A diffusion connection method for hollow ring components

By using a diffusion bonding system and multi-level step compensation technology, the problems of low material utilization and low efficiency in the processing of hollow titanium alloy ring parts were solved, achieving efficient preforming and diffusion bonding, ensuring processing quality and automated demolding.

CN117506350BActive Publication Date: 2026-11-17BEIJING HANGXING MACHINERY MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311689765.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2026-11-17
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

Existing processing methods for hollow titanium alloy rings result in low material utilization, difficulty in mass production, long production cycles, and low processing efficiency.

Method used

The diffusion bonding system, including a preforming device and a diffusion bonding device, is adopted. Through steps such as blank preparation, bending and forming, chemical milling and hole enlargement, machining and finishing, and vacuum diffusion bonding, the processing quality is ensured by using multi-level steps and compensation blocks, and automatic demolding and unloading are achieved through the ejector unit and unloading slide.

Benefits of technology

This approach achieves efficient material utilization, improves preforming processing efficiency and diffusion bonding efficiency, ensures processing quality and automated demolding, and reduces processing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117506350B_ABST
    Figure CN117506350B_ABST
Patent Text Reader

Abstract

This invention relates to a diffusion joining method for hollow ring parts, belonging to the field of precision plastic processing technology. It solves the problems of low material utilization, inconvenience for mass production, long production cycles, and low processing efficiency in existing forming and processing technologies. The diffusion joining method for hollow ring parts of this invention includes the following steps: A. Preparing the blank; B. Bending and forming; C. Chemical milling and hole enlargement; D. Machining and finishing; E. Vacuum diffusion joining; F. Completing vacuum diffusion joining. The diffusion joining method of this invention directly uses sheet metal cutting, eliminating material waste and achieving high material utilization; multiple blanks are extruded simultaneously, resulting in high pre-forming processing efficiency; and multiple diffusion joining modules are simultaneously placed in the joining furnace, further enhancing diffusion joining efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of precision plastic forming technology, and in particular to a diffusion connection method for hollow ring parts. Background Technology

[0002] Titanium alloy hollow ring components, represented by end frames, are mostly lightweight load-bearing structural parts. Conventional forging and machining methods are difficult to implement for titanium alloy hollow ring components. A method that uses thick plates for machining or casting to form a ring half-cavity, and then applying axial force to diffuse and connect them, can achieve the forming of the ring cavity structure.

[0003] Although the above processing methods can realize the processing of hollow titanium alloy ring parts, the material utilization rate is very low when machining the ring half cavity with a thick plate machine; the production cycle of casting the ring half cavity is long and the processing efficiency is low. Both of the above manufacturing methods lead to increased processing costs.

[0004] Therefore, there is an urgent need for a diffusion connection method for hollow ring components to solve the problems of low material utilization, inconvenience for mass production, long production cycle, and low processing efficiency. Summary of the Invention

[0005] Based on the above analysis, the present invention aims to provide a diffusion connection method for hollow ring parts to solve the problems of low material utilization, inconvenience for mass production, long production cycle and low processing efficiency of existing forming and processing technologies.

[0006] The objective of this invention is mainly achieved through the following technical solutions:

[0007] A diffusion connection method for a hollow ring component utilizes a diffusion connection system; the diffusion connection system includes a preforming device and a diffusion connection device.

[0008] The diffusion connection method includes the following steps:

[0009] A. Prepare the blank;

[0010] B. Bending and shaping;

[0011] C. Chemical milling for hole enlargement;

[0012] D. Machining and finishing;

[0013] E. Vacuum diffusion connection;

[0014] F. Complete the vacuum diffusion connection.

[0015] Furthermore, the D, machining finishing includes: machining the semi-finished blank to remove excess material at both ends; and machining a diffusion connection interface.

[0016] Furthermore, prior to step E and vacuum diffusion connection, the method includes the step of fabricating a diffusion connection module.

[0017] Furthermore, the fabrication of the diffusion connection module includes: placing the third positioning block and the fourth positioning block on the second positioning block, and connecting the side limiting block to the side limiting notch.

[0018] Furthermore, the fabrication of the diffusion connection module also includes: placing two finished blanks in the positioning hollow part and splicing them into a hollow ring.

[0019] Furthermore, the fabrication of the diffusion connection module also includes: placing a central limiting block into the hollow ring component.

[0020] Furthermore, the fabrication of the diffusion connection module also includes: fabricating multiple diffusion connection modules.

[0021] Furthermore, the cutting dimensions of the blank are 54mm × 35mm × 805mm.

[0022] Further, step A, preparing the blank, includes drilling a through hole with a diameter of Φ5mm along the length of the blank.

[0023] Furthermore, C, chemical milling and hole enlargement, includes: chemically milling the through hole to expand the Φ5mm hole to Φ20mm.

