Cutting tools
By employing a Ti(1-xy)AlxMyN coating structure on the cutting tool, the problem of short tool life in high-efficiency machining is solved, achieving a longer tool life and excellent film strength in high-efficiency machining.
Patent Information
- Application Number
- CN202180099330.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-06-30
AI Technical Summary
In high-efficiency machining, the lifespan of existing cutting tools is relatively short, making it difficult to meet the demands of high-efficiency machining.
A coating structure is adopted, wherein the first layer is composed of Ti(1-xy)AlxMyN, and x and y vary along the thickness direction. The maximum value of x, xmax, is above 0.20 and below 0.70, and the maximum value of y, ymax, is above 0.01 and below 0.20. By suppressing the inconsistency of lattice constant, a fine structure is formed to improve the film strength.
In high-efficiency machining, the cutting tool has a longer tool life and improves the peel resistance and film strength of the coating.
Smart Images

Figure CN117480023B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a cutting tool. Background Technology
[0002] Various studies have been conducted with the aim of extending the lifespan of cutting tools. Japanese Patent Application Publication No. 8-119774 (Patent Document 1) discloses a composite high-hardness material for tools having a substrate composed of cBN sintered body. This composite high-hardness material has a hard, heat-resistant coating with a composition represented by TiAlN. Furthermore, International Patent Publication No. 2021 / 085253 (Patent Document 2) discloses a surface-coated cutting tool having a tool substrate composed of cubic boron nitride sintered body and a hard coating layer on the surface of the tool substrate. This hard coating layer has a lower layer (AlTiN layer) directly above the tool substrate and an upper layer (AlTiBN layer) above the lower layer. The upper layer has a composition modulation structure in which the boron concentration repeatedly varies along the layer thickness direction.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 8-119774
[0006] Patent Document 2: International Publication No. 2021 / 085253 Summary of the Invention
[0007] The cutting tool disclosed herein comprises a substrate and a coating disposed on the substrate, wherein,
[0008] The coating comprises a first layer.
[0009] The thickness of the first layer is greater than 0.2 μm and less than 9 μm.
[0010] The first layer consists of Ti (1-x-y) Al x M y N constitutes,
[0011] M is an element selected from the group consisting of zirconium, hafnium, elements of Group 5 of the periodic table, elements of Group 6 of the periodic table, silicon, and boron.
[0012] In the first layer, x and y vary along the thickness direction of the first layer.
[0013] The maximum value of x is x max Values between 0.20 and 0.70
[0014] The minimum value of x minValues above 0 and below 0.6
[0015] The x max With the x min Satisfying 0.01≤x max -x min ≤0.7,
[0016] The maximum value of y is y max Values between 0.01 and 0.20
[0017] The minimum value of y min Values above 0 and below 0.19.
[0018] The y max With the y min Satisfying 0.01≤y max -y min ≤0.2. Attached Figure Description
[0019] Figure 1 This is a perspective view illustrating one manner of a cutting tool according to the present disclosure.
[0020] Figure 2 This is a schematic cross-sectional view illustrating one manner of the cutting tool of this disclosure.
[0021] Figure 3 This is a schematic cross-sectional view illustrating other ways of using the cutting tool of this disclosure.
[0022] Figure 4 This is a schematic cross-sectional view that further illustrates other ways of the cutting tool of this disclosure.
[0023] Figure 5 This is a schematic cross-sectional view illustrating another aspect of the cutting tool of this disclosure.
[0024] Figure 6 This is a schematic cross-sectional view that further illustrates another aspect of the cutting tool of this disclosure.
[0025] Figure 7 This is an example illustrating the relationship between the depth of the first layer and x and y in one embodiment of the cutting tool disclosed herein.
[0026] Figure 8 This is an example of a graph illustrating the relationship between the depth of the first layer and x and y in another embodiment of the cutting tool disclosed herein.
[0027] Figure 9 It is a diagram illustrating the relationship between the concavity / convexity and the skewness of the opposite side.
[0028] Figure 10It is a diagram illustrating the relationship between the concavity / convexity and the skewness of the opposite side. Detailed Implementation
[0029] [The problem this disclosure aims to solve]
[0030] In recent years, the demand for high-efficiency machining has increased. Consequently, high-efficiency machining also requires cutting tools with longer tool life.
[0031] Therefore, the purpose of this disclosure is to provide a cutting tool that has a long tool life even in high-efficiency machining.
[0032] [The Effects of This Disclosure]
[0033] According to this disclosure, a cutting tool with a long tool life can be provided that also performs high-efficiency machining.
[0034] [Description of embodiments of this disclosure]
[0035] First, embodiments of this disclosure will be described.
[0036] (1) A cutting tool comprising a substrate and a coating disposed on the substrate, wherein...
[0037] The coating comprises a first layer.
[0038] The thickness of the first layer is greater than 0.2 μm and less than 9 μm.
[0039] The first layer consists of Ti (1-x-y) Al x M y N constitutes,
[0040] M is an element selected from the group consisting of zirconium, hafnium, elements of Group 5 of the periodic table, elements of Group 6 of the periodic table, silicon, and boron.
[0041] In the first layer, x and y vary along the thickness direction of the first layer.
[0042] The maximum value of x is x max Values between 0.20 and 0.70
[0043] The minimum value of x min Values above 0 and below 0.6
[0044] The x max With the x min Satisfying 0.01≤x max -x min ≤0.7,
[0045] The maximum value of y is ymax Values between 0.01 and 0.20
[0046] The minimum value of y min Values above 0 and below 0.19.
[0047] The y max With the y min Satisfying 0.01≤y max -y min ≤0.2.
[0048] The cutting tool disclosed herein can have a long tool life even in high-efficiency machining.
[0049] (2) Preferably, in the first layer, the average crystallite size is 5 nm or more and 90 nm or less. This further improves the film strength of the coating. Additionally, crack formation is suppressed in the first layer.
[0050] (3) Preferably, the coating further comprises a base layer.
[0051] The base layer is disposed directly above the substrate and directly below the first layer.
[0052] The thickness of the substrate layer is greater than 0.05 μm and less than 1.0 μm.
[0053] The base layer is made of Ti a Al 1-a N or Al p Cr 1-p N constitutes,
[0054] The value of a is greater than 0.2 and less than 1.0.
[0055] The p value is greater than or equal to 0 and less than or equal to 0.8. As a result, the adhesion between the substrate and the coating is improved in the cutting tool.
[0056] (4) Preferably, the residual stress of the first layer is above -3.0 GPa and below -0.1 GPa. As a result, the strength of the coated film is further improved.
[0057] (5) Preferably, the surface roughness Ra of the coating is... surf The thickness is above 0 μm and below 0.1 μm. As a result, the peel resistance of the coating is improved.
[0058] (6) Preferably, the skewness Rsk of the surface of the coating is... surf The value is above -2 and below 2. Therefore, the peel resistance of the coating is further improved.
[0059] (7) Preferably, the skewness Rsk of the surface of the substrate in contact with the coating is...sub The value is above -2 and below 2. Therefore, the peel resistance of the coating is further improved.
[0060] (8) Preferably, the X-ray diffraction intensity I relative to the (200) plane of the first layer (200) X-ray diffraction intensity I of the (111) plane of the first layer (111) and the X-ray diffraction intensity I of the (220) plane of the first layer. (220) The total of the I (200) The ratio I (200) / (I (200) +I (111) +I (220) The value is above 0.50. As a result, the peel resistance of the coating is further improved.
[0061] [Details of the embodiments disclosed herein]
[0062] Hereinafter, a specific example of a cutting tool according to one embodiment of the present disclosure (hereinafter also referred to as "this embodiment") will be described with reference to the accompanying drawings. In the drawings of this disclosure, the same reference numerals denote the same or equivalent parts. In addition, dimensional relationships such as length, width, thickness, and depth have been appropriately modified for the clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.
[0063] In this specification, expressions such as "A~B" refer to the upper and lower limits of a range (i.e., above A and below B). If no unit is recorded in A but only in B, the unit of A is the same as the unit of B.
[0064] In this specification, when compounds are represented by chemical formulas, all conventionally known atomic ratios are included unless otherwise specified, and are not necessarily limited to atomic ratios within the stoichiometric range. For example, when referred to as "TiAlSiN", the ratio of the number of atoms constituting TiAlSiN includes all conventionally known atomic ratios.
[0065] In the crystallographic descriptions in this specification, a single surface is indicated by ().
