Test methods for photovoltaic encapsulation films

By pretreatment and lamination testing of the photovoltaic packaging film, the crosslinking degree and peel strength are quickly evaluated, and the problem of difficulty in taking into account rapid testing and performance reliability and stability in the prior art is solved, and the photovoltaic packaging film is realized. rapid reliability assessment and risk identification.

CN117451977BActive Publication Date: 2024-11-05TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311388743.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2024-11-05
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

The prior art is difficult to take into account the reliability and stability of rapid testing and photovoltaic packaging film performance, especially in batch testing, and it is difficult to quickly identify reliability risks and stability.

Method used

By pretreating the photovoltaic packaging film, the conditions during long-term placement, transportation, turnover and storage are simulated, cross-linked cured laminated structure is formed, and the cross-linking degree and peel strength are quickly tested, and the parameter attenuation test results are passed Estimate long-term reliability and risks.

Benefits of technology

It has achieved rapid verification of key performance indicators of photovoltaic packaging films, timely identification of reliability risks, and reduced product failure risks. It has important practical significance for new materials development and batch testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117451977B_ABST
    Figure CN117451977B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a test method for photovoltaic encapsulation film, which includes: sampling a first laminate structure and detecting a target parameter to obtain a first parameter value of a pretreated first encapsulation film in the first laminate structure; the first laminate structure is formed by stacking and laminating a first panel, a first release film, a first encapsulation film, a second release film and a second panel; the pretreatment includes a constant temperature pretreatment or a high and low temperature cycle pretreatment; sampling a second laminate structure and detecting a target parameter to obtain a second parameter value of a second encapsulation film that has not been pretreated in the second laminate structure; the second laminate structure is formed by stacking and laminating a third panel, a third release film, a second encapsulation film, a fourth release film and a fourth panel; according to the first parameter value and the second parameter value, determining the parameter attenuation test result of the encapsulation film. Through the test method disclosed in the present disclosure, the key performance indicators of the photovoltaic encapsulation film can be quickly verified and its reliability risks can be identified in a timely manner.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a testing method for photovoltaic encapsulation adhesive film, and in particular to a testing method for rapidly evaluating the performance and quality stability of photovoltaic encapsulation adhesive film. Background Art

[0002] As the sustainable development of human economy and society places higher and higher demands on energy and environmental protection, photovoltaic power generation is gaining more and more attention. At present, crystalline silicon photovoltaic modules mainly include single-sided power generation modules and double-sided power generation modules. Packaging materials of different materials and structures can be selected according to different packaging methods and photovoltaic types. The usual photovoltaic module consists of a front plate (photovoltaic glass, plastic front plate, etc.), a transparent packaging film on the front, a solar cell, a transparent or white packaging film on the back, and a back plate (back plate or glass, etc.), and is packaged by vacuum heating, lamination, curing and packaging. The material, formula and process of the packaging film play a vital role in the performance and reliability of photovoltaic modules. At present, the mainstream photovoltaic packaging films on the market include EVA (ethylene-vinyl acetate copolymer), POE (polyolefin) and co-extruded EPE (EVA and POE multi-layer co-extruded material). The packaging film is composed of resin particles and various additives such as cross-linking agents, coupling agents, and anti-aging agents. The composition and proportion of the additives play an extremely important role in the performance of the packaging film. Especially for POE materials and co-extruded EPE materials, due to the influence of molecular structure, POE exhibits non-polar properties, while most additives mainly exhibit polar properties due to their special functions and functional group structures. Therefore, according to the "like dissolves like" principle, during long-term placement, transportation, turnover and storage, additive migration is likely to occur, resulting in risks such as unstable performance of the encapsulation film and reliability failure.

