Antifouling coating composition and coating film

By adding specific resins and antifouling agents to the antifouling coating composition, combined with rosin compounds, the problem of insufficient antifouling performance in water of existing antifouling coatings is solved, and long-term and efficient antifouling effects are achieved.

CN117480220BActive Publication Date: 2024-10-18NIPPON PAINT MARINE COATINGS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180097840.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-19
Publication Date
2024-10-18
Estimated Expiration
2041-05-19

AI Technical Summary

Technical Problem

Existing antifouling coating compositions have insufficient antifouling properties after being used in water, resulting in early consumption of the coating film and inability to maintain efficient antifouling effects for a long time.

Method used

An antifouling coating composition containing a hydrolyzable resin, a first non-hydrolyzable resin, a second non-hydrolyzable resin and an antifouling agent is used. By adjusting the glass transition temperature and dissolution parameters of the resin, combined with rosin compounds, a long-term A coating that releases antifouling ingredients.

Benefits of technology

It achieves a coating film that maintains high antifouling performance for a long time in water, reduces the consumption rate of the coating film, and extends the duration of the antifouling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117480220B_ABST
    Figure CN117480220B_ABST
Patent Text Reader

Abstract

Provided is an antifouling coating composition, comprising a hydrolyzable resin (A), a first non-hydrolyzable resin (B), a second non-hydrolyzable resin (C) and an antifouling agent (D); wherein the glass transition temperature Tg of the first non-hydrolyzable resin (B) is B [℃] and dissolution parameter SP B , and the glass transition temperature Tg of the second non-hydrolyzable resin (C) C [℃] and dissolution parameter SP C Satisfies: Formula [1]: Tg B ‑Tg C ≥60, formula [2]: SP B ≥9.5, formula [3]: SP C ≥9.5 and formula [4]: ​​|SP B ‑SP C |≤1.0[4].
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an antifouling coating composition and a coating film, and also to a ship and an underwater structure having the coating film. Background Art

[0002] Aquatic organisms such as barnacles, mussels, and algae are easily attached to underwater structures, ships, and fishing nets. The attachment of these organisms may hinder efficient operation of ships and cause fuel waste. In addition, problems such as clogging or shortened service life may occur in fishing nets. Therefore, in the past, in order to prevent the attachment of aquatic organisms, an antifouling coating composition was applied to the surface to form an antifouling coating film.

[0003] As an antifouling coating composition, an antifouling coating composition containing a hydrolyzable resin (binder resin) having a triorganosilyl group and an antifouling agent has been used in the past [for example, International Publication No. 2020 / 235516 (Patent Document 1)]. The antifouling coating film formed by the antifouling coating composition can exhibit antifouling performance for a long time because the surface of the coating film is constantly renewed due to the slow hydrolysis of the triorganosilyl group in water.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2020 / 235516 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The present invention aims to provide an antifouling coating composition comprising a hydrolyzable resin and an antifouling agent, which can exhibit high antifouling performance for a long period of time. Another object of the present invention is to provide a coating film formed from the antifouling coating composition, and a ship and an underwater structure having the coating film.

[0009] Means of solving problems

[0010] The present invention provides the following antifouling coating composition, coating film, ship and underwater structure.

[0011] [1] An antifouling coating composition comprising a hydrolyzable resin (A), a first non-hydrolyzable resin (B), a second non-hydrolyzable resin (C) and an antifouling agent (D); wherein the glass transition temperature Tg of the first non-hydrolyzable resin (B) is B [℃] and dissolution parameter SP B , and the glass transition temperature Tg of the second non-hydrolyzable resin (C) C [℃] and dissolution parameter SP C Satisfies the following equations [1] to [4]:

[0012] Tg B -Tg C ≥60 [1]

[0013] SP B ≥9.5 [2]

[0014] SP C ≥9.5 [3]

[0015] |SP B -SP C |≤1.0 [4].

[0016] [2] The antifouling coating composition according to [1], wherein Tg B In the range of 40°C or more and 80°C or less, SP B It is in the range of 9.6 or more and 10.3 or less.

[0017] [3] The antifouling coating composition according to [1] or [2], wherein Tg C In the range of -50°C or higher and -20°C or lower, SP C It is in the range of 9.8 or more and 10.6 or less.

[0018] [4] The antifouling coating composition according to any one of [1] to [3], wherein the glass transition temperature Tg of the hydrolyzable resin (A) is A In the range of 10°C to 80°C, the dissolution parameter SP A It is in the range of 8.5 or more and 9.7 or less.

[0019] [5] The antifouling coating composition according to any one of [1] to [4], wherein the hydrolyzable resin (A) has a silicon atom-containing group represented by the following formula (1):

[0020] [Chemical formula 1]

[0021]

[0022] In formula (1), R 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 6 carbon atoms.

[0023] [6] The antifouling coating composition according to any one of [1] to [5], further comprising a rosin compound (E).

[0024] [7] The antifouling coating composition according to any one of [1] to [6], wherein the content ratio of the first non-hydrolyzable resin (B) to the hydrolyzable resin (A) is 0.1 to 0.45 in terms of mass ratio.

[0025] [8] The antifouling coating composition according to any one of [1] to [7], wherein the content ratio of the second non-hydrolyzable resin (C) to the hydrolyzable resin (A) is 0.05 to 0.65 in terms of mass ratio.

[0026] [9] The antifouling coating composition according to any one of [1] to [8], wherein the content of the antifouling agent (D) is 0.3 parts by mass or more and 550 parts by mass or less per 100 parts by mass of the hydrolyzable resin (A).

[0027]

[10] A coating film formed from the antifouling coating composition according to any one of [1] to [9].

[0028]

[11] A ship having the coating film described in

[10] .

[0029]

[12] An underwater structure having the coating film described in

[10] .

[0030] Effects of the Invention

[0031] An antifouling coating composition comprising a hydrolyzable resin and an antifouling agent and capable of exhibiting high antifouling performance for a long period of time can be provided.

[0032] Furthermore, it is possible to provide a coating film formed from the antifouling coating composition, and a ship and an underwater structure having the coating film. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic plan view for explaining the evaluation method of the dynamic antifouling property of the coating film.

[0034] Figure 2 This is a schematic cross-sectional view for explaining a method for evaluating the dynamic antifouling property of a coating film.

[0035] Figure 3 It is a cross-sectional view schematically showing the state of the coating film corresponding to each evaluation standard for evaluating the drying property of the coating film. DETAILED DESCRIPTION

[0036] <Antifouling coating composition>

[0037] The antifouling coating composition of the present invention (hereinafter also referred to as "antifouling coating composition") comprises a hydrolyzable resin (A), a first non-hydrolyzable resin (B), a second non-hydrolyzable resin (C) and an antifouling agent (D). The hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) are all high molecular weight compounds, i.e., polymers of monomers.

[0038] In the present specification, "hydrolyzable resin" refers to a resin having at least one hydrolyzable group selected from the group represented by formula (1), the group represented by formula (2) and the group represented by formula (3). "Non-hydrolyzable resin" refers to a resin that does not have a group represented by formula (1), a group represented by formula (2) and a group represented by formula (3). The antifouling coating film formed by the antifouling coating composition containing the hydrolyzable resin (A) exhibits antifouling performance because the surface of the coating film is gradually hydrolyzed in water by the hydrolyzable groups of the hydrolyzable resin (A), thereby releasing the antifouling components from the antifouling agent (D) into water.

[0039] In order to impart high antifouling performance to the antifouling coating film formed in the conventional antifouling coating composition comprising a hydrolyzable resin and an antifouling agent, it is necessary to design the antifouling coating composition so that the antifouling coating film has a high consumption rate in water. However, in this case, the antifouling coating film cannot maintain the antifouling performance for a long time because the antifouling coating film disappears at an early stage.

[0040] Hereinafter, such a property of the coating film that the coating film exhibits high antifouling performance for a long period of time is also referred to as “long-term antifouling property” of the coating film.

[0041] The antifouling coating composition of the present invention contains a predetermined first non-hydrolyzable resin (B) and a predetermined second non-hydrolyzable resin (C) in addition to a hydrolyzable resin (A) and an antifouling agent (D), so that the antifouling component from the antifouling agent (D) can be effectively released from the antifouling coating film into water. Therefore, the antifouling coating film of the present invention can exert high antifouling performance even if the consumption rate when immersed in water is low. That is, according to the present invention, both a low coating film consumption rate (long-term antifouling performance) and high antifouling performance can be achieved.