[0066] [Implementation Method 1: Cutting Tool]
[0067] like Figures 2-6 As shown, the cutting tool 10 according to this embodiment includes a substrate 11 and a coating 40 disposed on the substrate 11, wherein,
[0068] The coating 40 includes a first layer 12.
[0069] The thickness of the first layer 12 is greater than 0.2 μm and less than 9 μm.
[0070] The first layer 12 is composed of Ti (1-x-y) Al x M y N constitutes,
[0071] M is an element selected from the group consisting of zirconium, hafnium, elements of Group 5 of the periodic table, elements of Group 6 of the periodic table, silicon, and boron.
[0072] In the first layer 12, x and y vary along the thickness direction of the first layer 12.
[0073] The maximum value of x is x max Values between 0.20 and 0.70
[0074] The minimum value of x min Values above 0 and below 0.6
[0075] The x max With the x min Satisfying 0.01≤x max -x min ≤0.7,
[0076] The maximum value of y is y max Values between 0.01 and 0.20
[0077] The minimum value of y min Values above 0 and below 0.19.
[0078] The y max With the y min Satisfying 0.01≤y max -y min ≤0.2.
[0079] The cutting tool disclosed herein can maintain a long tool life even in high-efficiency machining. The reason for this is speculated as follows.
[0080] In the first layer 12 mentioned above, x and y vary along the thickness direction of the first layer 12, and the maximum value of x is x. max The minimum value of x is greater than 0.20 and less than 0.70. min If x is greater than 0 and less than 0.6, then x max and the x min Satisfying 0.01≤x max -x min ≤0.7, the maximum value of y is... max The minimum value of y is greater than 0.01 and less than 0.20. min If the value is above 0 and below 0.19, then y max and the y minSatisfying 0.01≤y max -y min ≤0.2. Therefore, it originates from Ti. (1-x-y) Al x M y The lattice constant of N is difficult to be uniform, and particle growth is suppressed in the aforementioned first layer 12. Therefore, this first layer 12 can form a fine structure. As a result, the cutting tool 10 having a coating 40 containing such a first layer 12 has excellent film strength, and thus can have a long tool life even in high-efficiency machining.
[0081] The shape and application of the cutting tool 10 involved in this embodiment are not particularly limited. For example, the shape of the cutting tool 10 involved in this embodiment can be listed as a drill bit, an end mill, an indexable cutting insert for a drill bit, an indexable cutting insert for an end mill, an indexable cutting insert for milling, an indexable cutting insert for turning, a metal saw, a gear cutting tool, a reamer, a tap, and a cutting insert for crankshaft pin grinding.
[0082] Figure 1 This is a perspective view illustrating one embodiment of the cutting tool 10 of this disclosure. The cutting tool 10 of this shape is used as an indexable cutting insert, such as a turning insert.
[0083] Furthermore, the cutting tool 10 involved in this embodiment is not limited to having, for example, Figure 1 The cutting tool 10 shown herein comprises a substrate 11 and a coating 40 formed on the substrate 11. It also includes cutting tools in which only a portion of the cutting tool 10 (especially the tip portion (cutting edge)) is constructed using the aforementioned structure. For example, cutting tools in which only the tip portion of a base (support body) made of cemented carbide or the like is constructed using the aforementioned structure are also included in the cutting tools according to this embodiment. In this case, the tip portion is technically considered as the cutting tool. In other words, even when the aforementioned structure occupies only a portion of the cutting tool, the aforementioned structure is still referred to as the cutting tool.
[0084] Substrate
[0085] The substrate used in this embodiment can be any conventionally known substrate without particular limitation. Examples of such substrates include cemented carbide (e.g., tungsten carbide (WC) based cemented carbide, cemented carbide containing Co in addition to WC, cemented carbide containing carbonitrides such as Ti, Ta, and Nb in addition to WC), cermets (materials with TiC, TiN, TiCN, etc. as the main components), high-speed steel, tool steel, ceramics (titanium carbide (TiC), silicon carbide (SiC), silicon nitride (SiN), aluminum nitride (AlN), alumina (Al2O3), silane, and mixtures thereof), cubic boron nitride sintered bodies (cBN sintered bodies), diamond sintered bodies, and hard materials in which cubic boron nitride particles are dispersed in the bonding phase.
[0086] Among these various substrates, cubic boron nitride sintered bodies are particularly preferred. This is because cubic boron nitride sintered bodies exhibit exceptionally excellent wear resistance in the cutting of high-hardness ferrous materials, making them suitable as substrates for cutting tools used in the aforementioned applications.
[0087] When using cemented carbide as the substrate, the effects of this embodiment are observed even when the microstructure contains abnormal phases referred to as free carbon or η phase. It should be noted that the substrate used in this embodiment can be a substrate whose surface has been modified. For example, in the case of cemented carbide, a de-β layer can be formed on its surface, or in the case of cBN sintered body, a surface-hardened layer can be formed; even with such surface modification, the effects of this embodiment are observed.
[0088] When the cutting tool is an indexable cutting insert (indexable cutting insert for turning, indexable cutting insert for milling, etc.), the base material includes both base materials with and without chip breakers. The shape of the tool tip includes any shape among sharp edges (the edge where the rake face and flank face intersect), honing (a shape with rounded corners on the sharp edges), negative cutting edge (a chamfered shape), and a combination of honing and negative cutting edge.
[0089] (The skewness of the surface of the substrate in contact with the coating)
[0090] The skewness Rsk of the surface of the substrate in contact with the coating sub Preferably, the deviation is between -2 and 2. Here, "deviation" refers to the deviation of the roughness curve specified in JIS B 0601-2001, a parameter representing the deviation between the peaks and valleys of a surface. In other words, as... Figure 9 as well as Figure 10As shown, "skewness" is an indicator of the symmetry between the peaks and troughs when the average line L1 is the center. When the surface is skewed upwards relative to the average line L1, the "skewness" is a positive value. Figure 9 Additionally, when the surface is tilted downwards relative to the average line L1, the "skewness" is negative. Figure 10 Additionally, in Figure 9 as well as Figure 10 When the probability density distribution curve shown is a normal distribution, the skewness is "0".
[0091] If the skewness Rsk of the surface of the substrate in contact with the coating is... sub If the deviation is between -2 and 2, then the distribution deviation of peaks and valleys on the surface of the substrate in contact with the coating becomes smaller, improving the adhesion to the coating. Furthermore, the smaller deviation in the distribution deviation of peaks and valleys on the surface of the substrate in contact with the coating reduces stress concentration caused by processing loads, thus improving the peel resistance of the coating. The aforementioned skewness Rsk sub The relationship between the adhesion between the substrate and the coating and the peel resistance of the coating is a new discovery made by the inventors of this invention.
[0092] The above Rsk sub More preferably, it is -1.8 or higher; even more preferably, it is -1.6 or higher; and still more preferably, it is -1.4 or higher. Additionally, the aforementioned Rsk... sub More preferably, it is 1.8 or less; even more preferably, it is 1.6 or less; and still more preferably, it is 1.4 or less. Additionally, the aforementioned Rsk... sub More preferably, it is -1.8 or higher and 1.8 or lower; even more preferably, it is -1.6 or higher and 1.6 or lower; and still more preferably, it is -1.4 or higher and 1.4 or lower.
[0093] <Substrate surface skewness Rsk in contact with the coating> sub Determination methods >
[0094] The skewness Rsk of the surface of the substrate in contact with the coating subFor example, it can be determined using the following method. First, a cutting tool is used to cut along the normal direction of its flank face, including the cutting tip, to expose a cross-section. The cutting can be performed using a focused ion beam apparatus or a cross-section polishing machine, etc. Using a scanning electron microscope (SEM), the cross-section is observed at 2000x magnification to obtain a reflected electron image. Next, using image processing software (e.g., "Winroof," manufactured by Mitani Corporation), the reflected electron image is magnified to 2.5x, thus obtaining the field of view. Then, within this field of view, an arbitrary portion of a 50μm square rectangle is selected, containing both the "coated surface" and the "surface of the substrate in contact with the coating (equivalent to the interface between the substrate and the coating)." The "surface of the substrate in contact with the coating" is traced and extracted as a line. Using image processing software (e.g., "Winroof," manufactured by Mitani Corporation), the extracted line is quantified, and the average value of this value is calculated. Here, "numericalizing the line" means that, when the extracted line is placed on the xy coordinate axis, the y-axis value of the line is output at 0.05 μm intervals in the x-axis direction. Then, based on this average value, an average line is drawn in a direction approximately parallel to the surface of the substrate in contact with the coating. Next, this average line is set as the X-axis, and the direction perpendicular to the X-axis is set as the Y-axis. Using this as the coordinate axis, the surface roughness curve Z(x) of the coating surface is obtained in this coordinate axis using the aforementioned image processing software. Then, by substituting Z(x) into the following equation (1), Rq is obtained. Here, "l" is "50 μm".