[0003] Common means and methods for evaluating the performance, quality stability and reliability of photovoltaic encapsulation films are mainly divided into short-term tests and long-term reliability tests. Short-term tests include cross-linking tests and peel strength tests. Cross-linking tests and peel strength tests are important indicators that directly affect long-term reliability. Cross-linking tests and peel strength tests have the advantages of fast test speed and simple operation, but it is often difficult to characterize and predict the long-term performance and stability of photovoltaic samples. Long-term reliability tests include damp heat tests, wet freeze tests, thermal cycle tests, anti-PID (Potential Induced Degradation) tests, creep tests, UV aging tests, etc. (refer to IEC61215 and IEC61730 standards). Although these long-term reliability tests can effectively identify the long-term reliability of packaging materials, they are affected by the shortage of testing resources, high testing costs, long testing time and limited number of samples, making it difficult to achieve rapid evaluation feedback and large-scale testing verification.

[0004] It is difficult for existing technologies to take into account both rapid testing and stable performance reliability. How to quickly identify the performance, quality and reliability of photovoltaic encapsulation films and ensure the stability, safety and reliability of batch use has always been a topic that technicians in this field need to explore. Summary of the invention

[0005] In order to solve at least one of the above problems, a testing method for photovoltaic encapsulation film is provided. Through this testing method, key performance indicators of photovoltaic encapsulation film can be quickly verified and reliability risks of photovoltaic encapsulation film can be identified in time.

[0006] According to another aspect of the present disclosure, a method for testing a photovoltaic encapsulation film is provided, and the method may include: sampling a first laminate structure and detecting a target parameter to obtain a first parameter value of a pretreated first encapsulation film in the first laminate structure; wherein the first laminate structure is formed by stacking and laminating a first panel, a first release film, the pretreated first encapsulation film, a second release film and a second panel; pretreatment includes constant temperature pretreatment or high and low temperature cycle pretreatment; sampling a second laminate structure and detecting a target parameter to obtain a second parameter value of an unpretreated second encapsulation film in the second laminate structure; wherein the second laminate structure is formed by stacking and laminating a third panel, a third release film, the unpretreated second encapsulation film, a fourth release film and a fourth panel; and determining a parameter attenuation test result of the encapsulation film based on the first parameter value and the second parameter value.

[0007] Optionally, the target parameter may include a degree of cross-linking of the packaging film, wherein, in the first laminate structure, the area of ​​the first release film and the second release film are the same as the area of ​​the first panel, the pretreated first packaging film, and the second panel; and in the second laminate structure, the area of ​​the third release film and the fourth release film are the same as the area of ​​the third panel, the unpretreated second packaging film, and the fourth panel.

[0008] Optionally, the first parameter value is a first crosslinking degree and the second parameter value is a second crosslinking degree, and the parameter attenuation test result includes a crosslinking degree attenuation value, and the crosslinking degree attenuation value=(second crosslinking degree-first crosslinking degree) / first crosslinking degree.

[0009] Optionally, the target parameter may include the peel strength of the packaging film, wherein, in the first laminated structure, the area of ​​the first release film is smaller than the area of ​​the first panel and the pretreated first packaging film, and the area of ​​the second release film is smaller than the area of ​​the pretreated first packaging film and the second panel; and in the second laminated structure, the area of ​​the third release film is smaller than the area of ​​the third panel and the non-pretreated second packaging film, and the area of ​​the fourth release film is smaller than the area of ​​the non-pretreated second packaging film and the fourth panel.

[0010] Optionally, the first parameter value is a first peel strength and the second parameter value is a second peel strength, and the parameter attenuation test result includes a peel strength attenuation value, and the peel strength attenuation value=(second peel strength−first peel strength) / first peel strength.

[0011] Optionally, the pre-treated first packaging adhesive film comprises two stacked pre-treated packaging adhesive films, and the unpre-treated second packaging adhesive film comprises two stacked unpre-treated packaging adhesive films.

[0012] Optionally, the constant temperature pretreatment can be performed in a constant temperature environment test box, and the temperature is 30° C. to 85° C., and the duration is 2 hours to 48 hours.