[0042] [1] Hydrolyzable resin (A)

[0043] The antifouling coating composition comprises one or more hydrolyzable resins (A). The hydrolyzable resin (A) has at least one hydrolyzable group selected from the group represented by formula (1), the group represented by formula (2) and the group represented by formula (3).

[0044] [Chemical formula 2]

[0045]

[0046] [In formula (1), R 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 6 carbon atoms.]

[0047] [Chemical formula 3]

[0048]

[0049] [In formula (2), M represents a divalent metal atom, R 4 represents an organic acid residue or an alcohol residue.]

[0050] [Chemical formula 4]

[0051]

[0052] [In formula (3), M represents a divalent metal atom.]

[0053] The hydrolyzable resin (A) is not particularly limited, and a (meth)acrylic resin having a hydrolyzable group can be used appropriately. The hydrolyzable group can be disposed on a side chain of a polymer of the (meth)acrylic resin.

[0054] In the present specification, "(meth)acrylic resin" refers to a resin in which at least a part of the resin contains a structural unit derived from (meth)acrylic acid or a derivative thereof (one example is (meth)acrylic acid ester). The derivatives of (meth)acrylic acid also include metal (meth)acrylic acid salts.

[0055] In this specification, "(meth)acrylic acid" means at least one selected from methacrylic acid and acrylic acid.

[0056] In the present specification, the "(meth)acryloyl group" means at least one selected from the group consisting of a methacryloyl group and an acryloyl group.

[0057] In the present specification, the "(meth)acrylic monomer" refers to a polymerizable monomer having a (meth)acryloyl group or a (meth)acryloyloxy group.

[0058] Examples of the hydrolyzable resin (A) include:

[0059] Hydrolyzable resin (A1): a (meth)acrylic resin having only a group represented by the formula (1) as a hydrolyzable group,

[0060] Hydrolyzable resin (A2): a (meth)acrylic resin having, as a hydrolyzable group, a group represented by formula (1), a group represented by formula (2) and / or a group represented by formula (3);

[0061] Hydrolyzable resin (A3): a (meth)acrylic resin having only a group represented by the formula (2) and / or a group represented by the formula (3) as a hydrolyzable group.

[0062] The hydrolyzable resin (A) may contain one or more resins selected from the hydrolyzable resins (A1) to (A3).

[0063] From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the hydrolyzable resin (A) preferably contains the hydrolyzable resin (A1) or the hydrolyzable resin (A2), and more preferably the hydrolyzable resin (A1) or the hydrolyzable resin (A2).

[0064] Examples of the hydrolyzable resin (A1) include copolymers of a polymerizable monomer (a1) and a polymerizable monomer (a2), wherein the polymerizable monomer (a1) has a group represented by formula (1), and the polymerizable monomer (a2) is another polymerizable monomer that can copolymerize with the polymerizable monomer (a1). The copolymer may be a random copolymer. One or more of the polymerizable monomers (a1) and (a2) may be used respectively. The hydrolyzable resin (A1) may be obtained by copolymerizing the polymerizable monomer (a1) and the polymerizable monomer (a2) in the presence of a free radical polymerization initiator.

[0065] The polymerizable monomer (a1) and the polymerizable monomer (a2) are preferably (meth)acrylic monomers.

[0066] As a polymerizable monomer (a1), a radical polymerizable (meth)acrylic-based monomer represented by Formula (4) is mentioned, for example.

[0067] [Chemical formula 5]

[0068]

[0069] [In formula (4), R 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 6 carbon atoms. 5 represents a hydrogen atom or a methyl group.]

[0070] Examples of the (meth)acrylic monomer represented by formula (4) include trimethylsilyl (meth)acrylate, triethylsilyl (meth)acrylate, tri-n-propylsilyl (meth)acrylate, triisopropylsilyl (meth)acrylate, diisopropyl-sec-butylsilyl (meth)acrylate, diisopropyl-isobutylsilyl (meth)acrylate, diisopropyl-tert-butylsilyl (meth)acrylate, diisopropylhexylsilyl (meth)acrylate, diisopropylphenylsilyl (meth)acrylate, isopropyl-di-sec-butylsilyl (meth)acrylate, and isopropyl-diisobutyl-tert-butylsilyl (meth)acrylate. The invention also includes but is not limited to: (i) tri-butylsilyl (meth)acrylate, (ii) tri-tert-butylsilyl (meth)acrylate, (iii) tri-tert-butylsilyl (meth)acrylate, (iv) tri-tert-butyldiphenylsilyl (meth)acrylate, (v) tri-phenylsilyl (meth)acrylate, (v) tri-cyclohexylsilyl (meth)acrylate, (v) dicyclohexylbenzylsilyl (meth)acrylate, (v) diisopropylcyclohexylsilyl (meth)acrylate, and (v) isopropyldicyclohexylsilyl (meth)acrylate.

[0071] The (meth)acrylic monomer represented by formula (4) may be used alone or in combination of two or more.

[0072] From the viewpoint of achieving both low coating film consumption rate and high antifouling performance, in formula (1) and formula (4), R 1 , R 2 and R 3 Each independently is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and further preferably an alkyl group having 3 or 4 carbon atoms.

[0073] From the viewpoint of achieving both low coating film consumption rate and high antifouling performance, in formula (1) and formula (4), preferably, R 1 , R 2 and R 3 At least one of them is an alkyl group with 3 carbon atoms, and more preferably, R 1 , R 2 and R 3 At least one of them is isopropyl, and more preferably, R 1 , R 2 and R 3 At least two of them are isopropyl, and it is further preferred that R 1 , R 2 and R 3 All are isopropyl.

[0074] The polymerizable monomer (a1) may be a monomer other than the (meth)acrylic monomer represented by the formula (4).

[0075] Monomers other than the (meth)acrylic monomer represented by formula (4) may be used alone or in combination of two or more. The (meth)acrylic monomer represented by formula (4) and monomers other than the (meth)acrylic monomer may be used in combination. The polymerizable monomer (a1) preferably contains the (meth)acrylic monomer represented by formula (4).

[0076] Examples of monomers other than the (meth)acrylic monomer represented by formula (4) include maleic acid diesters having a group represented by formula (1). 1 , R 2 and R 3 , and the above records related to formula (1) are also cited.

[0077] Examples of the maleic acid diester include bis(triisopropylsilyl) maleate, triisopropylsilyl methyl maleate, triisopropylsilyl ethyl maleate, triisopropylsilyl n-butyl maleate, triisopropylsilyl sec-butyl maleate, triisopropylsilyl isobutyl maleate, triisopropylsilyl tert-butyl maleate, triisopropylsilyl n-pentyl maleate, triisopropylsilyl isopentyl maleate (triisopropylsilyl isopentyl maleate), and triisopropylsilyl cyclohexyl maleate.

[0078] Examples of the polymerizable monomer (a2) include:

[0079] Alkyl (meth)acrylates having an ester portion with a carbon number of 1 or more and 20 or less (preferably 1 or more and 8 or less), such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, etc.;

[0080] Hydroxyl-containing alkyl (meth)acrylates having an ester moiety with a carbon number of 1 to 20 (preferably 1 to 8), such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.;

[0081] Alkoxyalkyl (meth)acrylates, such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, etc.;

[0082] (Meth) acrylic monomers containing oxyalkylene chains, such as (meth) acrylic acid methoxy polyethylene glycol (the number of repetitions of -OC2H4- is, for example, 2 to 9);

[0083] (Meth) acrylate cyclic hydrocarbon esters, such as phenyl (meth) acrylate, benzyl (meth) acrylate, cyclohexyl (meth) acrylate, methylcyclohexyl (meth) acrylate, etc.;

[0084] Unsaturated monobasic acids, such as (meth) acrylic acid, cinnamic acid, crotonic acid, etc.;

[0085] Unsaturated dibasic acids and their monoalkyl esters, such as maleic acid, fumaric acid, itaconic acid, their monoalkyl esters, etc.;

[0086] Dibasic acid adducts of unsaturated monobasic acid hydroxyalkyl esters, such as maleic acid adducts of 2-hydroxyethyl (meth)acrylate, phthalic acid adducts of 2-hydroxyethyl (meth)acrylate, succinic acid adducts of 2-hydroxyethyl (meth)acrylate, etc.;

[0087] Other polymerizable vinyl compounds, such as (meth)acrylamide, (meth)acrylonitrile, styrene, α-methylstyrene, o-, m- or p-methylstyrene, vinyl acetate, vinyl propionate, vinyl benzoate, vinyl toluene, etc.