[0024] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0025] (1) The diffusion connection method of the present invention directly selects sheet material for cutting, so there is no material waste and the material utilization rate is high; multiple blanks are extruded and formed at the same time, and the pre-forming processing efficiency is high; multiple diffusion connection modules are placed in the connection furnace at the same time, and the diffusion connection efficiency is high; during demolding, the semi-finished blank can be demolded by itself and lifted by the top plate; if the semi-finished blank hugs the punch body, an iron sheet is inserted into the notch and pressed between the punch body and the semi-finished blank to separate the semi-finished blank from the punch body; because the length of the second support rod is less than the length of the first support rod, the unloading slide has a slope, and the semi-finished blank can slide down on the inclined unloading slide by itself to complete the automatic unloading;

[0026] (2) The diffusion connection system of the present invention has a multi-level step, including a first level step, a second level step and a third level step. During the pre-forming process, it ensures that the vertices of the outer surface of the punch body can be connected to the midpoint of the semi-circular ring blank, 1 / 3 circular ring blank or 1 / 4 circular ring blank, thereby pressing the semi-circular ring blank, 1 / 3 circular ring blank or 1 / 4 circular ring blank into a semi-circular ring semi-finished blank, 1 / 3 circular ring semi-finished blank or 1 / 4 circular ring semi-finished blank with left and right symmetry, thus ensuring the quality of the pre-forming process;

[0027] (3) The compensation block of the diffusion connection system of the present invention is used to fill the second or third step, and compensate the inner surface of the first die seat into a complete semi-circular arc surface to ensure the pre-forming quality of the semi-circular ring semi-finished blank and the 1 / 3 ring semi-finished blank; the end faces of the first step and the second step are provided with fixing grooves, and the fixing strip can be inserted into the fixing groove to connect the first block to the first step and the second block to the second step, thereby compensating the inner surface of the first die seat;

[0028] (4) The fixing groove of the diffusion connection system of the present invention is a dovetail groove, and the fixing strip is a trapezoidal strip. The fixing strip cannot be disengaged from the fixing groove in the direction of the inner surface of the first die seat, so as to prevent the compensation block from disengaging from the step.

[0029] (5) The top material unit of the diffusion connection system of the present invention includes a top material plate and a top material support rod. After the preforming is completed, the thermoforming machine can support the top material support rod. The top material support rod drives the top material plate to push the semi-finished blank out of the die and complete the demolding. Attached Figure Description

[0030] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0031] Figure 1 This is a flowchart illustrating the diffusion connection method.

[0032] Figure 2 This is a schematic diagram of the overall structure of the billet;

[0033] Figure 3 This is a schematic diagram of the overall structure of the semi-finished blank;

[0034] Figure 4 This is a schematic diagram of the overall structure of the finished blank;

[0035] Figure 5 This is a schematic diagram of the overall structure of the hollow ring component;

[0036] Figure 6 This is a schematic diagram of the overall structure of the diffusion connection system;

[0037] Figure 7 This is a schematic diagram of the overall structure of the preforming mold in Example 2;

[0038] Figure 8 This is a schematic diagram of the overall structure of the first punch holder;

[0039] Figure 9 This is a schematic diagram of the overall structure of the steps;

[0040] Figure 10 A schematic diagram of the overall structure of the compensation block;

[0041] Figure 11 A schematic diagram of the overall structure of the first punch seat when the compensation block is connected to the step;

[0042] Figure 12 This is a schematic diagram of the overall structure of the preforming mold in Example 3;

[0043] Figure 13 This is a schematic diagram of the overall structure of the preforming device;

[0044] Figure 14 This is a schematic diagram of the overall structure of a thermoforming machine;

[0045] Figure 15 A schematic diagram of the overall structure of the diffusion connection mold;

[0046] Figure label:

[0047] 1-Pre-forming mold; 2-Thermoforming machine; 3-Diffusion bonding mold; 4-Connecting furnace; 11-Punch; 12-Die; 13-Pull frame; 14-Ejector unit; 15-Unloading rack; 16-Unloading rod; 21-Machine body; 22-Pressure rod; 23-Ejector rod; 24-First door; 25-Second door; 31-First positioning block; 32-Second positioning block; 33-Third positioning block; 34-Fourth positioning block; 35-Center limiting block; 36-Side limiting block; 37-Side limiting notch; 38-Side ejector rod; 39-Pin; 100-Hollow ring; 101-Blank; 102- 103-Finished blank; 104-Through hole; 111-Top plate; 112-Punch body; 113-Notch; 121-First die holder; 122-Step; 123-Compensating stop; 124-Fixing strip; 125-Fixing groove; 126-Second die holder; 127-Positioning assembly; 141-Ejector plate; 142-Ejector support rod; 1221-First step; 1222-Second step; 1223-Third step; 1231-First stop; 1232-Second stop; 1261-First positioning block; 1262-Second positioning block. Detailed Implementation

[0048] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0049] Example 1

[0050] A specific embodiment of the present invention, such as Figure 1 As shown, a diffusion connection method for hollow ring parts (hereinafter referred to as diffusion connection method) is disclosed, which uses a diffusion connection system to complete the vacuum diffusion connection of hollow ring parts 100.

[0051] In this embodiment, the hollow ring is made of TA15 titanium alloy with an axial thickness of 50mm, an outer diameter of Φ360mm, and an inner diameter of Φ300mm. The hollow cross-section of the hollow ring is a circle with a diameter of Φ20mm. The blank 101 is a semi-circular ring blank, and the finished blank 103 is a semi-circular ring finished blank.