[0013] Optionally, the high-low temperature cycle pretreatment is carried out in a high-low temperature cycle test box, and the temperature is -40°C to 85°C, the single cycle time does not exceed 6 hours, and the number of cycles is 1 to 8 times.

[0014] Optionally, the sampling positions of the method may include one or more positions of four corner positions and a central position in the first laminate structure and / or the second laminate structure.

[0015] Optionally, the sampling position of the method includes the position where the first release film and / or the second release film are located in the first laminate structure, and includes the position where the third release film and / or the fourth release film are located in the second laminate structure.

[0016] According to the test method of photovoltaic encapsulation film disclosed in the present invention, the photovoltaic encapsulation film is pretreated to simulate the long-term placement, transportation, turnover and storage process that the photovoltaic encapsulation film may experience, and then a cross-linked and cured laminated structure is obtained after lamination, and the cross-linking degree and peel strength are quickly tested, and the long-term reliability and risk are quickly estimated according to the test results. This test method has important practical significance for the development of new photovoltaic materials and reducing the risk of product failure. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1A schematic flow chart of a testing method according to an embodiment of the present disclosure is shown;

[0018] Figure 2 A schematic cross-sectional view of a laminate structure for testing a degree of crosslinking in a testing method according to an embodiment of the present disclosure is shown;

[0019] Figure 3 A schematic cross-sectional view of a laminate structure for testing peel strength in a testing method according to an embodiment of the present disclosure is shown;

[0020] Figure 4 A graph showing temperature changes over time during high and low temperature cycle pretreatment in a test method according to an embodiment of the present disclosure; and

[0021] Figure 5 A schematic diagram showing sampling positions of a testing method according to an embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand the technical solutions of the present disclosure, the exemplary embodiments will be described in detail below. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present disclosure. Instead, they are merely examples of systems and methods consistent with some aspects of the present embodiment disclosed as detailed in the attached claims.

[0023] The present disclosure provides a testing method for photovoltaic encapsulation films, the method comprising: sampling a first laminated structure 1 and detecting a target parameter to obtain a first parameter value of a pretreated first encapsulation film 13, 14 in the first laminated structure 1; wherein the first laminated structure 1 is formed by stacking and laminating a first panel 11, a first release film 12, pretreated first encapsulation films 13, 14, a second release film 15 and a second panel 16; the pretreatment may include a constant temperature pretreatment or a high and low temperature cycle pretreatment; sampling a second laminated structure 1' and detecting a target parameter to obtain a second parameter value of a second encapsulation film 13', 14' not pretreated in the second laminated structure 1'; wherein the second laminated structure 1' is formed by stacking and laminating a third panel 11', a third release film 12', unpretreated second encapsulation films 13', 14', a fourth release film 15' and a fourth panel 16'; and determining a parameter attenuation test result of the encapsulation film according to the first parameter value and the second parameter value.

[0024] In other words, reference Figure 1First, the photovoltaic encapsulation film is pretreated including constant temperature pretreatment or high and low temperature cycle pretreatment, so as to simulate the long-term placement, transportation, turnover, and storage process that the photovoltaic encapsulation film may experience; then, the pretreated photovoltaic encapsulation film and other necessary layers (for example, the above-mentioned panel, release film) are stacked and laminated to obtain a cross-linked and cured laminated structure (that is, the first laminated structure 1) (that is, step S1, forming a laminated structure with a pretreated film). Then, the first laminated structure 1 is sampled and the target parameters (for example, the test crosslinking degree and peel strength described later) are detected to obtain the first parameter values ​​of the pretreated first encapsulation films 13 and 14 in the first laminated structure 1 (that is, step S2, obtaining the first target parameter). On the other hand, as a reference, the unpretreated adhesive film and other necessary layers (e.g., the above-mentioned panel, release film) are stacked and laminated to obtain a cross-linked cured laminated structure (i.e., the second laminated structure 1') (i.e., step S3, forming a laminated structure with an unpretreated adhesive film), and then the second parameter value corresponding to the first parameter value is obtained (i.e., step S4, obtaining the second target parameter). Finally, according to the first target parameter and the second target parameter, the parameter attenuation test result of the pretreated adhesive film compared with the unpretreated adhesive film is determined (i.e., step S5, determining the parameter attenuation test result). In this way, the reliability and risk of photovoltaic cells can be quickly estimated.