[0088] From the viewpoint of improving the antifouling performance of the antifouling coating film, the content of the structural unit derived from the polymerizable monomer (a1) in the hydrolyzable resin (A1) is preferably 20% by mass or more, more preferably 30% by mass or more, and further preferably 40% by mass or more, and may be 50% by mass or more or 60% by mass or more, based on 100% by mass of the hydrolyzable resin (A1). From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the above content is preferably 80% by mass or less, more preferably 75% by mass or less, more preferably 70% by mass or less, and further preferably 65% ​​by mass or less, based on 100% by mass of the hydrolyzable resin (A1). The remainder of the hydrolyzable resin (A1) is a structural unit derived from the polymerizable monomer (a2).

[0089] Examples of the hydrolyzable resin (A2) include: a polymerizable monomer (a1), a polymerizable monomer (a3) ​​and / or a polymerizable monomer (a4), and a copolymer of a polymerizable monomer (a2), wherein the polymerizable monomer (a1) has a group represented by formula (1), the polymerizable monomer (a3) ​​has a group represented by formula (2), and the polymerizable monomer (a4) has a group represented by formula (3), and the polymerizable monomer (a2) can be copolymerized with these polymerizable monomers. The copolymer may be a random copolymer. One or more of the polymerizable monomers (a1) to (a4) may be used respectively. For example, the hydrolyzable resin (A2) can be obtained by copolymerizing the polymerizable monomer (a1) with the polymerizable monomer (a3) ​​and / or (a4) with the polymerizable monomer (a2) in the presence of a free radical polymerization initiator. With respect to the polymerizable monomers (a1) and (a2), the above description of the hydrolyzable resin (A1) is cited.

[0090] The polymerizable monomers (a1) to (a4) are preferably (meth)acrylic monomers.

[0091] Examples of the polymerizable monomer (a3) ​​include radical polymerizable (meth)acrylic monomers represented by formula (5). By using the (meth)acrylic monomer represented by formula (5), a hydrolyzable resin (A2) having a group represented by formula (2) can be obtained.

[0092] [Chemical formula 6]

[0093]

[0094] [In formula (5), M represents a divalent metal atom, R 4 represents an organic acid residue or an alcohol residue, R 6 represents a hydrogen atom or a methyl group.]

[0095] Examples of polymerizable monomers (a4) include free radical polymerizable (meth) acrylic monomers represented by formula (6). By using the (meth) acrylic monomers represented by formula (6), a hydrolyzable resin (A2) having a group represented by formula (3) can be obtained. The group represented by formula (3) is a crosslinking group that crosslinks the main chains of the polymer.

[0096] [Chemical formula 7]

[0097]

[0098] [In formula (6), M represents a divalent metal atom, R 7 and R 8 Each independently represents a hydrogen atom or a methyl group.]

[0099] Examples of the divalent metal atom M in formulas (2), (3), (5) and (6) include Mg, Zn, Cu and the like, and Zn or Cu is preferred. 4 An organic acid residue is preferred.

[0100] As in R 4 Examples of organic acids that form organic acid residues in the ester include acetic acid, monochloroacetic acid, monofluoroacetic acid, propionic acid, hexanoic acid, octanoic acid, 2-ethylhexanoic acid, decanoic acid, versatile carbonic acid, isostearic acid, palmitic acid, cresol acid, oleic acid, elaidic acid, linoleic acid, linolenic acid, stearic acid, ricinoleic acid, ricinoleic acid, brassinoic acid, erucic acid, α-naphthoic acid, β-naphthoic acid, benzoic acid, 2,4,5-trichlorophenoxyacetic acid, 2,4-dichlorophenoxyacetic acid, quinolinecarboxylic acid, nitrobenzoic acid, nitronaphthoic acid, purvinic acid and other monobasic organic acids.

[0101] Among them, when the organic acid residue is a fatty acid residue, there is a tendency that an antifouling coating film free from cracks and peeling can be formed for a long period of time.

[0102] Examples of other organic acids forming the organic acid residue include monocyclic organic acids other than aromatic organic acids, such as organic acids having a cycloalkyl group such as cycloalkane acid, resin acids such as tricyclic resin acids, and salts thereof.

[0103] Examples of tricyclic resin acids include monobasic acids having a diterpene hydrocarbon skeleton. Examples of monobasic acids having a diterpene hydrocarbon skeleton include compounds having abietane, pimarane, isopimarane, and abietic skeletons. More specifically, examples include abietic acid, neoabietic acid, dehydroabietic acid, hydrogenated abietic acid, palustric acid, pimaric acid, isopimaric acid, left-rotated pimaric acid, right-rotated pimaric acid, sandarac pimaric acid, and salts thereof. Among these, from the viewpoint of the antifouling properties of the coating film, abietane, hydrogenated abietic acid, and salts thereof are preferred.

[0104] The monocyclic organic acid does not need to be highly purified, and for example, rosin, pine resin acid, etc. may also be used. Examples of such organic acids include rosins, hydrogenated rosins, disproportionated rosins, naphthenic acid, etc. Rosins refer to gum rosin, wood rosin, tall oil rosin, etc. Rosins, hydrogenated rosins, and disproportionated rosins are preferred from the perspectives of being cheap and easily available, having excellent operability, and being easy to exhibit long-term antifouling properties.

[0105] The acid value of the monovalent cyclic organic acid is preferably 100 mgKOH / g to 220 mgKOH / g, more preferably 120 mgKOH / g to 190 mgKOH / g, and further preferably 140 mgKOH / g to 185 mgKOH / g.

[0106] The organic acid residue contained in the monomer represented by the formula (5) may be composed of one organic acid or two or more organic acids.

[0107] As having an organic acid residue as R 4 The method for preparing the monomer can be, for example, a method of reacting an inorganic metal compound, a carboxyl-containing free radical polymerizable monomer such as (meth)acrylic acid, and a non-polymerizable organic acid (an organic acid constituting the above-mentioned organic acid residue) in an organic solvent containing an alcohol compound.

[0108] The structural unit derived from the (meth)acrylic acid monomer represented by formula (5) can also be formed by a method in which a resin obtained by polymerizing a monomer composition containing a carboxyl group-containing free radical polymerizable monomer such as (meth)acrylic acid is reacted with a metal compound and a non-polymerizable organic acid (the organic acid constituting the above-mentioned organic acid residue).

[0109] Examples of the (meth)acrylic monomer represented by formula (6) include magnesium acrylate [(CH2=CHCOO)2Mg], magnesium methacrylate [(CH2=C(CH3)COO)2Mg], zinc acrylate [(CH2=CHCOO)2Zn], zinc methacrylate [(CH2=C(CH3)COO)2Zn], copper acrylate [(CH2=CHCOO)2Cu], copper methacrylate [(CH2=C(CH3)COO)2Cu], etc. These monomers may be selected and used alone or in combination as required.

[0110] As a method for producing the (meth)acrylic acid monomer represented by formula (6), for example, there can be mentioned a method in which a polymerizable unsaturated organic acid such as (meth)acrylic acid and a metal compound are reacted together with water in an organic solvent containing an alcohol compound. In this case, preferably, the water content in the reactant is adjusted to 0.01 mass % or more and 30 mass % or less.

[0111] Regarding the content of the structural unit derived from the polymerizable monomer (a1) in the hydrolyzable resin (A2), the above description on the hydrolyzable resin (A1) is cited.

[0112] From the viewpoint of improving the antifouling performance of the antifouling coating film, the total content of the structural units derived from the polymerizable monomers (a3) ​​and (a4) in the hydrolyzable resin (A2) is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 4% by mass or more, and may be 6% by mass or more, based on 100% by mass of the hydrolyzable resin (A2). From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the above content is preferably 30% by mass or less, more preferably 25% by mass or less, and more preferably 20% by mass or less, based on 100% by mass of the hydrolyzable resin (A2).