[0052] like Figure 2 and Figure 3 As shown, the blank 101 is a strip-shaped titanium alloy blank, which is formed by stamping sheet metal. The blank 101 has through holes 104, which are formed into the hollow part of the hollow ring part 100 after pre-forming and main forming processes. Due to different material compositions, the blank 101 can be directly stamped to different lengths. The blank 101 can be a semi-circular ring blank, a 1 / 3 circular ring blank, or a 1 / 4 circular ring blank. The length of the semi-circular ring blank is greater than the length of the 1 / 3 circular ring blank, and the length of the 1 / 3 circular ring blank is greater than the length of the 1 / 4 circular ring blank.

[0053] like Figure 4 and Figure 5 As shown, the hollow ring part 100 is formed by diffusion connection of multiple finished blanks 103, and the finished blanks 103 are obtained by cutting semi-finished blanks 102. There are 2-4 finished blanks 103, which are respectively semi-circular finished blanks, 1 / 3 circular finished blanks, or 1 / 4 circular finished blanks.

[0054] The diffusion connection method in this embodiment includes the following steps:

[0055] Step 1: Prepare billet 101, including the following sub-steps:

[0056] Step 11: Material feeding

[0057] Prepare the sheet metal;

[0058] Preferably, the sheet material is a TA15 titanium alloy plate with a thickness of 35mm and a width of 805mm, with an axial thickness allowance of 4mm.

[0059] Step 12: Cutting

[0060] The titanium alloy sheet is hydraulically cut, and the blank 101 is cut to a size of 54mm×35mm×805mm.

[0061] Step 13: Drilling

[0062] A through hole 104 with a length of 805 mm and a diameter of Φ5 mm is drilled in the length direction of the blank 101 using a deep hole drill.

[0063] By directly selecting sheet metal for cutting, there is no waste of materials, and the material utilization rate is high.

[0064] Step 2: Bending and shaping, including the following sub-steps:

[0065] Step 21: Assemble the thermoforming equipment

[0066] Open the first door 24 and fix one end of the punch 11 to the pressure rod 22;

[0067] There are two scenarios:

[0068] Case 1: The first die holder 121 of Embodiment 1 is fixedly connected to the machine body 21, and the ejector support rod 142 is connected to the ejector rod 23;

[0069] Case 2: The second die holder 126 of Example 2 is fixedly connected to the machine body 21, and the ejector rod 142 is connected to the ejector rod 23.

[0070] Step 22: Heating the preforming mold

[0071] Close the first door 24, turn on the pre-forming heating unit, raise the temperature inside the machine body 21 to 700℃-750℃ and keep it warm for 10 minutes.

[0072] Step 23: Load the blank 101

[0073] Open the first door 24:

[0074] Case 1: Place multiple blanks 101 on the first step 1221, connect the first stop 1231 to the first step 1221, and connect the second stop 1232 to the second step 1222 to compensate the inner surface of the first die holder 121.

[0075] Case 2: Place the first positioning block 271 and the second positioning block 272 on the platform of the second die holder 126, insert a positioning pin into the positioning pin hole, and fix the positioning component 127 and the second die holder 126 together; place multiple blanks 101 on the first positioning block 271.

[0076] Close the first door 24;

[0077] Keep warm for 15 minutes.

[0078] Step 24: Extrusion and mold closing

[0079] Press down the pressure rod 22, and the punch 11 extrudes the blank 101 towards the die 12 until the axis of the punch coincides with the axis of the die, extruding the blank 101 into a semi-finished blank 102.

[0080] Multiple blanks 101 are extruded and formed simultaneously, resulting in high pre-forming processing efficiency.

[0081] Step 3: Demolding

[0082] The first press drives the pressure rod 22 to pull up the punch 11, and the second press drives the ejector rod 23 to push the ejector unit upward.

[0083] Preferably, the push rod 23 moves upward by 35mm-60mm, and the pressure rod 22 moves upward by 60mm-85mm; due to its own weight, the semi-finished blank 102 can be demolded by itself and lifted by the top plate 141 at this time;

[0084] Open the first door 24 and the second door 25 to cool the pre-forming mold and the semi-finished blank 102;

[0085] Preferably, if the semi-finished blank 102 hugs the punch body 112, an iron sheet is inserted into the notch 113 and pressed between the punch body 112 and the semi-finished blank 102, the semi-finished blank 102 is separated from the punch body 112.

[0086] Step 4: Unloading

[0087] The unloading rods 16 are inserted sequentially into the unloading rod holes of the second support rod 52 and the first support rod 51, and the two unloading rods 16 form an unloading slide.

[0088] Because the length of the second support rod 52 is less than the length of the first support rod 51, the unloading slide has a slope;

[0089] The second press drives the push rod 23 and lowers the push unit. The semi-finished billet 102 is lifted by the unloading slide and slides on the inclined unloading slide to one side of the first support rod 51.

[0090] When the unloading rod 16 is pulled away from the second support rod 52, the semi-finished billet 102 slides out and falls under the action of gravity, completing the automatic unloading.

[0091] Step 5: Chemical milling and hole enlargement

[0092] Chemical milling was performed on through hole 104 to expand the Φ5mm hole to Φ20mm.