[0095] [Number 1]
[0096]
[0097] Next, by substituting Z(x) and Rq into the following equation (2), the skewness Rsk is obtained.
[0098] [Number 2]
[0099]
[0100] The skewness Rsk is calculated by taking the average value of the skewness Rsk obtained by performing the above measurements in any five fields of view in the above profile. sub .
[0101] Covering
[0102] The coating 40 is disposed on the substrate 11. Figures 2-6 ). Figures 2-6This is a schematic cross-sectional view illustrating one embodiment of the cutting tool of this disclosure. The "coating" improves the cutting tool's resistance to peeling, chipping, and wear by covering at least the tip portion of the substrate 11. The tip portion, as described herein, refers to the area within 500 μm along the surface of the substrate from the tip edge. Preferably, the coating 40 covers the entire surface of the substrate 11. However, even if a portion of the substrate 11 is not covered by the coating 40, or if the composition of the coating 40 is partially different, it does not depart from the scope of this embodiment.
[0103] The thickness of the aforementioned coating is preferably 0.4 μm or more and 8 μm or less, more preferably 0.6 μm or more and 7 μm or less, even more preferably 0.8 μm or more and 6 μm or less, even more preferably 1.0 μm or more and 5 μm or less, and particularly preferably 1.2 μm or more and 4 μm or less. Here, the thickness of the coating refers to the sum of the thicknesses of the individual layers constituting the coating. Examples of "layers constituting the coating" include, for example, the first layer described above, the base layer described above, and other layers described below besides the first layer and the base layer described above.
[0104] The thickness of the aforementioned coating can be determined as follows. First, a sample containing the coating is prepared by cutting at any point using a cutting tool. This sample can be prepared using a focused ion beam apparatus, a cross-section polishing machine, or the like. Next, the prepared cross-section is observed using a scanning electron microscope, and the magnification is adjusted to include the entire area in the thickness direction of the coating in the observed image. Then, the thickness is measured at five points, and the average value is taken as the coating thickness. The same procedure applies when measuring the thickness of the first layer, the substrate layer, and the other layers.
[0105] The aforementioned coating 40 includes a first layer 12. Furthermore, in one aspect of this embodiment, multiple first layers 12 may be provided as long as the effect of the cutting tool is maintained. Therefore, even if a portion of the coating is worn, the cutting tool can maintain excellent film strength because the first layer remains in the coating. Additionally, "including a first layer" means that the coating may include, in addition to the first layer, the aforementioned base layer and other layers described later, besides the first layer and the base layer.
[0106] (Skewing of the coated surface)
[0107] The skewness Rsk of the surface of the above-mentioned coating surf Preferably, the value is -2 or higher and 2 or lower. Therefore, on the surface of the coating, the deviation in the distribution of peaks and valleys is reduced, thus alleviating stress concentration caused by processing loads and improving the peel resistance of the coating. Furthermore, the aforementioned Rsk...surf More preferably, it is -1.8 or higher; even more preferably, it is -1.6 or higher; and still more preferably, it is -1.4 or higher. Additionally, the aforementioned Rsk... surf More preferably, it is 1.8 or less; even more preferably, it is 1.6 or less; and still more preferably, it is 1.4 or less. Additionally, the aforementioned Rsk... surf More preferably, it is -1.8 or higher and 1.8 or lower; even more preferably, it is -1.6 or higher and 1.6 or lower; and still more preferably, it is -1.4 or higher and 1.4 or lower.
[0108] (Surface roughness of the coating)
[0109] The surface roughness Ra of the above-mentioned coating surf Preferably, the surface roughness is 0 μm or more and 0.1 μm or less. Therefore, on the surface of the coating, due to the reduced unevenness, stress concentration caused by processing loads can be reduced, thus improving the peel resistance of the coating. Furthermore, the Ra... surf Preferably, the nanometer size is 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more. Furthermore, the Ra value described above... surf Preferably, it is 0.09 μm or less, more preferably 0.08 μm or less, and even more preferably 0.07 μm or less. Furthermore, the Ra value described above... surf Preferably, the surface roughness is 0.01 μm or more and 0.09 μm or less, more preferably 0.02 μm or more and 0.08 μm or less, and even more preferably 0.03 μm or more and 0.08 μm or less. Here, "surface roughness Ra" refers to the arithmetic mean roughness specified in JIS B 0601-2001.
[0110] It should be noted that the surface roughness Ra of the above-mentioned coating surf The measurement was performed according to the following steps. A 400μm square measurement area was defined within 1000μm of the rake face of the cutting tool and at a distance of 1000μm from the tool tip. The surface roughness of this measurement area was measured using a stylus-type surface shape measuring instrument. Following the same procedure, the surface roughness was measured at any five locations within the measurement area. The surface roughness Ra of the coating was calculated by averaging the surface roughness at these five locations. surf It should be noted that the aforementioned "skewness Rsk of the coated surface" refers to... surf "It can also be obtained using the same method."
[0111] <First Layer>
[0112] The thickness of the first layer is 0.2 μm or more and 9 μm or less. This improves the film strength of the coating. Furthermore, the thickness of the first layer is preferably 0.4 μm or more, more preferably 0.6 μm or more, and even more preferably 0.8 μm or more. Additionally, the thickness of the first layer is preferably 8 μm or less, more preferably 7 μm or less, and even more preferably 6 μm or less. Furthermore, the thickness of the first layer is preferably 0.4 μm or more and 8 μm or less, more preferably 0.6 μm or more and 7 μm or less, and even more preferably 0.8 μm or more and 6 μm or less.
[0113] The first layer mentioned above is composed of Ti (1-x-y) Al x M y The first layer is composed of N, where M is selected from the group consisting of zirconium, hafnium, elements from Group 5 of the periodic table, elements from Group 6 of the periodic table, silicon, and boron. This allows the first layer to possess excellent strength.
[0114] In the first layer 12 mentioned above, x and y vary along the thickness direction of the first layer 12, and the maximum value of x is x. max The minimum value of x is greater than 0.20 and less than 0.70. min If x is greater than 0 and less than 0.6, then x max and the x min Satisfying 0.01≤x max -x min ≤0.7, the maximum value of y is... max The minimum value of y is greater than 0.01 and less than 0.20. min If the value is above 0 and below 0.19, then y max and the y min Satisfying 0.01≤y max -y min ≤0.2. Therefore, this is due to Ti. (1-x-y) Al x M y The lattice constant of N is difficult to be uniform, and particle growth is suppressed in the aforementioned first layer 12. Therefore, this first layer 12 can form a fine structure. As a result, the cutting tool 10 equipped with a coating 40 containing such a first layer 12 can have superior film strength.
[0115] In addition, the above x max Preferably, the value is 0.25 or higher, more preferably 0.3 or higher, and even more preferably 0.35 or higher. The above x max Preferably, it is 0.65 or less, more preferably 0.6 or less, and even more preferably 0.55 or less. The above x maxPreferably, the value is 0.25 or higher and 0.65 or lower, more preferably 0.3 or higher and 0.6 or lower, and even more preferably 0.35 or higher and 0.55 or lower.
[0116] In addition, the above x min Preferably, it is 0.05 or more, more preferably 0.1 or more, and even more preferably 0.15 or more. Furthermore, the above-mentioned x... min Preferably, it is 0.57 or less, more preferably 0.54 or less, and even more preferably 0.50 or less. Additionally, the above x... min Preferably, the value is 0.05 or more and 0.57 or less, more preferably 0.1 or more and 0.54 or less, and even more preferably 0.15 or more and 0.50 or less.
[0117] In addition, the above y max Preferably, it is 0.015 or more, more preferably 0.02 or more, and even more preferably 0.025 or more. Furthermore, the above-mentioned y... max Preferably, it is 0.18 or less, more preferably 0.16 or less, and even more preferably 0.14 or less. Additionally, the above-mentioned y... max Preferably, the value is 0.015 or more and 0.18 or less, more preferably 0.02 or more and 0.16 or less, and even more preferably 0.025 or more and 0.14 or less.
[0118] In addition, the above y min Preferably, it is 0.005 or more, more preferably 0.01 or more, and even more preferably 0.015 or more. Furthermore, the above-mentioned y... min Preferably, it is 0.17 or less, more preferably 0.15 or less, and even more preferably 0.13 or less. Additionally, the above-mentioned y... min Preferably, the value is 0.005 or more and 0.17 or less, more preferably 0.01 or more and 0.15 or less, and even more preferably 0.015 or more and 0.13 or less.