[0113] The content of the structural unit derived from the polymerizable monomer (a2) in the hydrolyzable resin (A2) is usually 0.1 mass % to 90 mass % in 100 mass % of the hydrolyzable resin (A2), preferably 5 mass % to 80 mass % and more preferably 10 mass % to 70 mass % in 100 mass % of the hydrolyzable resin (A2).

[0114] Examples of the hydrolyzable resin (A3) include copolymers of polymerizable monomers (a3) ​​and / or polymerizable monomers (a4) and polymerizable monomers (a2), wherein the polymerizable monomer (a3) ​​has a group represented by formula (2), the polymerizable monomer (a4) has a group represented by formula (3), and the polymerizable monomer (a2) can be copolymerized with these polymerizable monomers. The copolymer may be a random copolymer. One or more polymerizable monomers (a2) to (a4) may be used respectively. For example, the hydrolyzable resin (A3) can be obtained by copolymerizing the polymerizable monomers (a3) ​​and / or (a4) with the polymerizable monomer (a2) in the presence of a free radical polymerization initiator. With regard to the polymerizable monomers (a2) to (a4), the above descriptions of the hydrolyzable resins (A1) or (A2) are cited.

[0115] The polymerizable monomers (a2) to (a4) are preferably (meth)acrylic monomers.

[0116] From the viewpoint of improving the antifouling performance of the antifouling coating film, the total content of the structural units derived from the polymerizable monomers (a3) ​​and (a4) in the hydrolyzable resin (A3) is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 4% by mass or more, and may be 6% by mass or more, based on 100% by mass of the hydrolyzable resin (A3). From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the above content is preferably 30% by mass or less, more preferably 25% by mass or less, and more preferably 20% by mass or less, based on 100% by mass of the hydrolyzable resin (A3). The remainder is a structural unit derived from the polymerizable monomer (a2).

[0117] The weight average molecular weight (Mw) of the hydrolyzable resin (A) is usually 2000 or more and 300000 or less, preferably 5000 or more and 100000 or less, and more preferably 10000 or more and 80000 or less. When Mw is 2000 or more, when a coating film is formed from an antifouling coating composition containing the same, there is a tendency to be able to exhibit antifouling performance, and when Mw is 300000 or less, there is a tendency to easily make the hydrolyzable resin (A) uniformly dispersed in the antifouling coating composition. In this specification, Mw is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0118] From the viewpoint of achieving both a low coating film consumption rate and a high antifouling performance, the glass transition temperature Tg of the hydrolyzable resin (A) (when the antifouling coating composition contains two or more hydrolyzable resins (A), each of them) is preferably A The range of preferably 10°C to 80°C, the dissolution parameter SP A The range of 8.5 or more and 9.7 or less is preferable.

[0119] Glass transition temperature Tg of the hydrolyzable resin (A) A The temperature is more preferably 20°C to 80°C, further preferably 30°C to 80°C, further preferably 40°C to 80°C, particularly preferably 45°C to 80°C, and most preferably 45°C to 78°C.

[0120] Dissolution parameter SP of hydrolyzable resin (A) A The range is more preferably 8.55 to 9.7, further preferably 8.60 to 9.65, still further preferably 8.60 to 9.60, and particularly preferably 8.70 to 9.50.

[0121] In this specification, the glass transition temperature is a temperature measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7121.

[0122] The solubility parameter SP (solubility parameter) is a criterion for solubility. The larger the SP value, the higher the polarity, and conversely, the smaller the value, the lower the polarity.

[0123] In the present specification, the solubility parameter SP of a resin can be measured by the following method (reference: SUH, CLARKE, JPSA-1, 5, 1671 to 1681 (1967)).

[0124] At a measurement temperature of 20°C, weigh 0.5g of resin into a 100mL beaker, add 10mL of a good solvent (acetone) using a hole pipette, and dissolve it using a magnetic stirrer to prepare a dilute solution. Next, use a 50mL burette to slowly drop a low SP poor solvent (n-hexane) into the dilute solution, and take the point at which the dilute solution becomes turbid as the amount of low SP poor solvent added. In addition, slowly drop a high SP poor solvent (ion exchange water) into the above-mentioned dilute solution, and take the point at which the dilute solution becomes turbid as the amount of high SP poor solvent added. The SP value can be calculated by the known calculation method described in the above-mentioned references, etc., from the amount of each of the above-mentioned poor solvents added until the turbidity point is reached.

[0125] Glass transition temperature Tg of the hydrolyzable resin (A) A and the dissolution parameter SP A The Tg can be controlled by adjusting the type or content of the monomers forming the hydrolyzable resin (A). A It can also be estimated or estimated from the glass transition temperature of the monomers forming the hydrolyzable resin (A). A If the content of the (meth)acrylic acid monomer represented by formula (4) is increased, SP A There is a tendency to get smaller.

[0126] From the viewpoint of achieving both a low coating film consumption rate and a high antifouling performance, the content of the hydrolyzable resin (A) in the antifouling coating composition is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 80% by mass or less, further preferably 30% by mass or more and 70% by mass or less, further preferably 40% by mass or more and 65% by mass or less, particularly preferably 45% by mass or more and 65% by mass or less, based on 100% by mass of the total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition.

[0127] [2] First non-hydrolyzable resin (B) and second non-hydrolyzable resin (C)

[0128] In addition to the hydrolyzable resin (A), the antifouling coating composition further comprises a first non-hydrolyzable resin (B) and a second non-hydrolyzable resin (C). The glass transition temperature of the first non-hydrolyzable resin (B) is higher than the glass transition temperature of the second non-hydrolyzable resin (C). The antifouling coating composition may comprise two or more first non-hydrolyzable resins (B), and may comprise two or more second non-hydrolyzable resins (C). The meaning of "non-hydrolyzable resin" is as described above.

[0129] The first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) are preferably (meth)acrylic resins.

[0130] When the glass transition temperature of the first non-hydrolyzable resin (B) is Tg B [℃], dissolution parameter is set to SP B The glass transition temperature of the second non-hydrolyzable resin (C) is Tg C [℃], dissolution parameter is set to SP C When the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) satisfy the following formulas [1] to [4].

[0131] Tg B -Tg C ≥60 [1]

[0132] SP B ≥9.5 [2]

[0133] SP C ≥9.5 [3]

[0134] |SP B -SP C |≤1.0 [4]

[0135] The antifouling coating composition of the present invention, which contains a first non-hydrolyzable resin (B) and a second non-hydrolyzable resin (C) satisfying formulas [1] to [4] in addition to the hydrolyzable resin (A), can form an antifouling coating film having both a low coating film consumption rate and high antifouling performance.

[0136] From the perspective of achieving both low film consumption rate and high antifouling performance, Tg B With Tg C The difference (Tg B -Tg C ) is preferably 70°C or higher, more preferably 80°C or higher, further preferably 90°C or higher, and may be 100°C or higher. The difference is usually 150°C or lower, and may be 140°C or lower, 130°C or lower, or 120°C or lower.

[0137] From the perspective of achieving both low film consumption rate and high antifouling performance, Tg B It is preferably 40°C to 80°C, more preferably 45°C to 75°C, further preferably 50°C to 70°C, and still further preferably 50°C to 65°C.

[0138] From the perspective of achieving both low film consumption rate and high antifouling performance, Tg CIt is preferably -50°C to -20°C, more preferably -50°C to -25°C, further preferably -50°C to -30°C, and still further preferably -45°C to -35°C.

[0139] SP B and SP C All are above 9.5 (Formulas [2] and [3]). As long as Formula [4] is satisfied, SP B and SP C There is no particular limitation on the size relationship of SP C Greater than SP B In other embodiments, SP B Greater than SP C . |SP B -SP C | It is preferably 0.8 or less, more preferably 0.6 or less, further preferably 0.4 or less, and further preferably 0.3 or less.

[0140] From the perspective of achieving both low film consumption rate and high antifouling performance, SP B It is preferably 9.6 or more and 10.3 or less, more preferably 9.6 or more and 10.2 or less, and further preferably 9.7 or more and 10.1 or less.

[0141] From the perspective of achieving both low film consumption rate and high antifouling performance, SP C It is preferably 9.8 or more and 10.6 or less, more preferably 9.8 or more and 10.5 or less, and further preferably 9.9 or more and 10.4 or less.