[0093] Step 6: Machining and Finishing

[0094] The semi-finished blank 102 is machined to remove the excess at both ends, and a diffusion connection interface is machined to complete the production of the finished blank 103.

[0095] Step 7: Create the diffusion connection module, including the following sub-steps:

[0096] Step 71: Place the third positioning block 33 and the fourth positioning block 34 on the second positioning block 32, and connect the side limiting block 36 to the side limiting notch 37.

[0097] Step 72: Place the two finished blanks 103 in the positioning hollow part and assemble them into a hollow ring part 100; put the central limiting block 35 into the hollow ring part 100;

[0098] Step 73: Place the first positioning block 31 on the third positioning block 33 and the fourth positioning block 34, and connect the side limiting block 36 to the side limiting notch 37;

[0099] Step 74: Place the first positioning block 31 on the third positioning block 33 and the fourth positioning block 34, and connect the side limiting block 36 to the side limiting notch 37.

[0100] Repeat this step to create multiple diffusion connection modules.

[0101] Step 8: Vacuum diffusion connection

[0102] Multiple diffusion connection modules are stacked and placed into the connection furnace 4, and the side top rod 38 is connected to the side top cylinder;

[0103] Adjust the side push rod 38 to eliminate the gap between the third positioning block 33 and the fourth positioning block 34 and the side push cylinder;

[0104] Vacuum is drawn inside furnace 4, and the diffusion heating unit is turned on;

[0105] The diffusion heating unit heats the furnace body to 910-930℃ and performs vacuum diffusion connection on the hollow ring 100.

[0106] Step 9: Complete vacuum diffusion connection

[0107] Gas is introduced into furnace 4 and then cooled;

[0108] Remove the diffusion connection module from connection furnace 4;

[0109] Remove the hollow ring 100 to complete the diffusion connection.

[0110] Compared with existing technologies, directly using sheet metal eliminates material waste and increases material utilization; multiple blanks 101 are extruded simultaneously, resulting in high preforming processing efficiency; the preforming heating unit can heat to 700-750℃, and the thermoforming machine 2 can maintain this temperature range, which is beneficial for plastic preforming of the blanks 101 and ensures preforming processing accuracy; during demolding, due to its own gravity, the semi-finished blank 102 can demold itself and be lifted by the top plate 141; if the semi-finished blank 102 hugs the punch body 112, an iron sheet is inserted into the notch 113 and pressed between the punch body 112 and the semi-finished blank 102, separating the semi-finished blank 102 from the punch body 112; because the length of the second support rod 52 is less than the length of the first support rod 51, the unloading slide has a slope, and the semi-finished blank 102 can slide down on the inclined unloading slide to complete automatic unloading.

[0111] Example 2

[0112] Another specific embodiment of the present invention, such as Figure 6 As shown, a diffusion joining system for implementing the diffusion joining method of Embodiment 1 is disclosed, including a preforming device and a diffusion joining device. The preforming device includes a preforming mold 1 and a thermoforming machine 2, with the preforming mold 1 disposed within the thermoforming machine 2. The diffusion joining device includes a diffusion joining mold 3 and a joining furnace 4, with the diffusion joining mold 3 disposed within the joining furnace 4. The preforming device is used to press a blank 101 into a semi-finished blank 102; the semi-finished blank 102 is machined to form a finished blank 103; the diffusion joining device is used to diffusely join multiple finished blanks 103 to form a hollow ring 100.

[0113] Preferably, such as Figure 7 As shown, the preforming mold 1 includes a punch 11 and a die 12. The punch 11 is used to press down the blank 101, and the die 12 presses the blank 101 into a semi-finished blank 102.

[0114] Preferably, the punch 11 includes a top plate 111 and a punch body 112, with the punch body 112 disposed at one end of the top plate 111. The top plate 111 is used to connect to the thermoforming machine 2, and the punch body 112 has an outer surface and a punch axis. The outer surface is a semi-circular arc surface, and the punch body 112 is used to press the blank 101 into a semi-finished blank 102.

[0115] Preferably, the punch 11 further includes a notch 113, which is located at one end of the outer surface and is a groove parallel to the punch axis. After the semi-circular ring semi-finished blank is bent and formed, it may tightly grip the outer surface of the punch body 112, making demolding difficult. Inserting an iron sheet into the notch 113 and pressing it between the punch body 112 and the semi-circular ring semi-finished blank can separate the semi-circular ring semi-finished blank from the punch body 112, facilitating demolding. Preferably, there are two notches 113, respectively located at both ends of the punch arc surface, facilitating demolding from both sides of the punch 11.

[0116] Preferably, the punch 11 further includes a first hollow portion, which is disposed on the top plate 111 and the punch body 112. The punch body 112 also includes a punch outer wall, which encloses the first hollow portion to reduce the weight of the punch 11. The thickness of the punch outer wall is the same at all points, so that the punch 11 can be heated evenly during the heating process of the thermoforming machine 2.