[0025] The first laminated structure 1 and the second laminated structure 1' have the same basic structure, the only difference is that the encapsulation film laminated in the first laminated structure 1 is a pre-treated encapsulation film, while the encapsulation film laminated in the second laminated structure 1' is an unpre-treated encapsulation film. Here, the "lamination" in the laminated structure obtained by stacking and laminating refers to the stacked layers being cured and packaged by vacuum heating and laminating.

[0026] The release film can be easily separated from the adjacent layer, which is conducive to the test of the target parameter. The first release film 12 and the second release film 15 in the first laminated structure 1 can be the same type of release film; the third release film 12' and the fourth release film 15' in the second laminated structure 1' can be the same type of release film; the first release film 12 and the second release film 15 in the first laminated structure 1 can be the same type of release film as the third release film 12' and the fourth release film 15' in the second laminated structure 1'.

[0027] The panel is a panel for photovoltaic cells. It should be understood that the first panel 11 and the second panel 16 in the first laminate structure 1 can be panels of the same type; the third panel 11' and the fourth panel 16' in the second laminate structure 1' can be panels of the same type; the first panel 11 and the second panel 16 in the first laminate structure 1 can be panels of the same type as the third panel 11' and the fourth panel 16' in the second laminate structure 1'. In some embodiments, the first panel 11 and the third panel 11' can be glass panels used as front panels; and the second panel 16 and the fourth panel 16' can be used as photovoltaic back panels.

[0028] In some embodiments, the target parameter may include the degree of crosslinking of the encapsulating film. In this case, in the first laminate structure 1, the area of ​​the first release film 12 and the second release film 15 is the same as the area of ​​the first panel 11, the pre-treated first encapsulating film 13, 14, and the second panel 16; and in the second laminate structure 1', the area of ​​the third release film 12' and the fourth release film 15' is the same as the area of ​​the third panel 11', the unpre-treated second encapsulating film 13', 14', and the fourth panel 16'. In other words, when the target parameter is the degree of crosslinking of the encapsulating film, the reference Figure 2 In the first laminate structure 1, the first release film 12 completely separates the first panel 11 from the pre-treated first packaging films 13 and 14, and the second release film 15 completely separates the pre-treated first packaging films 13 and 14 from the second panel 16, which is conducive to separating the first packaging films 13 and 14 when performing a cross-linking degree test. Similarly, in this case, in the second laminate structure 1', the third release film 12' completely separates the third panel 11' from the unpre-treated second packaging films 13' and 14', and the fourth release film 15' completely separates the unpre-treated second packaging films 13' and 14' from the fourth panel 16', which is conducive to separating the unpre-treated second packaging films 13' and 14' when performing a cross-linking degree test.

[0029] When the target parameter is the degree of cross-linking of the packaging film, the first parameter value can be the first degree of cross-linking (i.e., the degree of cross-linking of the pretreated first packaging film 13, 14) and the second parameter value can be the second degree of cross-linking (i.e., the degree of cross-linking of the unpretreated second packaging film 13', 14'), and the parameter attenuation test result includes a cross-linking degree attenuation value, which is = (second degree of cross-linking - first degree of cross-linking) / first degree of cross-linking.