[0142] With Tg A and SP A Similarly, Tg B , SP B , Tg C and SP C It can be controlled by adjusting the type or content of the monomers forming the resin. B , Tg C It can also be estimated or estimated based on the glass transition temperature of the monomer. A and SP C There is a trend of getting bigger.

[0143] The first non-hydrolyzable resin (B) is not particularly limited as long as it satisfies the formulas [1], [2] and [4], and examples thereof include (meth)acrylic resins formed from one or more of the monomers selected from the above-mentioned monomer group as examples of the polymerizable monomer (a2). Specifically, the first non-hydrolyzable resin (B) is represented by a trade name, and examples thereof include "Dianal BR-106" manufactured by Mitsubishi Chemical Corporation, "ETERAC 7123-X-50" (BALBIS) manufactured by BALBIS Corporation, "PARALOID B66" manufactured by The Dow Chemical Company, and "DEGALAN 64 / 12N" manufactured by Evonik Degussa (Japan) Ltd.

[0144] The second non-hydrolyzable resin (C) is not particularly limited as long as it satisfies formulas [1], [3], and [4]. Examples thereof include (meth)acrylic resins formed from one or more of the monomers selected from the above monomer group as examples of the polymerizable monomer (a2). Specifically, examples of the second non-hydrolyzable resin (C) include "Lutonal A25" manufactured by BASF.

[0145] The second non-hydrolyzable resin (C) is not limited to the (meth)acrylic resin, and examples thereof include polyvinyl alkyl ether and the like.

[0146] The weight average molecular weight (Mw) of the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) is usually 2000 or more and 300000 or less, preferably 5000 or more and 100000 or less, and more preferably 10000 or more and 80000 or less. When Mw is 2000 or more, it is advantageous in achieving both a low coating film consumption rate and high antifouling performance. When Mw is 300000 or less, there is a tendency to easily disperse these resins uniformly in the antifouling coating composition.

[0147] From the viewpoint of achieving both a low coating film consumption rate and a high antifouling performance, the content of the first non-hydrolyzable resin (B) in the antifouling coating composition is preferably 2% by mass or more and 50% by mass or less, more preferably 3% by mass or more and 40% by mass or less, further preferably 5% by mass or more and 35% by mass or less, even more preferably 5% by mass or more and 30% by mass or less, particularly preferably 5% by mass or more and 25% by mass or less, based on 100% by mass of the total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition.

[0148] From the viewpoint of achieving both a low coating film consumption rate and a high antifouling performance, the content of the second non-hydrolyzable resin (C) in the antifouling coating composition is preferably 2% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 45% by mass or less, further preferably 10% by mass or more and 40% by mass or less, further preferably 15% by mass or more and 35% by mass or less, particularly preferably 20% by mass or more and 35% by mass or less, based on 100% by mass of the total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition.

[0149] From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the content ratio ((B) / (A)) of the first non-hydrolyzable resin (B) to the hydrolyzable resin (A) in the antifouling coating composition is preferably 0.02 to 1, more preferably 0.05 to 0.8, further preferably 0.1 to 0.6, and even more preferably 0.1 to 0.5 in terms of mass ratio.

[0150] From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the content ratio ((C) / (A)) of the second non-hydrolyzable resin (C) to the hydrolyzable resin (A) in the antifouling coating composition is preferably 0.01 to 1, more preferably 0.02 to 0.9, further preferably 0.05 to 0.8, further preferably 0.05 to 0.65, and may be 0.1 to 0.2, 0.3 to 0.6 or less in terms of mass ratio.

[0151] From the viewpoint of achieving both a low coating film consumption rate and high antifouling performance, the content ratio ((B) / (C)) of the first non-hydrolyzable resin (B) to the second non-hydrolyzable resin (C) in the antifouling coating composition is preferably 0.05 to 9, more preferably 0.1 to 6, further preferably 0.2 to 2, further preferably 0.2 to 1.5, and particularly preferably 0.2 to 1, in terms of mass ratio.

[0152] From the viewpoint of achieving both a low coating film consumption rate and a high antifouling performance, the total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition is preferably 5% by mass or more and 40% by mass or less, and more preferably 10% by mass or more and 20% by mass or less, based on 100% by mass of the solid content contained in the antifouling coating composition.

[0153] The solid content contained in the antifouling coating composition refers to the total amount of components other than the solvent contained in the antifouling coating composition.

[0154] [3] Antifouling agent (D)

[0155] The antifouling coating composition contains one or more antifouling agents (D). The antifouling agent (D) is not particularly limited, and known antifouling agents can be used, for example, inorganic compounds, metal-containing organic compounds, metal-free organic compounds and the like.

[0156] Examples of the antifouling agent (D) include cuprous oxide; manganese ethylenebisdithiocarbamate; zinc dimethyldithiocarbamate; 2-methylthio-4-tert-butylamino-6-cyclopropylamino-s-triazine; 2,4,5,6-tetrachloroisophthalonitrile; N,N-dimethyldichlorophenylurea; zinc ethylenebisdithiocarbamate; rhodamine copper (cuprous thiocyanate); 4,5-dichloro-2-n-octyl-4-isothiazoline-3-one (4,5-dichloro-2-octyl-3(2H)isothiazolone); N-(fluorodichloromethylthio)phthalimide N,N'-dimethyl-N'-phenyl-(N-fluorodichloromethylthio)sulfonamide; zinc salt of 2-pyridinethiol-1-oxide (pyridinethione zinc); copper salt of 2-pyridinethiol-1-oxide (pyridinethione copper); tetramethylthiuram disulfide; 2,4,6-trichlorophenylmaleimide; 2,3, 5,6-Tetrachloro-4-(methylsulfonyl)pyridine; 3-iodo-2-propylbutylcarbamate; diiodomethyl trisulfone; phenyl(bispyridyl)bismuth dichloride; 2-(-thiazolyl)-benzimidazole; triphenylboron pyridinium salt; stearylamine triphenylboron; laurylamine triphenylboron; zinc dimethyldithiocarbamoyl ethylenebisdithiocarbamate; 1,1-dichloro-N-[(dimethylamino)sulfonyl]-1-fluoro-N-phenyl Methanesulfonamide; 1,1-dichloro-N-[(dimethylamino)sulfonyl]-1-fluoro-N-(4-methylphenyl)methanesulfonamide; N'-(3,4-dichlorophenyl)-N,N'-dimethylurea; N'-tert-butyl-N-cyclopropyl-6-(methylthio)-1,3,5-triazine-2,4-diamine; 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile; medetomidine, etc.

[0157] The content of the antifouling agent (D) in the antifouling coating composition is usually 0.3 parts by mass or more and 550 parts by mass or less, preferably 1 part by mass or more and 500 parts by mass or less, more preferably 5 parts by mass or more and 300 parts by mass or less, further preferably 5 parts by mass or more and 200 parts by mass or less, and further preferably 10 parts by mass or more and 150 parts by mass or less, based on 100 parts by mass of the hydrolyzable resin (A).

[0158] When the content of the antifouling agent (D) is too low, the coating film tends to fail to exhibit antifouling performance, while when the content of the antifouling agent is too high, defects such as cracks and peeling may occur in the coating film.

[0159] [4] Rosin compounds (E)

[0160] The antifouling coating composition may also contain a rosin compound (E). Since the rosin compound (E) does not belong to a resin (a polymer as a monomer), it does not belong to the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C). By making the antifouling coating composition contain a rosin compound (E), there is a tendency to improve the antifouling performance of the coating film.

[0161] The rosin compound (E) refers to rosin or a rosin derivative. Examples of the rosin derivative include hydrogenated rosin, disproportionated rosin, maleated rosin, formylated rosin, and polymerized rosin.

[0162] When the antifouling coating composition contains a rosin-based compound (E), the content of the rosin-based compound (E) is preferably 1 part by mass or more and 50 parts by mass or less, more preferably 2 parts by mass or more and 40 parts by mass or less, and even more preferably 5 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition.

[0163] [5] Other ingredients

[0164] The antifouling coating composition may also contain other components other than those mentioned above. Examples of other components include: coating film consumption regulator, pigment, plasticizer, solvent, water-binding agent, anti-sagging agent, anti-coloring agent, anti-settling agent, defoaming agent, ultraviolet absorber, surface regulator, viscosity regulator, leveling agent, dispersant (colloidal silica, etc.), etc.