[0117] Preferably, such as Figure 8 As shown, the die 12 includes a first die base 121 and steps 122. The first die base 121 includes an opening into which the punch 11 can be inserted. The steps 122 are disposed at both ends of the opening. The first die base 121 includes an inner surface and a die axis. The inner surface is a semi-circular arc surface. The two steps 122 are symmetrically arranged with respect to the die axis. The distance between the two steps 122 is not less than the length of the blank 101. The two steps 122 are used to place the blank 101, so that the first die base 121 and the punch body 112 can press the blank 101 into a semi-finished blank 102 together.

[0118] Preferably, such as Figure 9 As shown, step 122 is a multi-level step, including a first-level step 1221, a second-level step 1222, and a third-level step 1223. The two ends of the second-level step 1222 are connected to the first-level step 1221 and the third-level step 1223, respectively. The two first-level steps 1221 are used to place the semi-circular ring blank, the two second-level steps 1222 are used to place the 1 / 3 circular ring blank, and the two third-level steps 1223 are used to place the 1 / 4 circular ring blank. During preforming, it is ensured that the vertices of the outer surface of the punch body 112 can be connected to the midpoint of the semi-circular ring blank, the 1 / 3 circular ring blank, or the 1 / 4 circular ring blank, thereby pressing the semi-circular ring blank, the 1 / 3 circular ring blank, or the 1 / 4 circular ring blank into symmetrical semi-circular ring semi-finished blanks, 1 / 3 circular ring semi-finished blanks, or 1 / 4 circular ring semi-finished blanks, ensuring the quality of preforming.

[0119] like Figure 10 and Figure 11As shown, during the processing of the semi-circular ring blank and the 1 / 3 circular ring blank, the semi-circular ring blank and the 1 / 3 circular ring blank will connect with the second-level step 1222 and the third-level step 1223, thereby destroying the final formed shape of the semi-circular ring blank and the 1 / 3 circular ring blank, causing quality defects. Preferably, the die 12 also includes a compensation block 123, which can connect with the second-level step 1222 or the third-level step 1223 to fill the second-level step 1222 or the third-level step 1223, compensating the inner surface of the first die holder 121 into a complete semi-circular arc surface, ensuring the pre-forming processing quality of the semi-circular ring blank and the 1 / 3 circular ring blank.

[0120] Preferably, the compensation block 123 includes a first block 1231 and a second block 1232. One end of the first block 1231 and the second block 1232 is provided with a fixing strip 124. The end faces of the first step 1221 and the second step 1222 are provided with fixing grooves 125. The fixing strip 124 can be inserted into the fixing groove 125, which can connect the first block 1231 to the first step 1221 and the second block 1232 to the second step 1222, thereby compensating for the inner surface of the first die holder 121.

[0121] Preferably, the fixing groove 125 is a dovetail groove and the fixing strip 124 is a trapezoidal strip. The fixing strip 124 cannot disengage from the fixing groove 125 in the direction of the inner surface of the first die seat 121, thus preventing the compensation block 123 from disengaging from the step 122.

[0122] Preferably, the die cavity 12 further includes a second hollow portion disposed within the first die cavity base 121. The first die cavity base 121 also includes a die cavity outer wall, which encloses the second hollow portion to reduce the weight of the die cavity 12. The thickness of the die cavity outer wall is uniform throughout, ensuring that the die cavity 12 is heated evenly during the heating process in the thermoforming machine 2.

[0123] Preferably, such as Figure 7 As shown, the preforming mold in this embodiment also includes a pull frame 13. The pull frame 13 is a square frame through which the punch 11 can pass. The pull frame 13 is located at both ends of the opening, and both ends of the pull frame 13 can be connected to the steps 122. The pull frame 13 is used to pull the two steps 122 to prevent the die 12 from deforming under stress during the preforming process and to increase the strength of the die 12.

[0124] Preferably, the preforming mold in this embodiment further includes an ejector unit 14, which is disposed on the die cavity 12. The ejector unit 14 includes an ejector plate 141 and an ejector support rod 142. The ejector plate 141 is disposed at the bottom of the opening of the first die cavity 121, and the ejector support rod 142 passes through the first die cavity 121. The two ends of the ejector support rod 142 are respectively connected to the ejector plate 141 and the thermoforming machine 2. After preforming is completed, the thermoforming machine 2 can support the ejector support rod 142, and the ejector support rod 142 drives the ejector plate 141 to eject the semi-finished blank 102 out of the die cavity 12, thus completing the demolding.

[0125] Preferably, the end face of the top plate 141 is an arc surface, and the arc of the inner surface of the first die holder 121 is the same, so as to ensure that the arc of the semi-finished blank 102 is consistent and to ensure the pre-forming quality of the semi-finished blank 102.

[0126] Preferably, to facilitate unloading, the preforming mold in this embodiment further includes an unloading unit, which is disposed on the punch 11. The unloading unit includes an unloading frame 15 and an unloading rod 16. The unloading frame 15 is L-shaped, one end of the unloading frame 15 is connected to the punch body 112, and the other end of the unloading frame 15 is provided with an unloading rod hole. The unloading rod 16 can be inserted into the unloading rod hole and connected to the unloading frame 15.