[0119] In addition, the above x max -x min Preferably, it is 0.05 or more, more preferably 0.1 or more, and even more preferably 0.15 or more. The above x max -x min Preferably, it is 0.6 or less, more preferably 0.5 or less, and even more preferably 0.4 or less. The above x max -x min Preferably, the value is 0.05 or more and 0.6 or less, more preferably 0.1 or more and 0.5 or less, and even more preferably 0.15 or more and 0.4 or less.
[0120] In addition, the above y max -y minPreferably, it is 0.015 or more, more preferably 0.02 or more, and even more preferably 0.025 or more. Furthermore, the above-mentioned y... max -y min Preferably, it is 0.18 or less, more preferably 0.16 or less, and even more preferably 0.15 or less. Additionally, the above-mentioned y... max -y min Preferably, the value is 0.015 or more and 0.18 or less, more preferably 0.02 or more and 0.16 or less, and even more preferably 0.025 or more and 0.15 or less.
[0121] The above x max The above x min The above y max and the aforementioned y min The following can be used to determine the composition of the Ti layer. First, using Auger electron spectroscopy along the thickness direction of the first layer from the back face of the coating, the composition of the first layer of Ti is determined. (1-x-y) Al x M y The types of elements represented by M in N and their atomic concentration ratios, as well as the atomic concentration ratio of Al, were determined. Analytical conditions and ion sputtering (Ar) were used. + The conditions are as follows.
[0122] (Analysis conditions)
[0123] Energy of a primary electron: 10 keV
[0124] Current: Approximately 3nA
[0125] Incident angle: 0 degrees relative to the normal of the specimen's back face.
[0126] Analysis area: approximately 10 μm × 10 μm
[0127] (Ion sputtering (Ar) + ) conditions)
[0128] Energy: 1keV
[0129] Incident angle: approximately 0 degrees relative to the normal of the sample's back face.
[0130] Sputtering rate: approximately 2 nm / min
[0131] Perform the above measurements at any 5 points. Calculate x based on the average of the measured atomic concentration ratios at these 5 points. max y max x min y min Additionally, it is also possible to determine the type of element represented by M.
[0132] In this specification, "in the first layer, x and y change along the thickness direction of the first layer" is a concept that includes both the manner of "in the first layer, x and y change periodically along the thickness direction of the first layer with the same period width" and the manner of "in the first layer, x and y change periodically along the thickness direction of the first layer with the same period width".
[0133] In the first layer described above, where x and y vary periodically along the thickness direction of the first layer with the same period width, the average of the period width can be set to be 1 nm or more and 500 nm or less. The average of the period width is determined by the aforementioned x... max y max x min y min The periodicity of x and y is determined by plotting the curves with the horizontal axis representing the depth of the first layer and the vertical axes representing the concentrations of x and y.
[0134] In the first layer described above, when x and y vary periodically along the thickness direction of the first layer with the same periodic width, the aforementioned x max and the above y max Preferably, it is the maximum value of x and the maximum value of y in each of the aforementioned period widths. Furthermore, the aforementioned x... min and the above y min Preferably, the minimum values of x and y are the respective minimum values of the aforementioned period widths. Thus, the first layer 12 can form a further finer structure. As a result, the cutting tool 10 equipped with a coating 40 containing such a first layer 12 can have superior film strength.
[0135] In the cutting tool of this embodiment, the aforementioned period width may also be composed of a first-1 region (not shown) and a first-2 region (not shown) stacked along the thickness direction of the first layer, wherein in the first-1 region, x is the maximum value x. max Furthermore, the above y is the maximum value y. max In this first-second region, the aforementioned x is the minimum value x. min Furthermore, the aforementioned y is the minimum value y. min .use Figure 7 The relationship between the depth of the first layer and x and y in this case is explained.
[0136] exist Figure 7 In the graph, the horizontal axis represents the depth of the first layer, and the vertical axis represents the concentrations x and y. The intersection of the vertical and horizontal axes is the location of the first layer closest to the surface of the coating, that is, the location where the depth of the first layer is 0 μm. This location of 0 μm depth in the first layer is... Figure 7This is denoted as A1. In the region from depth 0 μm (A1) to depth A2 μm in the first layer, the above x represents the maximum value x. max Furthermore, the above y is the maximum value y. max This region corresponds to region 1-1. Within the region at depth A2μm to depth A3μm, the aforementioned x is the minimum value x. min Furthermore, the aforementioned y is the minimum value y. min This region corresponds to regions 1-2. Furthermore, in the region from depth A3μm to depth A4μm, the aforementioned x is the maximum value x. max Furthermore, the above y is the maximum value y. max This region corresponds to region 1-1. In the region from depth A4μm to depth A5μm, the aforementioned x is the minimum value x. min Furthermore, the aforementioned y is the minimum value y. min This area is equivalent to area 1-2.
[0137] exist Figure 7 In this context, the sum of the depths of an adjacent set of regions 1-1 and 1-2, i.e., the distance W1 from depth 0 μm (A1) to depth A3 μm, or the distance W1 from depth A3 μm to depth A5 μm, is equivalent to the aforementioned period width.
[0138] In the cutting tool of this embodiment, the aforementioned period width may also be composed of a first-1 region (not shown) and a first-2 region (not shown) stacked along the thickness direction of the first layer, wherein in the first-1 region, x is the maximum value x. max Furthermore, the aforementioned y is the minimum value y. min In this first-second region, the aforementioned x is the minimum value x. min Furthermore, the above y is the maximum value y. max .use Figure 8 The relationship between the depth of the first layer and x and y in this case is explained.
[0139] exist Figure 8 In the graph, the horizontal axis represents the depth of the first layer, and the vertical axis represents the concentrations x and y. The intersection of the vertical and horizontal axes is the location of the first layer closest to the surface of the coating, that is, the location where the depth of the first layer is 0 μm. This location of 0 μm depth in the first layer is... Figure 8 This is denoted as B1. In the region from depth 0 μm (B1) to depth B2 μm in the first layer, the above x represents the maximum value x. max Furthermore, the aforementioned y is the minimum value y. min This region corresponds to region 1-1. Within the region at depth B2μm to depth B3μm, the aforementioned x is the minimum value x. min Furthermore, the above y is the maximum value y. maxThis region corresponds to regions 1-2. Furthermore, in the region from depth B3 to depth B4 μm, the aforementioned x represents the maximum value x. max Furthermore, the aforementioned y is the minimum value y. min This region corresponds to region 1-1. Within the region at depth B4μm to depth B5μm, the aforementioned x is the minimum value x. min Furthermore, the above y is the maximum value y. max This area is equivalent to area 1-2.
[0140] exist Figure 8 In this context, the sum of the depths of an adjacent set of regions 1-1 and 1-2, i.e., the distance W2 from depth 0 μm (B1) to depth B3 μm, or the distance W2 from depth B3 μm to depth B5 μm, is equivalent to the aforementioned period width.
[0141] (Crystal size)
[0142] In the first layer described above, the average crystallite size is preferably 5 nm or more and 90 nm or less. This miniaturization of the crystallite size further enhances the strength of the coating containing the first layer. Furthermore, it suppresses the reduction in toughness of the first layer caused by excessively small crystallite sizes, thus suppressing crack formation in the first layer. The average crystallite size is preferably 8 nm or more, more preferably 12 nm or more, and even more preferably 15 nm or more. The average crystallite size is preferably 80 nm or less, more preferably 70 nm or less, and even more preferably 60 nm or less. The average crystallite size is more preferably 8 nm or more and 80 nm or less, more preferably 12 nm or more and 70 nm or less, and even more preferably 15 nm or more and 60 nm or less.
[0143] The average crystallite size mentioned above can be determined, for example, by X-ray diffraction (XRD) measurement under the following conditions. Specifically, first, the surface of the above-mentioned coating is irradiated with X-rays, and X-ray diffraction (XRD) measurement is performed to measure the full width at half maximum (FWHM). By substituting this full width at half maximum β into the Scherrer formula shown in (I) below, the crystallite size γ is derived.
[0144] γ=Kλ / βcosθ(I)
[0145] Here, K represents the shape factor. Additionally, in this specification, K is "0.9". Furthermore, λ refers to the X-ray wavelength. Furthermore, β refers to the Full Width Half Maximum (FWHM), expressed in radians. Furthermore, θ refers to the Bragg angle of the (200) peak of the first layer. It should be noted that this measurement is performed at five arbitrarily selected locations. Next, the average crystallite size is calculated by averaging the crystallite size at the five measurement locations. Furthermore, in cases where the coating includes a surface layer (other layers), the XRD measurement is performed after exposing the first layer.