[0165] Examples of pigments include: extender pigments such as precipitated barium, talc, clay, chalk, white silica, alumina white, bentonite, calcium carbonate, magnesium carbonate, silicic acid, silicates, aluminum oxide hydrate, calcium sulfate, etc.; coloring pigments such as titanium oxide, zirconium oxide, basic lead sulfate, tin oxide, carbon black, white lead, graphite, zinc sulfide, zinc oxide (zinc white), chromium oxide, nickel titanium yellow, chrome titanium yellow, iron oxide yellow, iron oxide red, iron oxide black, azo red / yellow pigments, chrome yellow, phthalocyanine green, phthalocyanine blue, ultramarine blue, quinacridone, etc.

[0166] The pigment may be used alone or in combination of two or more.

[0167] As the plasticizer, for example, there can be listed: phthalate plasticizers, such as dioctyl phthalate (DOP), dimethyl phthalate, dicyclohexyl phthalate, diisodecyl phthalate (DIDP), etc.; aliphatic dibasic acid ester plasticizers, such as isobutyl adipate, dibutyl sebacate, etc.; glycol ester plasticizers, such as diethylene glycol dibenzoate, pentaerythritol alkyl esters, etc.; phosphate ester plasticizers, such as tricresyl phosphate (tricresyl phosphate), triaryl phosphate (triaryl phosphate), trichloroethyl phosphate, etc.; epoxy plasticizers, such as epoxy soybean oil, epoxy octyl stearate, etc.; organic tin-based plasticizers, such as dioctyltin laurate, dibutyltin laurate, etc.; trioctyl trimellitate, triacetin, etc.

[0168] The plasticizer may be used alone or in combination of two or more.

[0169] As the solvent, for example, the following can be listed: hydrocarbons, such as toluene, xylene, ethylbenzene, cyclopentane, octane, heptane, cyclohexane, petroleum solvents, etc.; ethers, such as dioxane, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, etc.; esters, such as butyl acetate, propyl acetate, benzyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, etc.; ketones, such as ethyl isobutyl ketone, methyl isobutyl ketone, etc.; alcohols, such as n-butanol, propanol, etc.

[0170] The solvent may be used alone or in combination of two or more.

[0171] <Method for producing antifouling coating composition>

[0172] The antifouling coating composition can be prepared by mixing the prescribed components and other components added as needed using a mixer such as a ball mill, a pebble mill, a roll mill, a sand mill, a disperser, etc. For example, the hydrolyzable resin (A), the first non-hydrolyzable resin (B), and the second non-hydrolyzable resin (C) can be mixed in the form of a solution.

[0173] <Coating>

[0174] The coating film of the present invention is an antifouling coating film formed from the antifouling coating composition of the present invention. The antifouling coating film of the present invention can achieve both a low coating film consumption rate (long-term antifouling property) and high antifouling performance.

[0175] The antifouling coating film can be formed by applying the antifouling coating composition on the surface of the object to be coated according to a conventional method and then, if necessary, removing the solvent by volatilization at room temperature or under heating.

[0176] The thickness of the antifouling coating film is, for example, 50 μm or more and 500 μm or less, and preferably 100 μm or more and 400 μm or less.

[0177] The method for applying the antifouling coating composition is not particularly limited, and examples thereof include dipping, spraying, brushing, roller coating, electrostatic coating, and electrodeposition coating.

[0178] The objects to be coated are not particularly limited, and examples thereof include: ships; various fishing nets and other fishing gear, including aquaculture; harbor facilities; oil booms; water intake equipment for power plants, etc.; pipes such as cooling water pipes; bridges; buoys; industrial water facilities; underwater structures such as seabed bases, etc. The objects to be coated are preferably ships and underwater structures.

[0179] The coated surface of the coated object can be pretreated as needed. In addition, the antifouling coating of the present invention can be formed on a base coating composed of other coatings such as rust-proof coating (anticorrosion coating) formed on the coated object to form a composite coating.

[0180] Example

[0181] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0182] <Production Examples A1 to A10: Preparation of Hydrolyzable Resins A1 to A10>

[0183] 34 g of xylene as a solvent was added to a four-necked flask equipped with a thermometer, a cooling tube, a stirrer, a dropping funnel, a nitrogen inlet tube and a temperature controller, and the temperature was maintained at 95±3°C. Here, a mixed solution consisting of the monomers shown in Table 1 in the amounts shown in Table 1 (the unit of the mixed amount of the monomers shown in Table 1 is "g") and 1.0 g of tert-butyl peroxy-2-ethylhexanoate as a free radical polymerization initiator was added to the dropping funnel, and it was dripped into the four-necked flask over a period of 4 hours, and then after keeping warm for 4 hours, 33 g of xylene was added and cooled to obtain a solution containing a hydrolyzable resin. Hereinafter, the solutions containing hydrolyzable resins A1 to A10 (also referred to as resins A1 to A10, respectively) are also referred to as "resin solutions A1 to A10", respectively.

[0184] The glass transition temperatures Tg of the obtained resins A1 to A10 were measured. A , dissolution parameter SP A , weight average molecular weight Mw and solid content of resin solutions A1 to A10. The results are shown in Table 1. The measurement method is as follows.

[0185] (i) Glass transition temperature

[0186] The glass transition temperature Tg was measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7121. The differential scanning calorimeter (DSC) used was "X-DSC7000" manufactured by SII Nanotechnologies Corporation.

[0187] (ii) Dissolution parameters

[0188] Determine using the method already described.

[0189] (iii) Weight average molecular weight Mw

[0190] The weight average molecular weight Mw of the resin is a weight average molecular weight in terms of polystyrene measured by GPC. The measurement conditions are as follows.

[0191] Equipment: Tosoh Corporation "HLC-8220 GPC"

[0192] Chromatographic column: TSKgel SuperHZM-M×2

[0193] Eluent: Tetrahydrofuran

[0194] Measurement temperature: 35℃

[0195] Detector: RI

[0196] (iv) Solid content

[0197] The solid content was calculated according to the following formula.

[0198] Solid content (mass %) = 100 × (total mass of raw materials used in the preparation of the resin solution excluding the solvent) / (mass of the obtained resin solution)

[0199] [Table 1]

[0200]

[0201] <Production Examples B1 to B7: Preparation of First Non-hydrolyzable Resins B1 to B7>

[0202] 34 g of xylene as a solvent was added to a four-necked flask equipped with a thermometer, a cooling tube, a stirrer, a dropping funnel, a nitrogen inlet tube and a temperature controller, and the temperature was maintained at 95±3°C. Here, a mixed solution consisting of the monomers shown in Table 2 in the amounts shown in Table 2 (the unit of the mixed amount of the monomers shown in Table 2 is "g") and 1.0 g of tert-butyl peroxy-2-ethylhexanoate as a free radical polymerization initiator was added to the dropping funnel, and it was dripped into the four-necked flask over a period of 4 hours, and then after keeping warm for 4 hours, 66 g of xylene was added and cooled to obtain a solution containing a non-hydrolyzable resin. Hereinafter, the solutions containing non-hydrolyzable resins B1 to B7 (also referred to as resins B1 to B7, respectively) are also referred to as "resin solutions B1 to B7", respectively.

[0203] The glass transition temperatures Tg of the obtained non-hydrolyzable resins B1 to B7 were measured. B , dissolution parameter SP B , weight average molecular weight Mw and solid content of resin solutions B1 to B7. The results are shown in Table 2. The measurement method is the same as that of (i) to (iii) above.

[0204] <Preparation of first non-hydrolyzable resins B8 to B10>

[0205] Commercially available (meth)acrylic resins were prepared as first non-hydrolyzable resins B8 to B10 (also referred to as resins B8 to B10, respectively). The glass transition temperatures Tg of the non-hydrolyzable resins B8 to B10 were measured. B , dissolution parameter SP B The results are shown in Table 2. The determination method is the same as in (i) to (iii) above. In addition, the solid contents (nominal values) of the non-hydrolyzable resins B8 to B10 are shown in Table 2.