[0127] Preferably, such as Figure 12 As shown, the unloading rack 15 includes a first support rod 51 and a second support rod 52. The first support rod 51 is located on one side of the punch body 112, and the second support rod 52 is located on the other side of the punch body 112. There are two first support rods 51 and two support rods 52, and the length of the second support rod 52 is less than the length of the first support rod 51. The two ends of the unloading rod 16 are respectively inserted into the unloading rod holes of the first support rod 51 and the second support rod 52, and the two unloading rods 16 form an unloading slide. Because the length of the second support rod 52 is less than the length of the first support rod 51, the unloading slide has a slope. During unloading, the unloading slide can support the semi-finished blank 102, and the semi-finished blank 102 can slide on the inclined unloading slide to the side of the first support rod 51, which facilitates the unloading operation of the preforming mold in this embodiment.

[0128] Preferably, such as Figure 13 and Figure 14 As shown, the preforming mold 1 is set inside the thermoforming machine 2. The thermoforming machine 2 includes a machine body 21, a pressure rod 22, an ejector rod 23, a first door 24 and a second door 25. The pressure rod 22, the ejector rod 23, the first door 24 and the second door 25 are all set on the machine body 21.

[0129] Preferably, the top plate 111 can be fixedly connected to the pressure rod 22, which is used to press down the punch 11. The first die holder 121 or the second die holder 126 can be fixedly connected to the machine body 21. The ejector support rod 142 can be connected to the ejector rod 23, which is used to support the ejector support rod 142. The ejector support rod 142 drives the ejector plate 141 to eject the semi-finished blank 102 out of the die 12, thus completing the demolding. The pressure rod 22 is connected to the first press (not shown in the figure), which is used to drive the pressure rod 22 to move up and down. The ejector rod 23 is connected to the second press (not shown in the figure), which is used to drive the ejector rod 23 to move up and down.

[0130] Preferably, the thermoforming machine 2 further includes a preforming heating unit (not shown in the figure), which is used to heat the inside of the machine body 21 and to keep the preforming mold and blank 101 warm; the first door 24 and the second door 25 are respectively disposed at both ends of the machine body 21, and the first door 24 and the second door 25 are used to seal the machine body 21 to prevent the heat inside the machine body 21 from leaking out.

[0131] Titanium alloys exhibit significantly reduced deformation resistance under hot conditions and good plasticity. The preforming heating unit can heat the material to 700-750℃, and the hot forming machine 2 can maintain this temperature range, which is beneficial for plastic preforming of the blank 101 and ensures the accuracy of preforming.

[0132] Preferably, such as Figure 15 As shown, the diffusion connection mold 3 includes a first positioning block 31, a second positioning block 32, a third positioning block 33, and a fourth positioning block 34. Both the third positioning block 33 and the fourth positioning block 34 have recessed portions. The third positioning block 33 and the fourth positioning block 34 can be mounted on the second positioning block 32. The recessed portions of the third positioning block 33 and the fourth positioning block 34 form a positioning hollow portion, in which the hollow ring component 100 can be mounted. The third positioning block 33 and the fourth positioning block 34 prevent the radial separation of multiple finished blanks 103. The first positioning block 31 is mounted on the third positioning block 33 and the fourth positioning block 34 and presses down on the hollow ring component 100. The first positioning block 31 and the second positioning block 32 prevent the axial separation of multiple finished blanks 103, and the third positioning block 33 and the fourth positioning block 34 ensure the axial length of the hollow ring component 100.

[0133] Preferably, in order to prevent radial deformation of the hollow ring 100, the diffusion connection mold 3 further includes a central limiting block 35. The central limiting block 35 is a cylindrical limiting block. The central limiting block 35 is disposed between the first positioning block 31 and the second positioning block 32 and can be placed inside the hollow ring 100. The central limiting block 35 is used to radially support the hollow ring 100 and prevent radial deformation of the hollow ring 100 during diffusion connection.

[0134] Preferably, the first positioning block 31 and the second positioning block 32 have the same structure, and the third positioning block 33 and the fourth positioning block 34 have the same structure. Side limiting blocks 36 are provided at both ends of the first positioning block 31 and both ends of the second positioning block 32, and side limiting notches 37 are provided at both ends of the third positioning block 33 and both ends of the fourth positioning block 34. The side limiting blocks 36 can connect with the side limiting notches 37. The side limiting blocks 36 and the side limiting notches 37 are used to limit the third positioning block 33 and the fourth positioning block 34, preventing deformation of the hollow positioning portion and ensuring the quality of the diffusion connection processing.

[0135] The first positioning block 31, the second positioning block 32, the third positioning block 33, the fourth positioning block 34, the center limiting block 35, and the hollow ring 100 constitute a diffusion connection module. Multiple diffusion connection modules can be placed in the connection furnace 4 at the same time to make full use of the furnace space and improve the diffusion connection efficiency.

[0136] Preferably, to ensure that the multiple finished billets 103 can be reliably diffused and connected, the third positioning block 33 and the fourth positioning block 34 need to radially compress the hollow ring 100. The connecting furnace 4 includes a side-top cylinder (not shown in the figure), which can push the third positioning block 33 and the fourth positioning block 34. To ensure that the side-top cylinder can be reliably connected to the third positioning block 33 and the fourth positioning block 34, a side-top rod 38 is provided on the third positioning block 33 and the fourth positioning block 34. The side-top rod 38 is provided on the side wall of the third positioning block 33 and the fourth positioning block 34.