[0146] (Conditions for X-ray diffraction measurement)
[0147] Scan axis: 2θ-θ
[0148] X-ray source: Cu-Kα rays
[0149] Detector: 0-dimensional detector (scintillation counter)
[0150] Tube voltage: 45kV
[0151] Tube current: 40mA
[0152] Incident optical system: using a mirror
[0153] Light-receiving optical system: utilizing an analyzer crystal (PW3098 / 27)
[0154] Step size: 0.03°
[0155] Total time: 2 seconds
[0156] Scan range (2θ): 10°~120°
[0157] It has been confirmed that, even if different measurement points are arbitrarily selected and the above measurements are performed at those measurement points, the same results can be obtained in the same cutting tool.
[0158] (Residual stress in the first layer)
[0159] The residual stress of the first layer is preferably -3.0 GPa or higher and -0.1 GPa or lower. This further improves the film strength of the cutting tool. Furthermore, the residual stress of the first layer is preferably -2.8 GPa or higher, more preferably -2.5 GPa or higher, and even more preferably -2.2 GPa or higher. The residual stress of the first layer is preferably -0.2 GPa or lower, more preferably -0.3 GPa or lower, and even more preferably -0.4 GPa or lower. It should be noted that when the residual stress is negative, this residual stress refers to "compressive residual stress".
[0160] <Method for determining residual stress in the first layer>
[0161] The aforementioned residual stress can be determined using the 2θ-sin²ψ method (tilt method) with X-rays. Specifically, the measurement conditions are as follows. For example, for any three points on the back face of the first layer, the first layer is analyzed using the 2θ-sin²ψ method (tilt method) with X-rays, and the average value of the residual stresses obtained at these three points is taken as the residual stress in the first layer. Furthermore, in the case where the coating includes a surface layer (other layers), the above XRD measurement is performed after exposing the first layer.
[0162] It has been confirmed that, even if different measurement points are arbitrarily selected and the above measurements are performed at those measurement points, the same results can be obtained in the same cutting tool.
[0163] (Measurement conditions)
[0164] Tube voltage: 45kV
[0165] Tube current: 200mA
[0166] X-ray source: Cu-Kα rays
[0167] Incident optical system: collimator
[0168] Peak used: TiN(2,0,0)
[0169] (The ratio of the X-ray diffraction intensity of the (200) plane of the first layer to the sum of the X-ray diffraction intensity of the (200) plane of the first layer, the X-ray diffraction intensity of the (111) plane of the first layer, and the X-ray diffraction intensity of the (220) plane of the first layer)
[0170] X-ray diffraction intensity I relative to the (200) plane of the first layer mentioned above (200) The X-ray diffraction intensity I of the (111) plane of the first layer mentioned above (111) X-ray diffraction intensity I of the (220) plane of the first layer mentioned above (220) The total of the above I (200) The ratio I (200) / (I (200) +I (111) +I (220) The preferred value is 0.50 or higher. This improves the toughness of the coating, inhibits crack propagation, and thus further enhances the peel resistance of the coating. It should be noted that the X-ray diffraction intensity I of the (200) plane... (200) "" refers to the diffraction intensity (peak height) of the highest peak among the X-ray diffraction peaks from the (200) plane (hereinafter also referred to as "maximum diffraction intensity"). Furthermore, when two or more compounds contained in the coating each have X-ray diffraction peaks from the (200) plane, that is, when multiple X-ray diffraction peaks from the (200) plane exist at different locations, "the X-ray diffraction intensity I of the (200) plane" (200) "" refers to the sum of their maximum diffraction intensities (peak heights). For the X-ray diffraction intensity I of plane "(111) (111) "and "X-ray diffraction intensity I of plane (220) (220) The same applies to "".
[0171] In addition, the above I (200) / (I (200) +I (111) +I (220) Preferably, it is 0.53 or higher, more preferably 0.56 or higher, and even more preferably 0.60 or higher. Furthermore, the above-mentioned I... (200) / (I (200) +I (111) +I (220) Preferably, it is 0.97 or less, more preferably 0.94 or less, and even more preferably 0.90 or less. Furthermore, the above-mentioned I... (200) / (I (200) +I (111) +I (220) More preferably, the value is 0.53 or more and 0.97 or less, even more preferably 0.56 or more and 0.94 or less, and even more preferably 0.60 or more and 0.90 or less.
[0172] The above I (200) The above I (111) and the aforementioned I (220) For example, it can be determined by X-ray diffraction (XRD) measurements performed under the following conditions. Specifically, the above I...(200) The above I (111) and the aforementioned I (220) The X-ray diffraction (XRD) measurement was performed by irradiating the surface of the aforementioned coating with X-rays. It should be noted that the measurement was performed at five arbitrarily selected locations on the back face. Then, the I values at the measurement locations of the five locations were calculated. (200) The above I (111) and the aforementioned I (220) Their respective average values. Next, based on I... (200) The average value of I (111) The average value and I (220) The average value of I can be used to calculate the above I. (200) / (I (200) +I (111) +I (220) ).
[0173] (Conditions for X-ray diffraction measurement)
[0174] Scan axis: 2θ-θ
[0175] X-ray source: Cu-Kα rays
[0176] Detector: 0-dimensional detector (scintillation counter)
[0177] Tube voltage: 45kV
[0178] Tube current: 40mA
[0179] Incident optical system: using a mirror
[0180] Light-receiving optical system: utilizing an analyzer crystal (PW3098 / 27)
[0181] Step size: 0.03°
[0182] Total time: 2 seconds
[0183] Scan range (2θ): 10°~120°
[0184] It has been confirmed that, even if different measurement ranges are arbitrarily selected and the above measurements are performed within those ranges, the same results can be obtained using the same cutting tool.
[0185] <Basal layer>
[0186] The aforementioned coating also includes a base layer, which is preferably made of Ti. a Al 1-a N or Al p Cr 1-pN is formed. In this case, it is preferable that the base layer is disposed directly above the substrate and directly below the first layer. This improves the adhesion between the substrate and the coating.
[0187] The thickness of the aforementioned substrate layer is preferably 0.05 μm or more and 1.0 μm or less. This further improves the adhesion between the substrate and the coating. This is because if the substrate layer is too thin, it tends to be difficult to improve the adhesion between the substrate and the coating; conversely, if the substrate layer is too thick, it tends to hinder the improvement of film strength resulting from the miniaturization of particles in the first layer. Furthermore, the thickness of the aforementioned substrate layer is preferably 0.10 μm or more, more preferably 0.15 μm or more, and even more preferably 0.20 μm or more. Furthermore, the thickness of the aforementioned substrate layer is preferably 0.80 μm or less, more preferably 0.60 μm or less, and even more preferably 0.40 μm or less. Furthermore, the thickness of the aforementioned substrate layer is preferably 0.10 μm or more and 0.80 μm or less, more preferably 0.15 μm or more and 0.60 μm or less, and even more preferably 0.20 μm or more and 0.40 μm or less.
[0188] The aforementioned a is preferably 0.2 or more and 1.0 or less. This improves adhesion to the substrate and enhances the peel resistance of the coating. The aforementioned a is preferably 0.3 or more and 0.9 or less, more preferably 0.4 or more and 0.8 or less, and even more preferably 0.5 or more and 0.7 or less.
[0189] The value of p is preferably 0 or higher and 0.8 or lower. This improves adhesion to the substrate and enhances the peel resistance of the coating. The value of p is preferably 0.1 or higher and 0.77 or lower, more preferably 0.2 or higher and 0.74 or lower, and even more preferably 0.3 or higher and 0.7 or lower.
[0190] The values of 'a' and 'p' mentioned above can be determined as follows. First, cut the sample at any point using a cutting tool to create a cross-section containing the coating. This sample can be prepared using a focused ion beam apparatus, a cross-section polishing machine, or similar equipment. Next, the values can be determined by elemental analysis of the sample using energy-dispersive X-ray spectroscopy (EDX), which is integrated into a SEM.
[0191] <Other Layers>
[0192] Provided that the effect of this embodiment is not compromised, the coating may further include the other layers described above. For example... Figures 4-6 As shown, other layers mentioned above may include, for example, intermediate layer 14 and surface layer 15.