[0206] [Table 2]

[0207]

[0208] <Production Examples C1 to C8: Preparation of Second Non-hydrolyzable Resins C1 to C8>

[0209] 34 g of xylene as a solvent was added to a four-necked flask equipped with a thermometer, a cooling tube, a stirrer, a dropping funnel, a nitrogen inlet tube and a temperature controller, and the temperature was maintained at 95±3°C. Here, a mixed solution consisting of the monomers shown in Table 3 in the amounts shown in Table 3 (the unit of the mixed amount of the monomers shown in Table 3 is "g") and 1.0 g of tert-butyl peroxy-2-ethylhexanoate as a free radical polymerization initiator was added to the dropping funnel, and it was dripped into the four-necked flask over a period of 4 hours, and then after keeping warm for 4 hours, 33 g of xylene was added and cooled to obtain a solution containing a non-hydrolyzable resin. Hereinafter, the solutions containing non-hydrolyzable resins C1 to C8 (also referred to as resins C1 to C8, respectively) are also referred to as "resin solutions C1 to C8", respectively.

[0210] The glass transition temperatures Tg of the obtained non-hydrolyzable resins C1 to C8 were measured. C , dissolution parameter SP C , weight average molecular weight Mw and solid content of resin solutions C1 to C8. The results are shown in Table 3. The measurement method is the same as that of (i) to (iii) above.

[0211] <Preparation of the second non-hydrolyzable resins C9 and C10>

[0212] A commercially available resin was prepared as the second non-hydrolyzable resin C9 (also referred to as resin C9). A commercially available resin was prepared as the second non-hydrolyzable resin C10 (also referred to as resin C10). The glass transition temperatures Tg of the non-hydrolyzable resins C9 and C10 were measured. C and the dissolution parameter SP C The results are shown in Table 3. The measurement method is the same as in (i) to (ii) above. In addition, Table 3 shows the solid contents (nominal values) of the non-hydrolyzable resins C9 and C10.

[0213] [Table 3]

[0214]

[0215] The details of the abbreviations shown in Tables 1 to 3 are as follows.

[0216] (1) TIPSMA: triisopropylsilyl methacrylate

[0217] (2) TIPSA: triisopropylsilyl acrylate

[0218] (3) MEA: 2-methoxyethyl acrylate

[0219] (4)MEMA: 2-methoxyethyl methacrylate

[0220] (5) M-90G: methoxy polyethylene glycol methacrylate (number of repetitions of oxyethylene chains = 9)

[0221] (6) MMA: methyl methacrylate

[0222] (7) EA: Ethyl acrylate

[0223] (8) n-BA: n-butyl acrylate

[0224] (9) EHA: 2-ethylhexyl acrylate

[0225] (10) n-BMA: n-butyl methacrylate

[0226] (11) i-BMA: isobutyl methacrylate

[0227] (12) t-BMA: tert-butyl methacrylate

[0228] (13) Non-hydrolyzable resin B8: (meth)acrylic resin ("Dianal BR-106" manufactured by Mitsubishi Chemical Corporation, solid content 100% by mass)

[0229] (14) Non-hydrolyzable resin B9: (meth)acrylic resin ("ETERAC 7123-X-50" manufactured by BALBIS Corporation, a solution having a solid content of 50.0% by mass containing xylene as a solvent)

[0230] (15) Non-hydrolyzable resin B10: (meth)acrylic resin ("PARALOID B-66" manufactured by The Dow Chemical Company, solid content 100% by mass)

[0231] (16) Non-hydrolyzable resin C9: polyvinyl ethyl ether ("Lutonal A25" manufactured by BASF, solid content 95.0% by mass)

[0232] (17) Non-hydrolyzable resin C10: Chlorinated paraffin ("TOYOPARAX A50" manufactured by Tosoh Corporation, solid content 100% by mass)

[0233] <Examples 1 to 38, Comparative Examples 1 to 8>

[0234] [a] Preparation of antifouling coating composition

[0235] According to the mixing prescriptions (parts by mass) in Tables 4 to 10, the components shown in the tables were mixed and dispersed using a disperser (2000 rpm) to prepare antifouling coating compositions. The above-prepared resin solutions were prepared for the hydrolyzable resin (A) and the non-hydrolyzable resins (B) and (C). When commercial products were used, they were prepared as they were.

[0236] The details of the components described in Tables 4 to 10 are as follows.

[0237] (1) Antifouling agent D1: Cuprous oxide (manufactured by Furukawa Chemical Co., Ltd.)

[0238] (2) Antifouling agent D2: Copper pyrithione ("Copper Omadine" manufactured by Aki Chemical Co., Ltd.)

[0239] (3) Antifouling agent D3: Medetomidine ("Selektope" manufactured by I-TECH AB)

[0240] (4) Antifouling agent D4: 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (4,5-dichloro-2-n-octyl-3(2H)isothiazolone) ("SEA-NINE211" manufactured by Rohm and Haas Company)

[0241] (5) Rosin compounds (E): Gum rosin ("WW rosin" manufactured by Arakawa Chemical Industries, Ltd.)

[0242] (6) Other ingredients F1: xylene

[0243] (7) Other components F2: titanium oxide pigment ("TI-PURE R-900" manufactured by DuPont)

[0244] (8) Other components F3: Iron oxide red pigment ("Bayferox 130" manufactured by LANXESS)

[0245] (9) Other components F4: Silica pigment ("S-SIL20" manufactured by SAC Corporation)

[0246] (10) Other components F5: Anti-sagging agent ("DISPARON 6900-20X" manufactured by Kusumoto Chemicals Co., Ltd.)

[0247] In Tables 4 to 10, "(B) / (A)" represents the content ratio (mass ratio) of the non-hydrolyzable resin (B) to the hydrolyzable resin (A). "(C) / (A)" represents the content ratio (mass ratio) of the non-hydrolyzable resin (C) to the hydrolyzable resin (A).

[0248] [b] Evaluation of coating film consumption rate

[0249] The obtained antifouling coating composition was applied to a sandblasted plate previously coated with an antirust coating to a dry film thickness of 300 μm, and dried by placing it indoors for 2 days and nights to obtain a test plate with an antifouling coating film. The test plate was attached to the side of a cylinder with a diameter of 750 mm and a length of 1200 mm, and rotated continuously in seawater at a peripheral speed of 15 nautical miles day and night to measure the coating consumption of the test plate (cumulative reduction in coating thickness [μm]) over time. The results are shown in Tables 4 to 10.

[0250] [c] Evaluation of the antifouling properties (dynamic antifouling properties) of the coating film

[0251] The obtained antifouling coating composition was applied to a sandblasted plate previously coated with an antirust coating to a dry film thickness of 300 μm, and dried by leaving it indoors for 2 days and nights to obtain a test plate having an antifouling coating film.

[0252] Prepared Figure 1 as well as Figure 2 The metal water channel 10 shown in the figure has a groove with a width of 450 mm and a depth of 200 mm. As shown in the figure, the test plate 20 prepared above is placed on the bottom surface of the groove with the antifouling coating film facing upward.

[0253] The water channel 10 with the test plate 20 was placed in a room irradiated with sunlight in the Rinkai Evaluation Technology Center of Nippon Paint Marine Coatings Co., Ltd. in Tamano City, Okayama Prefecture. At this time, in order to maximize the time for sunlight to irradiate the test plate 20, the water channel 10 was arranged along the north-south direction ( Figure 1 ). The natural seawater continuously pumped from the Seto Inland Sea is continuously flowed to the waterway 10. The flow direction 30 of the natural seawater is from north to south. The water level of the natural seawater flowing in the waterway 10 changes from 40 mm to 200 mm in a cycle of 12 hours, imitating the tide level in nature. The flow rate of the natural seawater flowing in the waterway 10 is matched with the water level and is set from about 30 cm / second (when the water level is the lowest) to about 10 cm / second (when the water level is the highest).

[0254] The test of continuous flow of natural seawater into the waterway 10 was carried out for 12 months, and the attachment area of ​​marine organisms was obtained and evaluated according to the following criteria. The evaluation results at the time point of 6 months and 12 months of the test are shown in Tables 4 to 10. The evaluation result is preferably 3 or more.