[0030] In some embodiments, the target parameter may also include the peel strength of the packaging film. In this case, in the first laminate structure 1, the area of ​​the first release film 12 is smaller than the area of ​​the first panel 11, the pre-treated first packaging film 13, 14, and the area of ​​the second release film 15 is smaller than the area of ​​the pre-treated first packaging film 13, 14, and the second panel 16; and in the second laminate structure 1', the area of ​​the third release film 12' is smaller than the area of ​​the third panel 11', the unpre-treated second packaging film 13', 14', and the area of ​​the fourth release film 15' is smaller than the area of ​​the unpre-treated second packaging film 13', 14', and the fourth panel 16'. In other words, when the target parameter is the peel strength of the packaging film, the reference Figure 3 In the first laminate structure 1, the first release film 12 only partially separates the first panel 11 from the pre-treated first encapsulation films 13, 14, and the second release film 15 only partially separates the pre-treated first encapsulation films 13, 14 from the second panel 16, thereby facilitating the start of the first encapsulation films 13, 14 when performing a peel strength test (to be described below). Similarly, in this case, in the second laminate structure 1', the third release film 12' only partially separates the third panel 11' from the unpre-treated second encapsulation films 13', 14', and the fourth release film 15' only partially separates the unpre-treated second encapsulation films 13', 14' from the fourth panel 16', thereby facilitating the start of the second encapsulation films 13', 14' when performing a peel strength test.

[0031] When the target parameter is the peel strength of the packaging film, the first parameter value can be the first peel strength (i.e., the peel strength of the pretreated first packaging film 13, 14) and the second parameter value can be the second peel strength (i.e., the peel strength of the unpretreated second packaging film 13', 14'), and the parameter attenuation test result can include a peel strength attenuation value, which is (second peel strength-first peel strength) / first peel strength.

[0032] The first laminated structure 1 and the second laminated structure 1' can be formed by taking a photovoltaic glass plate with a size close to that of the photovoltaic module and simulating the structure of the photovoltaic module for lamination. The pretreated first encapsulation film can be an integrated encapsulation film, however, in some embodiments, in order to better simulate the actual photovoltaic panel structure, the pretreated first encapsulation film can include two stacked pretreated encapsulation films 13, 14. Similarly, the untreated second encapsulation film can be an integrated encapsulation film, however, in some embodiments, in order to better simulate the actual photovoltaic panel structure, the unpretreated second encapsulation film can include two stacked unpretreated encapsulation films 13', 14'.

[0033] The first encapsulation films 13, 14 and the second encapsulation films 13', 14' may include one or more of EVA films, POE films and co-extruded EPE films. The first encapsulation films 13 and the first encapsulation films 14 may be the same films or different films; the second encapsulation films 13' and the second encapsulation films 14' may be the same films or different films; the first encapsulation films 13 and the second encapsulation films 13' may be the same films; and the first encapsulation films 14 and the second encapsulation films 14' may be the same films.

[0034] In some embodiments, before pre-treating the photovoltaic encapsulation film, the outer layer of the photovoltaic encapsulation film exposed to the environment is removed. This is because the photovoltaic encapsulation film is usually stored in the form of a roll before pre-treatment, so the outer layer of the photovoltaic encapsulation film in the roll form exposed to the environment is usually contaminated. In addition, before pre-treating the photovoltaic encapsulation film, it is not allowed to use alcohol to wipe the surface of the photovoltaic encapsulation film to avoid the additive of the film being dissolved by alcohol, thereby affecting the test structure. In some embodiments, after removing the outer layer of the photovoltaic encapsulation film exposed to the environment, the photovoltaic encapsulation film can be cut to a certain size (for example, close to the size of the photovoltaic module) for a certain number for subsequent testing.

[0035] In some embodiments, the constant temperature pretreatment is a pretreatment in which the photovoltaic encapsulation film is placed in a constant temperature environment test chamber. The test conditions of the constant temperature environment test chamber are: a temperature of 30°C to 85°C and a duration of 2 hours to 48 hours; more preferably, the temperature is 40°C and the duration is 24 hours.