[0193] (Middle layer)
[0194] In this embodiment, the coating can, for example, be between adjacent first layers 12 ( Figure 4 ), or between the adjacent first layer 12 and surface layer 15 ( Figure 5 The system includes an intermediate layer 14. The intermediate layer 14 is disposed between the first layer 12 and other layers (such as the surface layer 15) other than the first layer 12. The composition of the intermediate layer can be, for example, titanium nitride (TiN), titanium carbonitride (TiCN), titanium aluminum nitride (TiAlN), titanium aluminum silicon nitride (TiAlSiN), titanium aluminum boron nitride (TiAlBN), titanium aluminum zirconium nitride (TiAlZrN), titanium aluminum hafnium nitride (TiAlHfN), titanium aluminum vanadium nitride (TiAlVN), titanium aluminum niobium nitride (TiAlNbN), titanium aluminum tantalum nitride (TiAlTaN), titanium aluminum chromium nitride (TiAlCrN), titanium aluminum molybdenum nitride (TiAlMoN), or titanium aluminum tungsten nitride (TiAlWN). Furthermore, the thickness of the intermediate layer can be, for example, 0.2 μm or more and 1 μm or less.
[0195] (Surface layer)
[0196] The coating in this embodiment may include a surface layer ( Figure 6 Surface layer 15 is the layer disposed on the outermost side of the coating 40. However, there are also cases where surface layer 15 is not formed at the blade tip edge.
[0197] As a surface layer 15, a TiN layer can be cited as an example. The TiN layer has a bright color (golden color), so if it is used as a surface layer 15, it has the advantage of making it easy to identify the corners of the cutting tool after cutting (identification of the used parts).
[0198] The thickness of the surface layer 15 can be, for example, greater than 0.01 μm and less than 0.3 μm.
[0199] [Implementation Method 2: Method for Manufacturing a Cutting Tool]
[0200] The manufacturing method of the cutting tool according to Embodiment 1 will be described below. It should be noted that the following manufacturing method is an example, and the cutting tool of Embodiment 1 can also be manufactured by other methods.
[0201] The method for manufacturing the cutting tool involved in this embodiment includes:
[0202] The first process for preparing the aforementioned substrate (hereinafter sometimes simply referred to as the "first process"); and
[0203] The third step (hereinafter, sometimes simply referred to as the "third step") involves forming the aforementioned coating on the substrate. Furthermore, this manufacturing method may further include a second step (hereinafter, sometimes simply referred to as the "second step") involving ion bombardment treatment of the surface of the substrate obtained through the first step and / or a fourth step (hereinafter, sometimes simply referred to as the "fourth step") involving dry sandblasting treatment of the surface of the coating obtained through the third step. Each step will be described below.
[0204] First step: Preparing the substrate
[0205] In the first step, the aforementioned substrate is prepared. As described above, any substrate conventionally known as such can be used as the substrate. For example, a substrate with the shape of ISO standard DNGA150408, made of cemented carbide material (equivalent to K10), is prepared. A substrate made of cubic boron nitride sintered body (shape: a triangular prism with a base of an isosceles triangle with a 55° apex and two 2mm sides surrounding the apex, and a thickness of 2mm) is joined to the tip (corner) portion of this substrate, thereby obtaining a joint. It should be noted that a brazing filler metal of Ti-Zr-Cu is used for joining. Next, the outer peripheral surface, upper surface, and lower surface of the joint are ground to form a negative cutting edge shape at the tip (the negative cutting edge width is 150μm, and the negative cutting edge angle is 25°). In this way, a substrate with a tip (cutting edge) made of cubic boron nitride sintered body can be obtained.
[0206] As described above, when grinding the outer peripheral surface, upper surface, and negative cutting edge of the joint, it is preferable to use a fine-grained grinding stone with a grit size of #700 or higher. Using a grinding stone smaller than #700 can easily result in unevenness caused by grinding marks, thus creating Rsk (grit defects). sub The absolute value of Rsk is trending towards increasing. Previously, it was believed that to improve the adhesion between the substrate and the coating, Rsk... sub Preferably, it is a certain size or larger. The inventors of this invention conducted in-depth research and found that when Rsk... sub When the value is -2 or higher and 2 or lower, the deviation in the distribution of peaks and valleys on the surface of the substrate in contact with the coating becomes smaller, which improves the adhesion between the substrate and the coating and reduces stress concentration caused by the load during processing, thus improving the peel resistance of the coating. Furthermore, the inventors of this invention have newly discovered that by using a fine-textured grinding stone with a grit size of #700 or higher, Rsk... sub It is greater than -2 and less than 2.
[0207] The second process: ion bombardment treatment of the substrate surface.
[0208] In the second step, the surface of the substrate is subjected to ion bombardment treatment. For example, firstly, the substrate is placed in the vacuum chamber of the film-forming apparatus. Next, the chamber is evacuated. Then, the substrate is heated to 500°C while the rotary table rotates at 3 rpm. Next, Ar gas is introduced into the vacuum chamber, causing a tungsten filament to discharge and generate Ar ions. A bias voltage is applied to the substrate, and the substrate is subjected to ion bombardment treatment using Ar ions under the following conditions.
[0209] (Conditions for ion bombardment treatment)
[0210] Pressure of Ar gas: 1 Pa
[0211] Substrate bias voltage: -600V to -1000V
[0212] Processing time: 10 to 45 minutes
[0213] Therefore, the above Rsk can be made sub It is greater than -2 and less than 2.
[0214] The inventors of this invention have discovered that by subjecting the surface of a substrate to ion bombardment treatment under the conditions described above, it is possible to remove Rsk sub Set it to the desired value.
[0215] The third process: forming a coating on the substrate.
[0216] In the third step, a coating is formed on the substrate. Additionally, the third step includes a "first layer coating step" in which a first layer is applied to at least a portion of the surface of the ion-bombarded substrate.
[0217] As a method of covering at least a portion of the aforementioned substrate with a first layer, physical vapor deposition (PVD) can be cited as an example.
[0218] Examples of PVD methods include AIP (Area-in-Place) plating (ion plating, which uses vacuum arc discharge to evaporate solid materials) and sputtering. For instance, when fabricating a TiAlSiN layer using AIP, a TiAlSi target as the metal evaporation source and N2 as the reactive gas can be used. Conversely, when fabricating a TiAlSiN layer using sputtering, a TiAlSi target as the metal evaporation source and sputtering gases such as N2, Ar, Kr, or Xe can be used as the reactive gas. Furthermore, the substrate temperature can be set to 300°C to 800°C, and the gas pressure can be set to 0.1 to 10 Pa.
[0219] The aforementioned first layer coating process includes one or both of the steps of process (i) of varying the bias voltage during film formation and process (ii) of preparing two target compositions and performing simultaneous evaporation. The inventors of this invention conducted in-depth research and discovered that this allows the aforementioned x and y to vary along the thickness direction of the first layer.
[0220] The above process (i) can be performed, for example, by using a TiAlSi target as the target and by discontinuously varying the bias voltage between 35V and 50V.
[0221] The above process (ii) can be performed, for example, by using a TiAlSi target and a TiAlN target as two targets and fixing the bias voltage to 30V.
[0222] The third step described above, in addition to the first layer covering step, may also include steps for forming other layers such as a base layer and a surface layer. These other layers can be formed using existing methods. It should be noted that the "step for forming the base layer" will sometimes be referred to as step (iii) below.
[0223] Fourth step: Dry sandblasting the coated surface.
[0224] In the fourth step, the surface of the coating obtained in the third step is subjected to dry sandblasting. For example, the fourth step is performed by dry sandblasting under the following conditions: the rake face, flank face, and negative edge face of the coating obtained in the third step are projected at a distance of 100 mm, with a projection angle adjusted to approximately 15 to 70 degrees, for a period of 60 to 120 seconds using an elastic abrasive medium containing diamond abrasive grains. This allows the surface roughness Ra of the coating to be increased. surf The thickness is greater than 0 μm and less than 0.1 μm, and the skewness Rsk of the coated surface is [not specified]. surf The value is between -2 and 2. It should be noted that when the projection angle relative to the sandblasted surface exceeds 70 degrees, the surface roughness and unevenness of the coated surface decrease, making coating removal easier, thus making it difficult to achieve the desired coating effect. Furthermore, when the projection angle is less than 15 degrees, it is difficult to obtain the grinding effect of the elastic abrasive media, thus making it difficult to reduce the surface roughness of the coated surface.
[0225] As described above, the inventors of this invention have discovered that by dry sandblasting the surface of the coating, Ra can be achieved. surf For sizes greater than 0 μm and less than 0.1 μm, and for Rsk surf It is greater than -2 and less than 2.
