser cladding process and the thickness of the cladding layer.

[0043] Table 1 Comparative Example 1 Second Base Layer Second Iron-Based Alloy Powder Composition Design

[0044]

[0045] It can be seen from Table 1 that when the composition of the second iron-based alloy powder in the second base layer is changed, the average hardness of the surface of the second base layer is reduced, indicating that the composition of the second iron-based alloy powder of the present invention has an improving effect on the wear resistance hardness.

[0046] Comparative Example 2

[0047] The difference between Example 2 and Example 1 is that Example 2 does not contain a second base layer. The average hardness of the end face of the spiral shaft after repair in Example 2 is 45.3HRC, which means that the second base layer can fill a certain size as an intermediate transition layer and also have a certain wear resistance improvement effect.

[0048] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A laser cladding repair process for spiral shafts in the food industry, characterized in that: The steps include: S1. Pre-treat the part of the spiral shaft to be repaired; S2. Clamp the spiral shaft with both ends facing each other, and laser clad two layers of base layer on the part to be repaired of the spiral shaft; S3. Preliminary processing of the end surface of the bottom layer of the spiral shaft; S4, laser cladding a wear-resistant layer on the surface of the base layer; S5. Final processing of the end surface of the wear-resistant layer of the spiral shaft; In step S2, the method of laser cladding two layers of primer layers is as follows: first, laser cladding the first iron-based alloy powder to the part to be repaired of the spiral shaft to form a first primer layer, and then laser cladding the second iron-based alloy powder to the surface of the first primer layer to form a second primer layer; the first iron-based alloy powder includes the following chemical components in weight percentage: Cr 18.4%, Ni 11.49%, Nb 1.03%, Mo 2.42%, and the balance is Fe and unavoidable impurities; the powder particle size of the first iron-based alloy is 270-400 mesh, and the average hardness is 25-35HRC; the second iron-based alloy powder includes the following chemical components in weight percentage: Cr 14.59%, Ni 0.48%, Mn 0.72%, Mo 0.036%, W 4.51%, and the balance is Fe and unavoidable impurities; the particle size of the second iron-based alloy powder is 270-400 mesh, and the average hardness is 40-50HRC; In step S4, a wear-resistant layer is laser-clad on the surface of the base layer. The method is to laser-clad the mixed powder to the surface of the base layer to form a wear-resistant layer. The mixed powder includes a third iron-based alloy powder and WC powder. The third iron-based alloy powder includes the following components in weight percentage: Cr 14.6%, Ni 0.48%, Mo 0.034%, Mn 0.73%, W 5.61%, and the balance is Fe and inevitable impurities; the third iron-based alloy powder has a particle size of 270~400 mesh and an average hardness of 55~60HRC.

2. A food industry spiral shaft laser cladding repair process as claimed in claim 1, characterized in that: In step S1, the method for pre-treating the part of the spiral shaft to be repaired comprises the following steps: S11. Use a handheld grinder and polisher to remove the rusted area of ​​the spiral shaft to be repaired; S12. Remove oil stains from the surface of the part of the spiral shaft to be repaired; S13. Use laser to ablate the corroded area to make it smooth.

3. A food industry spiral shaft laser cladding repair process as claimed in claim 2, characterized in that: In step S13, the process parameters for laser ablating the corrosion area to be flat are: laser power of 1300 W, spot size of 3 mm, robot running fitting speed of 120 cm / min, protective gas of Ar, gas flow rate of 8 L / min, program running trajectory along the spiral direction, and the laser head at an angle of 75° to the end face.

4. The laser cladding repair process for spiral shafts in the food industry as claimed in claim 1, characterized in that: In step S2, the laser cladding process parameters of the two layers of base layer are: laser power is 2800 W, spot size is 3 mm, robot running fitting speed is 90 cm / min, protective gas is Ar, gas flow rate is 8 L / min, program running trajectory is along the spiral direction, the laser head is at an angle of 75° to the end face, and the powder feeding rate is 2.0 r / min.

5. The laser cladding repair process for spiral shafts in the food industry as claimed in claim 1, characterized in that: In step S3, the method for initially processing the end surface of the bottom layer of the spiral shaft is to grind the end surface of the spiral shaft flat by a grinder and measure the size to ensure that it is qualified.

6. The laser cladding repair process for spiral shafts in the food industry as claimed in claim 1, characterized in that: In step S4, the process parameters of laser cladding of the wear-resistant layer are as follows: laser power is 3200 W, spot size is 3 mm, robot running fitting speed is 90 cm / min, protective gas is Ar, gas flow rate is 8 L / min, program running trajectory is along the spiral direction, the laser head is at an angle of 75° to the end face, and the powder feeding rate is 2.5 r / min.

7. The laser cladding repair process for spiral shafts in the food industry as claimed in claim 1, characterized in that: In step S4, the method for final processing of the end surface is to grind the wear-resistant layer of the end surface of the spiral shaft flat by a grinder and measure the size of the finished product.

Citation Information

Patent Citations

  • Screw helicoidal surface repairing process