[0137] Preferably, the third positioning block 33 and the fourth positioning block 34 are further provided with side push rod holes, and the side push rod 38 is disposed in the side push rod holes; the side push rod 38 is a side push rod that can be adjusted in length so as to effectively eliminate the gap between the third positioning block 33 and the fourth positioning block 34 and the side push cylinder.

[0138] In an optional embodiment, the side push rod 38 is threadedly connected to the side push rod hole. Rotating the side push rod 38 can adjust the length of the side push rod 38 protruding from the side wall of the third positioning block 33 and the fourth positioning block 34.

[0139] In another optional embodiment, the third positioning block 33 and the fourth positioning block 34 are also provided with pins 39, and the side push rod 38 and the side push rod hole are both provided with pin holes. The side push rod 38 and the side push rod hole are connected by pins 39. The pins 39 connect the side push rod 38 to different pin holes, which can adjust the length of the side push rod 38 protruding from the side wall of the third positioning block 33 and the fourth positioning block 34.

[0140] Preferably, the connecting furnace 4 further includes a furnace body (not shown in the figure) and a diffusion heating unit (not shown in the figure), both of which are disposed in the furnace body. A negative pressure can be formed inside the furnace body by evacuation, and the diffusion heating unit can heat the furnace body to 910-930°C. The connecting furnace 4 is used for vacuum diffusion connection of the hollow ring component 100.

[0141] Compared to existing technologies, the preforming mold step 122 in this embodiment is a multi-level step, including a first-level step 1221, a second-level step 1222, and a third-level step 1223. During preforming, this ensures that the vertices of the outer surface of the punch body 112 can connect with the midpoints of the semi-circular ring blank, 1 / 3 circular ring blank, or 1 / 4 circular ring blank, thereby pressing the semi-circular ring blank, 1 / 3 circular ring blank, or 1 / 4 circular ring blank into symmetrical semi-circular ring semi-finished blanks, 1 / 3 circular ring semi-finished blanks, or 1 / 4 circular ring semi-finished blanks, ensuring the quality of the preforming process. The compensation block 123 is used to fill the second-level step 1222 or the third-level step 1223, compensating the inner surface of the first die holder 121 into a complete semi-circular arc surface, ensuring the semi-circular ring semi-finished blank and 1 / 3 circular ring semi-finished blank are symmetrically formed. The pre-forming quality of the annular semi-finished blank; the compensation block 123 includes a first block 1231 and a second block 1232. One end of the first block 1231 and the second block 1232 is provided with a fixing strip 124. The end faces of the first step 1221 and the second step 1222 are provided with fixing grooves 125. The fixing strip 124 can be inserted into the fixing groove 125, which can connect the first block 1231 to the first step 1221 and the second block 1232 to the second step 1222, thereby compensating for the inner surface of the first die seat 121. The fixing groove 125 is a dovetail groove, and the fixing strip 124 is a trapezoidal strip. The fixing strip 124 cannot detach from the fixing groove 125 in the direction of the inner surface of the first die seat 121, thus preventing the compensation block 123 from detaching from the step 122.

[0142] Ejector unit 14 includes an ejector plate 141 and an ejector support rod 142. After preforming, the thermoforming machine 2 can support the ejector support rod 142, which drives the ejector plate 141 to eject the semi-finished blank 102 out of the die 12, completing demolding. The unloading unit includes an unloading rack 15 and unloading rods 16, with the two unloading rods 16 forming an unloading slide. During unloading, the unloading slide can support the semi-finished blank 102, and the semi-finished blank 102 can be tilted... The material slides onto the first support rod 51 on the unloading slide, facilitating the unloading operation of the preforming mold in this embodiment; the ejector rod 23 of the thermoforming machine 2 in this embodiment can support the ejector support rod 142, and the ejector support rod 142 drives the ejector plate 141 to eject the semi-finished blank 102 out of the cavity mold 12, completing the demolding; the preforming heating unit can heat to 700-750℃ and maintain this temperature range, which is beneficial for the preforming processing of the blank 101 and ensures the accuracy of the preforming processing.

[0143] Multiple diffusion connection modules can be placed simultaneously in the connecting furnace 4 to make full use of the furnace space and improve diffusion connection efficiency; the first positioning block 31 presses down the hollow ring 100, the first positioning block 31 and the second positioning block 32 prevent multiple finished billets 103 from separating axially, and the third positioning block 33 and the fourth positioning block 34 ensure the axial length of the hollow ring 100; the side push rod 38 is a side push rod that can be adjusted in length; the side push rod 38 is threadedly connected to the side push rod hole, or the pin 39 connects the side push rod 38 to different pin holes, both of which can adjust the length of the side push rod 38 protruding from the side wall of the third positioning block 33 and the fourth positioning block 34, so as to effectively eliminate the gap between the third positioning block 33 and the fourth positioning block 34 and the side push cylinder.

[0144] Example 3

[0145] Another specific embodiment of the present invention, such as Figure 12 As shown, another diffusion connection system is disclosed, which improves the cavity 12 of Embodiment 2.