[0226] Other processes
[0227] In the manufacturing method described in this embodiment, in addition to the steps described above, for example, a step of treating the surface of the film can be performed by a method other than the fourth step described above.
[0228] Example
[0229] The present invention will be described in detail below with reference to specific embodiments, but the present invention is not limited to these embodiments.
[0230] Making Cutting Tools
[0231] [Sample No. 1 to Sample No. 48, and Sample No. 101 to Sample No. 104]
[0232] The cutting tools for specimens No.1 to No.48 and specimens No.101 to No.104 were manufactured using the following manufacturing method.
[0233] <First step: Preparing the substrate>
[0234] First, a substrate of ISO standard DNGA150408 shape, made of cemented carbide material (equivalent to K10), is prepared. Next, a cubic boron nitride sintered substrate (shape: a 2mm thick triangular prism with an isosceles triangle base of 55° apex angle and 2mm sides surrounding the apex angle) is joined to the tip portion (corner portion) of this substrate, thereby obtaining a bond. It should be noted that a Ti-Zr-Cu brazing filler metal is used for the joining. Next, the outer peripheral surface, upper surface, and lower surface of the bond are ground to form a negative cutting edge shape at the tip (negative cutting edge width 150μm, negative cutting edge angle 25°). Grinding is performed using a grinding stone with the grit number shown in the "Grinding Stone" column of "First Process" in Tables 1 and 2. In this way, a matrix composed of cubic boron nitride sintered body is obtained for the tip (cutting edge) portion.
[0235]
[0236]
[0237] The second process: ion bombardment treatment of the substrate surface.
[0238] The substrate was placed in the vacuum chamber of the film-forming apparatus. Next, the chamber was evacuated. Then, the substrate was heated to 500°C while the rotary table rotated at 3 rpm. Next, Ar gas (pressure: 1 Pa) was introduced into the vacuum chamber, causing a tungsten filament to discharge and generate Ar ions. A bias voltage was applied to the substrate, and the substrate was subjected to ion bombardment treatment using these Ar ions. It should be noted that the bias voltage and time for the ion bombardment treatment are shown in the "Bias Voltage" and "Time" columns of "Second Step" in Tables 1 and 2.
[0239] The third process: forming a coating on the substrate.
[0240] <Process (iii): Process for forming the base layer>
[0241] Next, in samples No. 40 to No. 45, in order to form a base layer on the surface of the above-mentioned substrate, an arc ion plating method was used, and step (iii) was performed under the conditions of the target recorded in the "Target" column of "Step to Form Base Layer" in Table 2 and the bias voltage recorded in the "Bias Voltage" column of "Step to Form Base Layer" in Table 2.
[0242] <First Layer Covering Process>
[0243] Next, an arc ion plating method is used to form a first layer on the surface of the substrate or the base layer. The above process (i) is performed in samples No.1 to No.10, and the above process (ii) is performed in samples No.11 to No.48 and samples No.101 to No.104.
[0244] In step (i), the target listed in the "Target" column of "Step (i)" under "First Layer Covering Step" in Tables 1 and 2, along with N2 gas as the reactant gas, are used to perform the first layer covering step with the bias voltage listed in the "Bias Voltage" column. The 30 / 150 listed in the "Bias Voltage" column refers to the discontinuous switching between bias voltages of 30V and 150V. More specifically, the bias voltage is maintained at 30V for 120 seconds, then switched to 150V and maintained for 120 seconds, and this switching is repeated as one cycle. That is, one cycle lasts 240 seconds.
[0245] In step (ii), the first layer coating process is performed using the two targets listed in the "Target" column of "Step (ii)" under "First Layer Coating Process" in Tables 1 and 2, N2 gas as the reactant gas, and the bias voltage listed in the "Bias Voltage" column. For example, in sample No. 11, TiAlSi and TiAl are used as targets, N2 gas is used as the reactant gas, and the bias voltage is set to 30V.
[0246] It should be noted that in sample No. 31, both targets are "TiAlSi" targets, but the composition ratio of one target (Ti∶Al∶Si=30∶50∶20) is different from that of the other target (Ti∶Al∶Si=32∶49∶19). That is, two types of targets were used in sample No. 31.
[0247] It should be noted that in sample No. 23, both targets were "TiAlB" targets, but the composition ratio of one target (Ti∶Al∶B=30∶50∶20) differed from that of the other target (Ti∶Al∶B=32∶49∶19). That is, two types of targets were used in sample No. 23.
[0248] In addition, in sample No. 102, both targets were "TiAlB" targets. The composition ratio of one target was Ti:Al:B = 40:50:10, and the composition ratio of the other target was Ti:Al:B = 50:40:10.
[0249] Furthermore, while Samples No. 12, No. 101, No. 103, and No. 104 share the commonality of using both "TiAlB" and "TiAl" targets, they differ in the target composition ratios, as described below. In Sample No. 12, the composition ratio of the "TiAlB" target is Ti:Al:B = 50:48:2, and the composition ratio of the "TiAl" target is Ti:Al = 50:50. Similarly, in Sample No. 101, the composition ratio of the "TiAlB" target is Ti:Al:B = 48:50:2, and the composition ratio of the "TiAl" target is Ti:Al = 50:50. Finally, in Samples No. 103 and No. 104, the composition ratio of the "TiAlB" target is Ti:Al:B = 50:48:2, and the composition ratio of the "TiAl" target is Ti:Al = 50:50.
[0250] Fourth step: Dry sandblasting the coated surface.
[0251] Next, in order to prepare specimens No.1 to No.38, No.40 to No.48, and No.101 to No.104, sandblasting was performed on the machined surfaces (rake face, flank face, and negative cutting edge surface) of the coated surface obtained in the third process, under the conditions described in Tables 1 and 2. The sandblasting was performed under the following conditions: for the coated rake face, flank face, and negative cutting edge surface, the projection distance was 100 mm, the projection angle was adjusted to approximately 15 to 70 degrees, and the sandblasting was performed using an elastic abrasive medium with diamond abrasive grains for 60 seconds.
[0252] By performing the above procedures, cutting tools for specimens No.1 to No.48 and specimens No.101 to No.104 with the configurations shown in Tables 3 and 4 are manufactured.
[0253] Evaluation of Cutting Tool Characteristics
[0254] Using the cutting tools of specimens No. 1 to No. 48 and specimens No. 101 to No. 104, which were prepared as described above, the characteristics of the cutting tools were evaluated as follows. It should be noted that the cutting tools of specimens No. 1 to No. 48 correspond to the examples, and the cutting tools of specimens No. 101 to No. 104 correspond to the comparative examples.
[0255] <x max x min y max y min The determination of a and p, and the determination of M.
[0256] For the cutting tools of samples No. 1 to No. 48 and samples No. 101 to No. 104, the Ti in the first layer was determined by the method described in Embodiment 1. (1-x-y) Al x M y The types of "M" in N, "x" max “x” min “y” max "and "y min Ti in the basal layer a Al 1-a N or Al p Cr 1-p N's "a" and "p". In the results obtained, "M" and "x" will be included. max “x” min “y” max “y” min "M" and "x" are recorded in Table 3 and Table 4 respectively. max "One item, "x min "One item, "y max "One item, "y min In addition, the results of “a” and “p” are recorded in the “a” and “p” items of Table 3 and Table 4, respectively.
[0257]
[0258]
[0259] <Determination of the thickness of the first layer and the base layer>
[0260] For the cutting tools of samples No. 1 to No. 48 and samples No. 101 to No. 104, the thickness of the first layer was determined using the method described in Embodiment 1. The results are recorded in the "Thickness of the First Layer [μm]" field of Tables 3 and 4, respectively. Furthermore, for the cutting tools of samples No. 40 to No. 45, the thickness of the base layer was determined using the method described in Embodiment 1. The results are recorded in the "Thickness of the Base Layer [μm]" field of Tables 3 and 4, respectively.
[0261] <Measurement of the average size of microcrystals in the first layer>
[0262] For the cutting tools of samples No. 1 to No. 48 and samples No. 101 to No. 104, the average crystallite size of the first layer was determined by the method described in Embodiment 1. The results obtained are recorded in the "Crystallite Size [nm]" field of Tables 3 and 4, respectively.
[0263] <Determination of Residual Stress in the First Layer>
[0264] For the cutting tools of specimens No.1 to No.48 and specimens No.101 to No.104, the residual stress of the first layer was determined by the method described in Embodiment 1. The results obtained are recorded in the "Residual Stress [GPa]" column of Tables 3 and 4, respectively.