[0036] In some embodiments, the high and low temperature cycle pretreatment is a pretreatment in which the photovoltaic encapsulation film is placed in a high and low temperature cycle test chamber. The test conditions of the high and low temperature cycle test chamber are: the temperature is -40°C to 85°C, the single cycle time does not exceed 6 hours, and the number of cycles is 1 to 8 times; more preferably, the temperature is -20°C to 40°C, and the number of cycles is 4 times. Further, see Figure 4 , shows a graph of temperature changes over time during high and low temperature cycle pretreatment in the test method according to an embodiment of the present disclosure. Figure 4 For example, the value of t2-t1 may be in the range of 10 minutes to 30 minutes, and the value of t5-t4 may be in the range of 10 minutes to 30 minutes. The time from 0 hours to t6 is one cycle. Between t2 and t4, the temperature rise rate may not exceed 100°C / h, and between t5 and t6, the temperature drop rate may not exceed 100°C / h.

[0037] Sampling the first laminate structure 1 and the second laminate structure 1' refers to obtaining samples from the sampling positions described below: Figure 5As shown, the sampling positions of the test method preferably include one or more positions among four corner positions G1 , G2 , G3 , G4 and a central position C in the first laminate structure 1 and / or the second laminate structure 1 ′.

[0038] In addition, when the target parameter is the peel strength of the packaging film as described above, the sampling position of this method also satisfies the position where the first release film 12 and / or the second release film 15 are located in the first laminated structure 1, and the position where the third release film 13' and / or the fourth release film 15' are located in the second laminated structure 1'. In this way, it can be ensured that the sample for peel strength test includes the part where the film is bonded to the panel and the part where the film and the panel are separated by the release film, so that the test can be carried out near the release film.

[0039] In some embodiments, the crosslinking degree test can be carried out by xylene extraction method or DSC method (refer to IEC62788-1-6). In the xylene method, the stainless steel mesh used to place the sample (the first laminated structure 1 and the second laminated structure 1' after sampling) can be 50 mesh to 400 mesh, the weight of the sample can be 0.1g to 1g, and the extraction time can be 3 hours to 10 hours; more preferably, the stainless steel mesh can be 120 mesh, the weight of the sample can be 0.2g, and the extraction time can be 5 hours. In the DSC method, a raw sample of the photovoltaic encapsulation film that is not cross-linked is placed in a specific container. Crosslinking will occur during the heating process of the sample, generating an exothermic peak, and the corresponding thermal enthalpy value is recorded. The cooked sample of the cross-linked photovoltaic encapsulation film is tested in the same way, and the thermal enthalpy value is recorded. The degree of crosslinking is calculated based on the difference in thermal enthalpy between the raw sample that is not cross-linked and the cooked sample that is cross-linked.

[0040] The peel strength test is described below by taking the first laminate structure 1 as an example. It should be understood that the peel strength test is also applicable to the second laminate structure 1'. It should also be understood that the peel strength test described here is only exemplary, but not limited to this. Figure 3 The peel strength test may include: using a tensile gauge to clamp one end of the sample of the first laminate structure 1, and peeling the first panel 11 from the first packaging film 13, 14 or peeling the second panel 16 from the first packaging film 13, 14 from the other end of the sample of the first laminate structure 1, to obtain the peel strength. More specifically, for example, a sample of a certain width is taken, and a tensile gauge is used to clamp the first laminate structure 1, at the end of the sample. Figure 3 in the right end, and from the first laminated structure 1, the Figure 3The first panel 11 is separated from the first packaging films 13 and 14 at the left end (starting point) in the middle. Here, since the first release film 12 is present near the starting point, it is easy to start at the starting point. The tensile gauge clamps the first panel 11 at the starting point, pulls the sample at a certain speed, records the pulling force value, and calculates the peeling strength. The peeling strength test method can refer to GB / T 2790 and GB / T 2791, for example. Alternatively, the tensile gauge can be used to clamp the first laminate structure 1, Figure 3 in the left end, and from the first laminated structure 1, the Figure 3 The second panel 16 is separated (started) from the first packaging films 13 and 14 at the right end (starting point) in the middle, thereby recording the tensile force value and calculating the peeling strength.