[0255] 5: The attachment area of ​​marine organisms is 0% or more and less than 5%

[0256] 4: The attachment area of ​​marine organisms is more than 5% and less than 10%

[0257] 3: The attachment area of ​​marine organisms is more than 10% and less than 15%

[0258] 2: The attachment area of ​​marine organisms is more than 15% and less than 30%

[0259] 1: The attachment area of ​​marine organisms is more than 30%

[0260] [d] Evaluation of storage stability of antifouling coating composition

[0261] 200 mL of the antifouling coating composition was placed in a container, and the stirring properties after storage at 40° C. for 6 months were evaluated according to the following criteria. The evaluation results are shown in Tables 4 to 10. The evaluation results were preferably C or higher.

[0262] A: Can be easily stirred.

[0263] B: Can be stirred.

[0264] C: Can be stirred with a little force.

[0265] D: Difficult to stir.

[0266] E: Cannot be stirred.

[0267] [e] Evaluation of wet-dry adhesion of coatings

[0268] The obtained antifouling coating composition was applied to a sandblasted plate previously coated with an antirust coating, and the dry film thickness was 300 μm, and the plate was dried by placing it indoors for 2 days and nights to obtain a test plate with an antifouling coating film. The obtained test plate was fixed on a raft set up in Aioi Bay, Ako City, Hyogo Prefecture. At this time, the test plate was fixed at a position of about 15 cm above the sea using the raft stand. By fixing the test plate at a position of about 15 cm above the sea, the antifouling coating film repeatedly came into contact and was not in contact with seawater caused by waves.

[0269] The test plate was subjected to a checkerboard adhesion test (gap spacing 2 mm, number of grids 25) in accordance with JIS K 5600.5.6 six months after being fixed to the raft. The results are shown in Tables 4 to 10. The values ​​in the table are obtained by scoring the test results according to the following criteria. The evaluation score is preferably 6 or more.

[0270] Evaluation score 10: Each score is thin and both sides are smooth, and there is no peeling between the intersection of the score and the square grid.

[0271] Evaluation score 8: There is slight peeling at the intersection of the notches, there is no peeling in one square grid, and the area of ​​the defect is within 5% of the area of ​​all squares.

[0272] Evaluation score 6: There is peeling on both sides and at the intersection of the notch, and the area of ​​the defect is 5 to 15% of the total square area.

[0273] Evaluation score 4: The width of the peeling caused by the scratch is wide, and the area of ​​the defect portion is 15 to 35% of the total square area.

[0274] Evaluation score 2: The width of the peeling caused by the scratch is larger than 4 points, and the area of ​​the defect portion is 35 to 65% of the total square area.

[0275] Evaluation point 0: The peeled area is 65% or more of the entire square area.

[0276] [f] Evaluation of coating film drying

[0277] The obtained antifouling coating composition was applied to a sandblasted plate (size: 150×70×3.2 mm) previously coated with an antirust coating using an airless spray gun to a dry film thickness of 160 μm, and dried at 23° C. for 1 day to form a coating film, and this operation was repeated twice to prepare a test plate having an antifouling coating film with a dry film thickness of 320 μm. The obtained test plate was further dried at 23° C. for 7 days.

[0278] A 30×30×10 mm wooden piece was placed on the antifouling coating film (central part) of the dried test plate, and a force of 40 kgf / cm2 was applied vertically (coating film direction) from above the wooden piece. 2 The wood chips were removed and the state of the coating surface (degree of deformation) was visually evaluated according to the following criteria. The evaluation results are shown in Tables 4 to 10. Figure 3 A cross-sectional view schematically showing the coating film state corresponding to each evaluation criterion is also shown in FIG. The evaluation result is preferably 3 or more.

[0279] 5: Slightly visible traces of wood chips.

[0280] 4: Slight deformation is visible around the location where the wood chips are placed.

[0281] 3: Bulging is visible around the area where the wood chips were placed.

[0282] 2: A large bulge is visible around the location where the wood chips are placed.

[0283] 1: The bulge around the location where the wood chips are placed is large and protrudes outward significantly.

[0284] [Table 4]

[0285]

[0286] [Table 5]

[0287]

[0288] [Table 6]

[0289]

[0290] [Table 7]

[0291]

[0292] [Table 8]

[0293]

[0294] [Table 9]

[0295]

[0296] [Table 10]

[0297]

[0298] Explanation of symbols

[0299] 10: water channel; 20: test plate; 25: second adhesive layer; 30: flow direction of natural seawater.

Claims

1. An antifouling coating composition comprising a hydrolyzable resin (A), a first non-hydrolyzable resin (B), a second non-hydrolyzable resin (C) and an antifouling agent (D); wherein The glass transition temperature Tg of the first non-hydrolyzable resin (B) B ℃ and dissolution parameter SP B , and the glass transition temperature Tg of the second non-hydrolyzable resin (C) C ℃ and dissolution parameter SP C Satisfies the following equations [1] to [4]: Tg B - Tg C ≥ 60[1] 10.5 ≥ SP B ≥ 9.5[2] 10.6 ≥ SP C ≥ 9.5[3] |SP B - SP C | ≤ 1.0[4]; And, where Tg B The temperature is in the range of 40°C or more and 80°C or less; In the total amount of 100 mass % of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition, the content of the hydrolyzable resin (A) is 10 mass % or more and 90 mass % or less, the content of the first non-hydrolyzable resin (B) is 2 mass % or more and 50 mass % or less, and the content of the second non-hydrolyzable resin (C) is 2 mass % or more and 50 mass % or less; The content ratio of the first non-hydrolyzable resin (B) to the hydrolyzable resin (A) ((B) / (A)) is 0.02 or more and 1 or less in terms of mass ratio; The content ratio ((C) / (A)) of the second non-hydrolyzable resin (C) to the hydrolyzable resin (A) is 0.01 or more and 1 or less in terms of mass ratio; The content ratio ((B) / (C)) of the first non-hydrolyzable resin (B) to the second non-hydrolyzable resin (C) is 0.05 or more and 9 or less in terms of mass ratio; The total amount of the hydrolyzable resin (A), the first non-hydrolyzable resin (B) and the second non-hydrolyzable resin (C) contained in the antifouling coating composition is 5% by mass or more and 40% by mass or less in 100% by mass of the solid content contained in the antifouling coating composition; The content of the antifouling agent (D) in the antifouling coating composition is 0.3 parts by mass or more and 550 parts by mass or less relative to 100 parts by mass of the hydrolyzable resin (A).

2. The antifouling coating composition according to claim 1, wherein SP B It is in the range of greater than or equal to 9.6 and less than or equal to 10.

3.

3. The antifouling coating composition according to claim 1, wherein Tg C In the range of -50°C or more and -20°C or less, SP C It is in the range of greater than or equal to 9.8 and less than or equal to 10.

6.

4. The antifouling coating composition according to claim 1, wherein the glass transition temperature Tg of the hydrolyzable resin (A) is A In the range of 10°C or more and 80°C or less, the solubility parameter SP A It is in the range of greater than or equal to 8.5 and less than or equal to 9.

7.

5. The antifouling coating composition according to claim 1, wherein the hydrolyzable resin (A) has a silicon atom-containing group represented by the following formula (1): [Chemical formula 1] In formula (1), R 1 , R 2 and R 3 Each independently represents a C1 to C6 hydrocarbon group. 6 . The antifouling coating composition according to claim 1 , further comprising a rosin compound (E). 7 . The antifouling coating composition according to claim 1 , wherein the content ratio of the first non-hydrolyzable resin (B) to the hydrolyzable resin (A) is greater than or equal to 0.1 and less than or equal to 0.45 in terms of mass ratio. 8 . The antifouling coating composition according to claim 1 , wherein the content ratio of the second non-hydrolyzable resin (C) to the hydrolyzable resin (A) is greater than or equal to 0.05 and less than or equal to 0.65 in terms of mass ratio.

9. A coating film formed from the antifouling coating composition according to claim 1.

10. A ship comprising the coating film according to claim 9.

11. An underwater structure comprising the coating film according to claim 9.

Citation Information

Patent Citations

  • Multilayer antifouling coating and coated object having said coating on surface

    WO2020235516A1

  • Stain-proof coating composition, method for production of the composition, stain-proof coating film formed by using the composition, coated article having the coating film on the surface, and stain-pr

    CN101583677A

  • Antifouling coating composition, antifouling film, composite film, and in-water structure

    CN102686683A

  • Anti-pollution coating composition and coating objects provided with coating films

    CN106905802A