[0146] Preferably, the die cavity 12 includes a second die cavity base 126 and a positioning component 127. The second die cavity base 126 includes an opening, with platforms at both ends of the opening. The platforms are used to place a 1 / 4 circular ring blank and press it into a 1 / 4 circular ring semi-finished blank. The positioning component 127 can be disposed on the platform to expand the inner surface of the first die cavity base 121 until it is compensated into a complete semi-circular arc surface.

[0147] Preferably, the positioning component 127 includes a first positioning block 271 and a second positioning block 272. The second positioning block 272 can be set on the platform and is used to place a 1 / 3 circular billet and press it into a 1 / 3 circular semi-finished billet. The first positioning block 271 can be set on the second positioning block 272 and is used to place a semi-circular billet and press it into a semi-circular semi-finished billet.

[0148] Preferably, both the second die holder 126 and the positioning component 127 are provided with positioning pin holes (not shown in the figure). A positioning pin (not shown in the figure) is inserted into the positioning pin hole. The positioning pin can fix the positioning component 127 and the second die holder 126 together to prevent the positioning component 127 from detaching from the second die holder 126.

[0149] Compared to the die 12 in Embodiment 2, this embodiment only requires placing the required positioning component 127 on the platform of the second die holder 126 according to the processing requirements, which is simple to operate and saves processing time.

[0150] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method of diffusion bonding a hollow toroidal member, characterized by, The system utilizes a diffusion connection system, including a preforming device. The preforming device includes a preforming mold and a thermoforming machine. The preforming mold includes a punch, a die, and an ejector unit. The ejector unit includes an ejector plate and an ejector support rod. The ejector plate is positioned at the bottom of the opening of the first die holder of the die. The ejector support rod passes through the first die holder, and its two ends are connected to the ejector plate and the thermoforming machine, respectively. The die also includes steps and compensating stops. The steps are positioned at both ends of the opening of the first die holder, and the steps include a first-level step, a second-level step, and a third-level step. The two ends of the second-level step are connected to the first-level step and the third-level step, respectively. The two first-level steps are used to place the semi-circular ring blank, the two second-level steps are used to place the 1 / 3 circular ring blank, and the two third-level steps are used to place the 1 / 4 circular ring blank. The compensation block includes a first block and a second block. The ends of the first block and the second block are provided with fixing strips. The end faces of the first step and the second step are provided with fixing grooves. The fixing strips can be inserted into the fixing grooves to connect the first block to the first-level step and the second block to the second-level step. The method includes the following steps: A. Prepare the blank; B. Bending and forming: Place multiple blanks on the first step, connect the first stop to the first step, connect the second stop to the second step, and compensate the inner surface of the first die holder. The punch extrudes the blank towards the die, extruding the blank into a semi-finished blank; Demolding: The ejector unit moves upward; the thermoforming machine supports the ejector rod, which drives the ejector plate to eject the semi-finished blank out of the die, thus completing the demolding; C. Chemical milling for hole enlargement; D. Machining and finishing; E. Vacuum diffusion connection; F. Complete the vacuum diffusion connection.

2. The diffusion bonding method of hollow circular ring members according to claim 1, characterized by, The D. machining finishing includes: machining the semi-finished blank to remove excess material at both ends; and machining a diffusion connection interface.

3. The diffusion bonding method of hollow circular ring members according to claim 1, wherein Before step E, vacuum diffusion connection, the procedure also includes the step of fabricating a diffusion connection module.

4. The diffusion bonding method of hollow circular ring members according to claim 3, characterized by, The process of creating the diffusion connection module includes: placing the third positioning block and the fourth positioning block on the second positioning block, and connecting the side limiting block to the side limiting notch.

5. The diffusion bonding method of hollow circular ring members according to claim 4, characterized by, The fabrication of the diffusion connection module also includes: placing two finished blanks in the positioning hollow part and splicing them into a hollow ring.

6. The diffusion bonding method of hollow circular ring members according to claim 5, wherein The fabrication of the diffusion connection module further includes: placing a central limiting block into the hollow ring component.

7. The diffusion bonding method of hollow circular ring members according to claim 6, wherein The process of creating the diffusion connection module also includes: creating multiple diffusion connection modules.

8. The diffusion bonding method of hollow circular ring members according to claim 1, characterized by, The blank is cut to dimensions of 54mm × 35mm × 805mm.

9. The diffusion connection method for the hollow ring component according to claim 8, characterized in that, A. Preparing the blank includes drilling a through hole with a diameter of Φ5mm along the length of the blank.

10. The diffusion connection method for the hollow ring component according to claim 9, characterized in that, The C step, chemical milling and hole enlargement, includes: chemically milling the through hole to enlarge the Φ5mm hole to Φ20mm.

Citation Information

Patent Citations

  • Forming method for iron-based high-temperature alloy distributing ring

    CN106002103A

  • Superplastic forming die and method for variable-cross-section titanium alloy shell part

    CN113926905A

  • Vacuum diffusion welding method and mechanism for butt joint of long-size thin-wall pipe fittings

    CN117139812A

  • Method for bending titanium tube

    JP1990255221A