[0041] Despite Figure 3 In the embodiment, the first release film 12 and the second release film 15 are respectively disposed near both ends of the first laminate structure 1, however, the present disclosure is not limited thereto. It is sufficient as long as the first release film 12 and the second release film 15 are present near the beginning of the sample so that the peel strength test can be conveniently performed. In other words, the first release film 12 and the second release film 15 are disposed near the beginning of the sample so that the peel strength test can be conveniently performed. Figure 3 and Figure 5 , the first release film 12 and the second release film 15 may be located near the edge of the sampling position. The same applies to the second laminated structure 1'.

[0042] After completing the above cross-linking degree test and peeling strength test, the following can be obtained: a. the cross-linking degree, peeling strength with glass plate (first panel 11, third panel 11'), and peeling strength with photovoltaic back sheet (second panel 16 and fourth panel 16') of the photovoltaic encapsulation film without pretreatment; b. the cross-linking degree, peeling strength with glass plate, and peeling strength with photovoltaic back sheet of the photovoltaic encapsulation film pretreated at constant temperature; c. the cross-linking degree, peeling strength with glass plate, and peeling strength with photovoltaic back sheet of the photovoltaic encapsulation film pretreated by high and low temperature cycles. After that, the reliability tests such as wet heat, wet freeze, thermal cycle, PID resistance, and creep can also be carried out on the photovoltaic encapsulation film without pretreatment.

[0043] Table 1 below lists the above-mentioned related parameters obtained at sampling positions G1, G2, G3, G4 and C after testing samples of three photovoltaic encapsulation films: EVA, co-extruded EPE and POE. Here, the constant temperature pretreatment condition is selected as 30°C, 12 hours, and the high and low temperature cycle pretreatment condition is selected as -40°C to 25°C, 2 cycles.

[0044] Specifically, the EVA, co-extruded EPE and POE samples were pretreated by setting different high-temperature pretreatment test conditions and high-low temperature cycle pretreatment conditions. Then, the two pretreated samples and the unpretreated samples were stacked and laminated respectively, and the crosslinking degree and peel strength values ​​at positions G1-G4 and position C were tested respectively. The test results of the crosslinking degree and peel strength were compared with the reliability results of the unpretreated photovoltaic encapsulation film. The results show that by treating the photovoltaic encapsulation film with rapid high-temperature pretreatment and high-low temperature cycle pretreatment, and then testing the crosslinking degree and peel strength, the encapsulation film formula and process stability can be quickly evaluated, and the long-term reliability failure risk can be estimated in advance.

[0045] The present disclosure has developed a new test scheme, which pre-treats the photovoltaic encapsulation film, quickly tests the degree of cross-linking and peel strength after lamination, and quickly estimates the long-term reliability based on the test results. The present disclosure simulates the transportation and storage processes that the material must go through, quickly verifies the key performance indicators of the photovoltaic encapsulation film, and promptly identifies the reliability risks of the photovoltaic encapsulation film. Considering that different types of additives have different degrees of sensitivity to temperature, this test method designs two modes: high-temperature constant temperature pretreatment and high-low temperature cycle pretreatment, to pre-treat the encapsulation film to simulate the different types of situations that the encapsulation film may experience before use. This test method has important practical significance for the development of new photovoltaic materials and reducing the risk of product failure.

[0046] Table 1 Test parameters of EVA, co-extruded EPE and POE

[0047]

[0048] Among them, · indicates no obvious abnormality, and ○ indicates local slight delamination.

[0049] It should be understood that the target parameters to be detected for the first laminate structure 1 and the second laminate structure 1' are not limited to the degree of crosslinking and peel strength, but may also be other appropriate target parameters that can quickly verify the key performance indicators of the photovoltaic encapsulation film and promptly identify its reliability risks.