[0265] <Rsk sub Ra surf and Rsk surf Measurement>
[0266] For the cutting tools of specimens No. 1 to No. 48 and specimens No. 101 to No. 104, Rsk was determined by the method described in Embodiment 1. sub The results obtained are recorded in Tables 3 and 4, respectively, under "Rsk". sub "In addition, for the cutting tools of specimens No.1 to No.39 and specimens No.101 to No.104, Ra was determined by the method described in Embodiment 1." surf The results obtained are recorded in Tables 3 and 4, respectively, under the heading "Ra". surf In the "[μm]" section, Rsk was determined for the cutting tools of samples No. 1 to No. 48 and samples No. 101 to No. 104 using the method described in Embodiment 1. surf The results obtained are recorded in Tables 3 and 4, respectively, under "Rsk". surf "In one item."
[0267] (200) / (I (200) +I (111) +I (220) The determination of )
[0268] For the cutting tools of samples No. 1 to No. 48 and samples No. 101 to No. 104, the I of the first layer is determined by the method described in Embodiment 1. (200) / (I (200) +I (111) +I (220) The results obtained are recorded in Tables 3 and 4, respectively, under "R". (200) "In one item."
[0269] Cutting Test
[0270] The following cutting tests were conducted using the cutting tools of specimens No.1 to No.48 and specimens No.101 to No.104, which were prepared as described above.
[0271] For the cutting tools of specimens No. 1 to No. 48 and specimens No. 101 to No. 104, the workpiece was machined under the following cutting conditions. At a cutting distance of 50 m, the contacting cutting tools and the workpiece were temporarily separated. Then, after 3 seconds of separation, the workpiece was cut again under the following cutting conditions. This process was repeated until the cutting distance reached 4 km. Next, the maximum wear on the flank face of the cutting tool at the cutting distance of 4 km was measured. In cases of coating failure, wear tends to progress from the point of failure, thus tending to increase the maximum wear. Therefore, a smaller maximum wear means a longer tool life, even in high-efficiency machining. The maximum wear is recorded in the "Maximum Wear [μm]" field of Tables 3 and 4.
[0272] (Cutting conditions)
[0273] Workpiece to be machined: High-hardness steel SCM415 (HRC62) (diameter 100mm × length 300mm)
[0274] Cutting speed: V = 150 m / min.
[0275] Feed: f = 0.2 mm / rev.
[0276] Incision: ap = 0.5mm
[0277] Wet / Dry: Wet
[0278] This cutting condition is equivalent to high-efficiency machining.
[0279] <Results>
[0280] Samples No. 1 to No. 48 correspond to the Examples. Samples No. 101 to No. 104 correspond to the Comparative Examples. As can be seen from the results in Tables 3 and 4, the cutting tools of Samples No. 1 to No. 48, which correspond to the Examples, have a longer tool life even in high-efficiency machining compared to the cutting tools of Samples No. 101 to No. 104, which correspond to the Comparative Examples.
[0281] The embodiments and examples of this disclosure have been described above, but it is also intended from the outset that the above-described embodiments and examples may be appropriately combined or modified.
[0282] The embodiments and examples disclosed herein should be considered exemplary in all respects, and not restrictive. The scope of the invention is defined not by the foregoing embodiments and examples, but by the claims, and is intended to include all modifications equivalent to and within the scope of the claims.
[0283] Explanation of reference numerals in the attached figures
[0284] 1: Rake face; 2: Back face; 3: Tip edge; 10: Cutting tool; 11: Substrate; 12: First layer; 13: Base layer; 14: Intermediate layer; 15: Surface layer; 40: Coating; W1 and W2: Period width; A1~A5 and B1~B5: Depth of the first layer; L1: Average line.
Claims
1. A cutting tool comprising a substrate and a coating disposed on the substrate, wherein, The coating comprises a first layer. The thickness of the first layer is greater than 0.2 μm and less than 9 μm. The first layer consists of Ti (1-x-y) Al x M y N constitutes, M is an element selected from the group consisting of zirconium, hafnium, elements of Group 5 of the periodic table, elements of Group 6 of the periodic table, silicon, and boron. In the first layer, x and y vary along the thickness direction of the first layer. The maximum value of x is x max Values between 0.20 and 0.70 The minimum value of x min Values above 0 and below 0.
60. The x max With the x min Satisfying 0.01≤x max -x min ≤0.70, The maximum value of y is y max Values between 0.01 and 0.20 The minimum value of y min Values above 0 and below 0.
19. The y max With the y min Satisfying 0.01≤y max -y min ≤0.20, The values of x and y vary periodically along the thickness direction of the first layer with the same period width. The period width is formed by regions 1-1 and 1-2 stacked along the thickness direction of the first layer, respectively. In region 1-1, x is the maximum value x. max In this first-second region, x is the minimum value x. min , The surface roughness Ra of the coating surf It is above 0 μm and below 0.1 μm. The skewness Rsk of the surface of the coating surf It is above -2 and below 2. The skewness Rsk of the surface of the substrate in contact with the coating sub It is greater than -2 and less than 2.
2. The cutting tool according to claim 1, wherein, The thickness of the coating is greater than 0.4 μm and less than 8 μm.
3. The cutting tool according to claim 1 or 2, wherein, The thickness of the first layer is greater than 0.8 μm and less than 6 μm.
4. The cutting tool according to claim 1 or 2, wherein, The maximum value of x is x max It is above 0.35 and below 0.
55.
5. The cutting tool according to claim 1 or 2, wherein, The minimum value of x min It is above 0.15 and below 0.
50.
6. The cutting tool according to claim 1 or 2, wherein, The maximum value of y is y max It is above 0.025 and below 0.
14.
7. The cutting tool according to claim 1 or 2, wherein, The minimum value of y min It is above 0.005 and below 0.
17.
8. The cutting tool according to claim 1 or 2, wherein, The x max With the x min Satisfying 0.1≤x max -x min ≤0.
5.
9. The cutting tool according to claim 1 or 2, wherein, The y max With the y min Satisfying 0.02≤y max -y min ≤0.
16.
10. The cutting tool according to claim 1 or 2, wherein, In the first layer, the average crystallite size is above 5 nm and below 90 nm.
11. The cutting tool according to claim 10, wherein, The average size of the microcrystals is above 15 nm and below 60 nm.
12. The cutting tool according to claim 1, wherein, The coating also includes a base layer. The base layer is disposed directly above the substrate and directly below the first layer. The thickness of the substrate layer is greater than 0.05 μm and less than 1.0 μm. The base layer is made of Ti a Al 1-a N or Al p Cr 1-p N constitutes, The value of a is greater than 0.2 and less than 1.
0. The value of p is greater than or equal to 0 and less than or equal to 0.
8.
13. The cutting tool according to claim 12, wherein, The thickness of the substrate layer is greater than 0.20 μm and less than 0.40 μm.
14. The cutting tool according to claim 12 or 13, wherein, The value of a is greater than 0.5 and less than 0.
7.
15. The cutting tool according to claim 12 or 13, wherein, The value of p is greater than 0.2 and less than 0.
74.
16. The cutting tool according to claim 1 or 2, wherein, The residual stress of the first layer is above -3.0 GPa and below -0.1 GPa.
17. The cutting tool according to claim 1, wherein, The surface roughness Ra of the coating surf It is above 0.03μm and below 0.08μm.
18. The cutting tool according to claim 1, wherein, The skewness Rsk of the surface of the coating surf It is above -1.4 and below 1.
4.
19. The cutting tool according to claim 1, wherein, The skewness Rsk of the surface of the substrate in contact with the coating sub It is above -1.4 and below 1.
4.
20. The cutting tool according to claim 1 or 2, wherein, X-ray diffraction intensity I relative to the (200) plane of the first layer (200) X-ray diffraction intensity I of the (111) plane of the first layer (111) and the X-ray diffraction intensity I of the (220) plane of the first layer. (220) The total of the I (200) The ratio I (200) / (I (200) +I (111) +I (220) The value is above 0.
50.
21. The cutting tool according to claim 1 or 2, wherein, The substrate is a cubic boron nitride sintered body.
22. The cutting tool according to claim 1 or 2, wherein, The coating comprises a plurality of first layers, with an intermediate layer between adjacent first layers.
23. The cutting tool according to claim 1 or 2, wherein, A surface layer is provided on the outermost surface side of the coating.
Citation Information
Patent Citations
Combined material having high hardness for tool
JP1996119774A
Coated cutting tool
CN110944776A
Surface-coated cutting tool
JP2011224688A
Surface-coated cutting tool
WO2021085253A1