[0050] In addition, the present application detects the target parameters of the second laminated structure 1' including the adhesive film without pretreatment as a reference for the target parameters of the first laminated structure 1 including the adhesive film with pretreatment. However, when these target parameters of the photovoltaic panel (without pretreatment) to be evaluated are known (for example, the detection has been completed before leaving the factory, and the detected target parameters have been entered into the database), the second laminated structure may not be stacked, and no relevant tests are performed on the second laminated structure.

[0051] It should also be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the gist and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for testing a packaging film, characterized in that: The method comprises: Sampling the first laminated structure and detecting target parameters to obtain a first parameter value of a pretreated first encapsulation film in the first laminated structure; wherein the first laminated structure is formed by stacking and laminating a first panel, a first release film, the pretreated first encapsulation film, a second release film and a second panel; the pretreatment includes a constant temperature pretreatment or a high and low temperature cycle pretreatment, and the pretreatment of the first encapsulation film is performed before the first encapsulation film is laminated, so as to simulate the long-term placement, transportation, turnover and storage process that the photovoltaic encapsulation film may experience; Sampling the second laminated structure and detecting the target parameter to obtain the second parameter value of the untreated second encapsulation film in the second laminated structure; wherein the second laminated structure is formed by stacking and laminating a third panel, a third release film, the untreated second encapsulation film, a fourth release film and a fourth panel; and A parameter attenuation test result of the packaging film is determined according to the first parameter value and the second parameter value.

2. The testing method according to claim 1, characterized in that: The target parameters include the degree of crosslinking of the encapsulation film, Among them, in the first laminated structure, the area of ​​the first release film and the second release film is the same as the area of ​​the first panel, the pretreated first packaging film, and the second panel; and in the second laminated structure, the area of ​​the third release film and the fourth release film is the same as the area of ​​the third panel, the unpretreated second packaging film, and the fourth panel.

3. The testing method according to claim 2, characterized in that: The first parameter value is a first cross-linking degree and the second parameter value is a second cross-linking degree, The parameter attenuation test result includes a cross-linking degree attenuation value, and the cross-linking degree attenuation value=(second cross-linking degree-first cross-linking degree) / first cross-linking degree.

4. The testing method according to claim 1, characterized in that: The target parameters include the peel strength of the encapsulation film, Among them, in the first laminated structure, the area of ​​the first release film is smaller than the area of ​​the first panel and the pretreated first packaging film, and the area of ​​the second release film is smaller than the area of ​​the pretreated first packaging film and the second panel; and in the second laminated structure, the area of ​​the third release film is smaller than the area of ​​the third panel and the non-pretreated second packaging film, and the area of ​​the fourth release film is smaller than the area of ​​the non-pretreated second packaging film and the fourth panel.

5. The testing method according to claim 4, characterized in that: The first parameter value is a first peel strength and the second parameter value is a second peel strength, The parameter attenuation test result includes a peel strength attenuation value, and the peel strength attenuation value=(second peel strength−first peel strength) / first peel strength. 6 . The testing method according to claim 1 , wherein the pretreated first packaging adhesive film comprises two stacked pretreated packaging adhesive films, and the unpretreated second packaging adhesive film comprises two stacked unpretreated packaging adhesive films.

7. The testing method according to any one of claims 1 to 5, characterized in that: The constant temperature pretreatment is carried out in a constant temperature environment test box, and the temperature is 30° C. to 85° C., and the duration is 2 hours to 48 hours.

8. The testing method according to any one of claims 1 to 5, characterized in that: The high and low temperature cycle pretreatment is carried out in a high and low temperature cycle test box, and the temperature is -40°C to 85°C, the single cycle time does not exceed 6 hours, and the number of cycles is 1 to 8 times.

9. The testing method according to any one of claims 1 to 5, characterized in that: The sampling positions of the method include one or more positions among four corner positions and a central position of each of the first laminate structure and the second laminate structure.

10. The testing method according to claim 4 or 5, characterized in that: The sampling position of the method includes the position where the first release film and / or the second release film are located in the first laminated structure, and includes the position where the third release film and / or the fourth release film are located in the second laminated structure.